High-efficiency battery processing technology capable of improving yield based on laser-assisted sintering
By canceling the SE process, merging the front boron and post boron processes, and adopting low surface and shallow junction technology, the boron expansion process is simplified, which solves the problems of long production cycle and high manufacturing cost of battery processing technology under LECO technology, and achieves cell efficiency Improvement and energy savings.
Patent Information
- Application Number
- CN202410580395.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-10-01
AI Technical Summary
The existing battery processing technology using LECO laser-assisted sintering technology has a long production cycle, high manufacturing costs, and complex boron expansion technology processes, which increases manufacturing errors and energy consumption.
The SE process is cancelled, the front boron and the back boron are merged into one process, low surface and shallow junction technology is adopted, the boron expansion process parameters are adjusted, the BCl3 flow is reduced, the oxygen flow and time for high-temperature oxidation push-out are increased, and the boron expansion process is improved. Square resistance to 300Ω, simplifying the process and reducing manufacturing steps.
The production cycle is shortened, the manufacturing cost is reduced, the efficiency and yield of the cells are improved, the open circuit voltage and short circuit current in the electrical performance parameters are slightly improved, energy is saved, the process structure is simple, and the operation is easy.
Smart Images

Figure BDA0004833759810000081 
Figure BDA0004833759810000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of efficient battery processing, and in particular to a highly efficient battery processing technology capable of improving the yield rate based on laser-assisted sintering. Background Art
[0002] The high-efficiency battery processing technology is a method for sintering and removing the surface of the battery. Today, facing the deteriorating ecological environment and increasingly severe global warming, photovoltaic power generation, as a clean and renewable energy, has gradually occupied an unprecedented important position in changing the existing energy structure, improving the ecological environment, and developing sustainable green energy. As an important part of photovoltaic power generation, solar cells receive light and convert it into direct current. The conversion efficiency of a cell refers to the energy efficiency of solar cells in converting solar energy into electrical energy through photovoltaic technology, and is an important indicator for measuring the performance of a cell. Improving the conversion efficiency of a cell can make cells of the same size generate more power, thereby making the company's cell products more competitive. As a new type of crystalline silicon solar cell technology, Topcon (Tunnel Oxide Passivated Contact) cells improve conversion efficiency by improving traditional cell structures and materials. There are three main aspects that affect the conversion efficiency of cells:
[0003] Open circuit voltage Uoc: The open circuit voltage Uoc is the maximum voltage that a solar cell can output, when the output current is zero. The magnitude of the open circuit voltage is equivalent to the pre-bias voltage added by the photocurrent on both sides of the cell. That is, under illumination, when the solar cell is in an open circuit state, the photogenerated carriers can only accumulate on both sides of the PN junction to generate a photogenerated electromotive force, which is the open circuit voltage of the solar cell.
[0004] Short-circuit current Isc: Short-circuit current Isc refers to the current flowing through the battery when the voltage across the battery is zero (or the current when the battery is short-circuited). The short-circuit current originates from the collection of photogenerated carriers. For an ideal solar cell with minimum resistance impedance, the short-circuit current is equal to the photogenerated current. Therefore, the short-circuit current is the maximum current that the battery can output.
[0005] Fill factor FF: FF is an important indicator to measure the output characteristics of solar cells. It represents the maximum power that a solar cell can output when carrying the optimal load. The larger the value, the greater the output power of the solar cell.
[0006] After the introduction of LECO laser-assisted sintering technology, the front-end boron expansion technology process: front boron, SE, and back boron, has many manufacturing steps and a long production cycle. The complex doping process of SE technology and the use of laser equipment increase the manufacturing cost and potential sources of manufacturing errors. LECO technology can replace the front-end SE. Through the process of laser-assisted sintering of silver paste, LECO technology can directly form a low-resistance ohmic contact between metal and silicon without damaging the passivation layer of the silicon wafer, thereby reducing the overall contact resistance without the need for additional doping steps. Therefore, the technology can be upgraded to remove the laser selective emission area, while achieving the purpose of reducing costs and improving efficiency.
