Method for preparing antimony selenide buffer layer by hydrothermal method and applying antimony selenide buffer layer to germanium-selenium solar cell
The antimony selenide buffer layer is prepared by a hydrothermal method, which solves the problem of buffer layer thickness and uniformity control in germanium selenide solar cells, achieves passivation of interface defects and improves charge transport efficiency, and significantly improves the photovoltaic performance of germanium selenide solar cells. Conversion efficiency and performance.
Patent Information
- Application Number
- CN202410772451.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
AI Technical Summary
Germanium selenide solar cells face difficulties in improving interface electrical properties and device efficiency in practical applications. In particular, it is difficult to control the thickness and uniformity of the buffer layer, which affects the stability of the preparation process.
The antimony selenide buffer layer was prepared using a hydrothermal method. The antimony selenide buffer layer was deposited on the surface of the electron transport layer of the germanium selenide solar cell. Potassium antimony tartrate, Se and Na2SO3 solutions and thiourea were used as regulators in deionized water. Hydrothermal treatment controls the thickness and morphology of the antimony selenide buffer layer to ensure its uniformity and density.
The antimony selenide buffer layer prepared by the hydrothermal method has high uniformity and density, reduces interface defects, improves charge separation and transport efficiency, and improves the photoelectric conversion efficiency and overall performance of germanium selenide solar cells.
Smart Images

Figure CN118738205A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photoelectric film preparation, and specifically relates to a method for preparing an antimony selenide buffer layer in a germanium-selenium solar cell by a hydrothermal method, and a method for preparing a germanium-selenium solar cell with an antimony selenide buffer layer by applying the method to the germanium-selenium solar cell. Background Art
[0002] With the rapid development of photovoltaic technology, thin-film solar cells have gradually become a hot topic of research due to their advantages such as low material cost and simple manufacturing process. Germanium selenium (GeSe), as an emerging inorganic compound material, has emerged in the research of thin-film solar cells. The binary compound GeSe has abundant reserves of constituent elements, low toxicity, and attractive optoelectronic properties, including a suitable band gap (~1.14eV), a high absorption coefficient (greater than 10 5 cm -1 ), excellent stability. Due to its unique characteristics, it has the potential to develop into a new generation of solar cells for large-scale applications. However, GeSe solar cells still face some challenges in practical applications, especially the further improvement of their interface electrical properties and device efficiency. In order to solve these problems, the study found that a buffer layer was introduced between the GeSe absorption layer and the electron transport layer to optimize the interface contact properties and charge transfer efficiency.
[0003] Antimony selenide (Sb2Se3) is an emerging semiconductor material with a direct band gap, a high absorption coefficient and excellent chemical stability. These characteristics make it an ideal buffer layer material. At present, the antimony selenide buffer layer is generally prepared by a close-space sublimation method. Under low vacuum conditions, the distance between the evaporation source and the substrate is kept very small, and the antimony selenide powder is sublimated and quickly deposited on the substrate by rapid heating. However, since the thickness of the buffer layer is usually around 10nm, this rapid deposition will make it very difficult to control the thickness and uniformity of the buffer layer, which is not conducive to the stability of the preparation process.
[0004] Therefore, it is crucial to adopt a preparation process to obtain a buffer layer with uniform thickness and smooth surface, which will help accelerate the production and widespread application of high-efficiency GeSe solar cells. Summary of the invention
[0005] The purpose of the present invention is to propose a process for preparing a high-quality antimony selenide buffer layer in a high-efficiency germanium-selenium solar cell by a hydrothermal method, and a method for preparing a germanium-selenium solar cell with an antimony selenide buffer layer by applying the process to a germanium-selenium thin-film solar cell. The present invention prepares the antimony selenide buffer layer by a hydrothermal method to form a buffer layer with uniform thickness and dense structure. The buffer layer has high uniformity and can effectively passivate the interface defects of the germanium-selenium solar cell.
[0006] Specifically, the slow deposition process of the hydrothermal method allows the thickness and morphology of the antimony selenide buffer layer to be controlled, thereby ensuring the uniformity and density of the buffer layer. This high-quality buffer layer can reduce interface defects, reduce the recombination rate of carriers, and improve the separation and transportation efficiency of charges. Passivating interface defects not only improves the interfacial electrical properties of the battery, but also obtains a higher photoelectric conversion efficiency of the germanium selenium solar cell.
[0007] By adopting the hydrothermal method of the present invention to prepare the antimony selenide buffer layer, the overall performance of the germanium-selenium solar cell with the antimony selenide buffer layer is significantly improved. This improved buffer layer preparation process provides a more efficient and reliable solution for the application of germanium-selenium solar cells in photovoltaic technology.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] According to the first aspect of the present invention, a method for preparing an antimony selenide buffer layer in a germanium-selenium solar cell by a hydrothermal method, the method uses a hydrothermal method to deposit an antimony selenide