[0007] At present, after some companies in the industry have introduced LECO, the front-end boron diffusion technology process: front boron and back boron, only reducing the SE process, and the production cycle is relatively long. Boron diffusion is carried out in two steps, which increases the possibility of silicon wafers being contaminated during transportation from front boron to back boron. After merging front boron and back boron into one process, the yield of silicon wafers has been improved, star-shaped hidden cracks have been reduced, fragments have been reduced, and the efficiency of the new process has been improved. With the continuous development of science and technology, people have higher and higher requirements for the manufacturing process of efficient battery processing technology.
[0008] The existing battery processing technology has certain drawbacks when used. At present, after the company has introduced LECO laser-assisted sintering technology, the front-end boron expansion technology process is: front boron, SE, and post-boron.
[0009] The process flow of the pre-boron process is as follows: heating up - vacuuming - pre-deposition - pushing forward - cooling down. The pre-deposition source step has two steps. The pushing forward temperature is about 900°C. The monitoring range of the square resistance of the pre-boron is 130±10. The function of the pre-boron is to diffuse P-type impurities on the N-type substrate to form a PN junction to achieve a suitable doping concentration and square resistance. The SE process uses a laser to perform high-concentration doping at the contact point between the metal gate line and the silicon wafer and its vicinity, and low-concentration doping in the area outside the electrode. The monitoring range of the square resistance reduction in the SE laser-doped area is 45±5. The function of SE is to form a selective emitter. High-concentration doping is performed at the contact point between the metal gate line and the silicon wafer and its vicinity to reduce the contact resistance between the front metal electrode and the silicon wafer, while low-concentration doping is performed in the area outside the electrode to reduce the recombination of the diffusion layer. By optimizing the emitter, the output current and voltage of the solar cell are increased, thereby increasing the photoelectric conversion efficiency; the process flow of the post-boron process: heating-vacuuming-high-temperature push junction (high-temperature oxidation)-cooling, the temperature of the post-boron process for the high-temperature push junction step is 1040℃, and the square resistance monitoring range of the post-boron process is 240±30. The role of the post-boron process is to provide a higher temperature for the boron diffusion process, increase oxidation after SE, push junction and grow BSG (boron silicon oxide layer), and the grown BSG protects the SE area from being corroded and polished in the subsequent trough alkali polishing. First of all, the company's current front-end boron diffusion technology process: front boron, SE, and back boron. After the introduction of LECO laser-assisted sintering technology, in order to reduce costs and improve efficiency, it is necessary to explore new boron diffusion technologies to match LECO technology. In addition, after some companies in the industry have introduced LECO, the front-end boron diffusion technology process: front boron and back boron only reduces the SE process, and the production cycle is relatively long, which has brought certain adverse effects on people's use process. For this reason, we propose a battery efficient processing technology based on laser-assisted sintering that can improve the yield rate. Summary of the invention
[0010] Technical problems solved: In view of the shortcomings of the prior art, the present invention provides an efficient battery processing technology based on laser-assisted sintering that can improve the yield. After the SE process is cancelled, the front boron and the back boron are combined into one process, reducing the two processes in the front boron diffusion technology process, avoiding the use of SE laser equipment, and reducing the manufacturing cost. Due to the reduction in manufacturing steps, the production cycle can be shortened and the yield can be improved. The new boron diffusion technology is matched with the LECO technology. The efficiency of the battery cell is 0.05% higher than the original boron diffusion technology combined with the LECO technology of the production line, which can effectively solve the problems in the background technology.
[0011] Technical solution: To achieve the above purpose, the technical solution adopted by the present invention is: a high-efficiency battery processing technology based on laser-assisted sintering that can improve the yield rate, including the following operating steps:
[0012] S1: First, the boron diffusion process is carried out, including heating-vacuuming-pre-deposition-driving-high-temperature pushing junction, high-temperature oxidation-cooling, and the source operation is carried out in the pre-deposition step;
[0013] S2: Reduce recombination and lower the saturation current density in the passivation zone;
[0014] S3: The boron diffusion process parameters are adjusted in the direction of low surface and shallow junction, the flow rate of BCl3 is reduced, the oxygen flow rate of the high temperature oxidation push junction step is increased, and the oxidation time of the high temperature oxidation push junction step is increased;
[0015] S4: The square resistance after boron diffusion is increased to 300Ω. The high square resistance boron diffusion doping technology is optimized through deposition and advancement steps to reduce the doping concentration.
[0016] S5: High square resistance silicon wafers have lower surface impurity concentration, which effectively reduces the impurity recombination centers on the surface, improves the survival rate of surface minority carriers, and increases short-wave response, thereby effectively increasing Uoc and Isc and achieving the goal of improving efficiency.
[0017] As a preferred technical solution of the present application, the LECO technology is matched in the S1 step, the SE process is removed, and the front boron and the back boron are combined into a boron expansion process to avoid the use of SE laser equipment.
[0018] As a preferred technical solution of the present application, the advancing temperature in the step S1 is 900±50°C.
[0019] As a preferred technical solution of the present application, the temperature of high temperature oxidation pushing in step S1 is 1040°C.
[0020] As a preferred technical solution of the present application, the one-step boron diffusion and integration process in step S1 reduces the steps of silicon wafers entering and exiting the furnace tube twice, and reduces the energy consumption of heating the furnace tube.
[0021] As a preferred technical solution of the present application, the square resistance value of the boron expansion process in steps S4 and S5 is 300Ω, and the high square resistance silicon wafer effectively increases Uoc, thereby achieving the purpose of improving efficiency.
[0022] As a preferred technical solution of the present application, the S3 step adopts a technology combining low surface and shallow junction to reduce recombination and lower the saturation current density of the passivation region.
[0023] As a preferred technical solution of the present application, the square resistance monitoring range of the boron diffusion in the step S4 is 300±30Ω.
[0024] Beneficial effects: Compared with the prior art, the present invention provides a battery efficient processing technology based on laser-assisted sintering that can improve the yield rate, and has the following beneficial effects: After the SE in the original process flow is cancelled, the front boron and the back boron are combined into one process, which reduces the two processes in the front boron diffusion technology process, can avoid the use of SE laser equipment, and reduce the manufacturing cost. Because of the reduction in manufacturing steps, the production cycle can be shortened and the yield rate can be improved. The new boron diffusion technology matches the LECO technology, and the efficiency of the battery cell is 0.05% higher than the original boron diffusion technology combined with the LECO technology of the production line;
[0025] The process flow of the front-end boron diffusion originally included three steps: front boron diffusion, SE, and post-boron diffusion. The front-end boron diffusion proposed in the present invention only has one step of boron diffusion, which reduces two manufacturing steps, shortens the production cycle, eliminates the complex doping process of SE technology and the use of laser equipment, and reduces manufacturing costs and potential sources of manufacturing errors.
[0026] The square resistance of the boron expansion process proposed by the present invention is 300Ω, and the high square resistance silicon wafer effectively increases Uoc, thereby achieving the purpose of improving efficiency.
[0027] The one-step boron expansion combined process proposed in the present invention reduces the steps of silicon wafers entering and exiting the furnace tube twice, reduces the energy consumption of furnace tube heating, and is one step closer to low-carbon and environmental protection. After multiple experimental verifications, the boron expansion technology proposed in the present invention after the introduction of LECO is compared with the existing boron expansion technology. The efficiency of the battery cell is improved by about 0.05%, and the open circuit voltage Uoc and short circuit current Isc in the electrical performance parameters are slightly improved. At the same time, two manufacturing processes are reduced, energy is saved and consumption is reduced. The entire battery high-efficiency processing technology has a simple structure and is easy to operate. The effect of use is better than that of the traditional method. DETAILED DESCRIPTION
[0028] The efficient battery processing technology based on laser-assisted sintering can improve the yield rate, including the following steps:
[0029] S1: First, the boron diffusion process is carried out, including heating-vacuuming-pre-deposition-driving-high-temperature pushing junction, high-temperature oxidation-cooling, and the source operation is carried out in the pre-deposition step;
[0030] S2: Reduce recombination and lower the saturation current density in the passivation zone;
[0031] S3: The boron diffusion process parameters are adjusted in the direction of low surface and shallow junction, the flow rate of BCl3 is reduced, the oxygen flow rate of the high temperature oxidation push junction step is increased, and the oxidation time of the high temperature oxidation push junction step is increased;
[0032] S4: The square resistance after boron diffusion is increased to 300Ω. The high square resistance boron diffusion doping technology is optimized through deposition and advancement steps to reduce the doping concentration.
[0033] S5: High square resistance silicon wafers have lower surface impurity concentration, which effectively reduces the impurity recombination centers on the surface, improves the survival rate of surface minority carriers, and increases short-wave response, thereby effectively increasing Uoc and Isc and achieving the goal of improving efficiency.
[0034] After the SE process was cancelled, the front boron and post boron were merged into one process, reducing two processes in the front boron diffusion technology process. This can avoid the use of SE laser equipment and reduce manufacturing costs. Because of the reduction in manufacturing steps, the production cycle can be shortened and the yield rate can be improved. The new boron diffusion technology is matched with LECO technology. The efficiency of the battery cell is 0.05% higher than the original boron diffusion technology combined with LECO technology of the production line.
[0035] Furthermore, the LECO technology is matched in the S1 step, the SE process is removed, and the front boron and the back boron are combined into a boron expansion process to avoid the use of SE laser equipment.
[0036] Furthermore, the advancing temperature in step S1 is 900±50°C.
[0037] Furthermore, the temperature of the high temperature oxidation push-in step S1 is 1040°C.
[0038] Furthermore, the one-step boron diffusion process in step S1 reduces the steps of silicon wafers entering and exiting the furnace tube twice, and reduces the energy consumption of heating the furnace tube.
[0039] Furthermore, the square resistance of the boron diffusion process in steps S4 and S5 is 300Ω, and the high square resistance silicon wafer effectively increases Uoc, thereby achieving the purpose of improving efficiency.
[0040] Furthermore, in step S3, a technology combining low surface and shallow junction is used to reduce recombination and lower the saturation current density in the passivation region.
[0041] Furthermore, the square resistance monitoring range of the boron diffusion in step S4 is 300±30Ω.
[0042] Embodiment 1:
[0043] The process flow of boron diffusion is as follows: heating - vacuuming - pre-deposition - pushing - high-temperature pushing junction (high-temperature oxidation) - cooling. The source-passing step in the pre-deposition step has two steps. The heating temperature is 300°C, the pushing temperature is 600°C, and the high-temperature oxidation pushing junction temperature is 700°C. This reduces recombination and the saturation current density in the passivation zone. After boron diffusion, the square resistance is increased to 150Ω. At this time, the finished product yield is 90% and the efficiency is 94%.
[0044] Embodiment 2:
[0045] The process flow of boron diffusion is as follows: heating - vacuuming - pre-deposition - pushing - high-temperature pushing junction (high-temperature oxidation) - cooling. The source-passing step in the pre-deposition step has two steps. The heating temperature is 600°C, the pushing temperature is 900°C, and the high-temperature oxidation pushing junction temperature is 1040°C. This reduces recombination and reduces the saturation current density in the passivation zone. After boron diffusion, the square resistance is increased to 240Ω. At this time, the finished product yield is 95% and the efficiency is 98%.
[0046] Embodiment 3:
[0047] The process flow of boron diffusion is as follows: heating - vacuuming - pre-deposition - pushing - high-temperature pushing junction (high-temperature oxidation) - cooling. The source-passing step in the pre-deposition step has two steps. The heating temperature is 600°C, the pushing temperature is 900°C, and the high-temperature oxidation pushing junction temperature is 1040°C. This reduces recombination and reduces the saturation current density in the passivation zone. After boron diffusion, the square resistance is increased to 300Ω. At this time, the finished product yield is 98% and the efficiency is 98.05%.
[0048] Embodiment 4:
[0049] The process flow of boron diffusion is as follows: heating - vacuuming - pre-deposition - pushing - high-temperature pushing junction (high-temperature oxidation) - cooling. The source-passing step in the pre-deposition step has two steps. The heating temperature is 800°C, the pushing temperature is 1000°C, and the high-temperature oxidation pushing junction temperature is 1200°C. This reduces recombination and reduces the saturation current density in the passivation zone. After boron diffusion, the square resistance is increased to 330Ω. At this time, the finished product yield is 93% and the efficiency is 95%.
[0050]
[0051]
[0052] As can be seen from the above, the best embodiment is embodiment 3, in which the pushing temperature is 900°C, the high temperature oxidation pushing temperature is 1040°C, the recombination is reduced, the saturation current density in the passivation zone is reduced, and the square resistance is increased to 300Ω after boron diffusion. It has been experimentally verified that the efficiency of the battery cell is 0.05% higher than the original boron diffusion technology combined with LECO technology of the production line.
[0053] Working principle: The present invention proposes a new boron diffusion technology to match the LECO technology, removes the SE process, and combines the front boron and the back boron into a boron diffusion process. The process flow of boron diffusion is as follows: heating - vacuuming - pre-deposition - pushing - high-temperature pushing (high-temperature oxidation) - cooling. The source-passing step in the pre-deposition step has two steps. The pushing temperature is about 900°C, and the high-temperature oxidation pushing temperature is 1040°C.
[0054] In order to reduce recombination and lower the saturation current density in the passivation zone, this process adjusts the boron diffusion process parameters in the direction of low surface + shallow junction: reducing the flow rate of BCl3, increasing the oxygen flow rate of the high-temperature oxidation push-junction step, and increasing the oxidation time of the high-temperature oxidation push-junction step.
[0055] This process increases the square resistance to 300Ω after boron diffusion. The monitoring range of the square resistance of boron diffusion is 300±30Ω. The high square resistance boron diffusion doping technology reduces the doping concentration through deposition and advancement step optimization. The high square resistance silicon wafer has a lower surface impurity concentration, which effectively reduces the surface impurity recombination center, improves the survival rate of surface minority carriers, and increases the short-wave response (the quantum efficiency QE of short-wavelength light). This effectively increases Uoc and Isc, achieving the purpose of improving efficiency.
[0056] It should be noted that, in this article, relational terms such as first and second (number one, number two), etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0057] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. An efficient battery processing technology based on laser-assisted sintering that can improve the yield rate, characterized by: The steps include: S1: First, the boron diffusion process is carried out, including heating-vacuuming-pre-deposition-driving-high-temperature pushing junction, high-temperature oxidation-cooling, and the source operation is carried out in the pre-deposition step; S2: Reduce recombination and lower the saturation current density in the passivation zone; S3: The boron diffusion process parameters are adjusted in the direction of low surface and shallow junction, the flow rate of BCl3 is reduced, the oxygen flow rate of the high temperature oxidation push junction step is increased, and the oxidation time of the high temperature oxidation push junction step is increased; S4: The square resistance after boron diffusion is increased to 300Ω. The high square resistance boron diffusion doping technology is optimized through deposition and advancement steps to reduce the doping concentration. S5: High square resistance silicon wafers have lower surface impurity concentration, which effectively reduces the impurity recombination centers on the surface, improves the survival rate of surface minority carriers, and increases short-wave response, thereby effectively increasing Uoc and Isc and achieving the purpose of improving efficiency.
2. The high-efficiency battery processing technology based on laser-assisted sintering capable of improving the yield rate according to claim 1, characterized in that: In the S1 step, the LECO technology is matched, the SE process is removed, and the front boron and the back boron are combined into a boron expansion process to avoid the use of SE laser equipment.
3. The high-efficiency battery processing technology based on laser-assisted sintering capable of improving the yield rate according to claim 1, characterized in that: The advancing temperature in the S1 step is 900±50°C.
4. The high-efficiency battery processing technology based on laser-assisted sintering capable of improving the yield rate according to claim 1, characterized in that: The temperature of the high temperature oxidation push-in step in the S1 step is 1040°C.
5. The efficient battery processing technology based on laser-assisted sintering capable of improving yield rate according to claim 1, characterized in that: The one-step boron diffusion process in step S1 reduces the steps of silicon wafers entering and exiting the furnace tube twice, and reduces the energy consumption of heating the furnace tube.
6. The high-efficiency battery processing technology based on laser-assisted sintering capable of improving the yield rate according to claim 1, characterized in that: The square resistance of the boron expansion process in steps S4 and S5 is 300Ω, and the high square resistance silicon wafer effectively increases Uoc, thereby achieving the purpose of improving efficiency.
7. The high-efficiency battery processing technology based on laser-assisted sintering capable of improving the yield rate according to claim 1, characterized in that: In the S3 step, a technology combining low surface and shallow junction is used to reduce recombination and lower the saturation current density in the passivation region.
8. The high-efficiency battery processing technology based on laser-assisted sintering capable of improving the yield rate according to claim 1, characterized in that: The monitoring range of the square resistance of the boron diffusion in the step S4 is 300±30Ω.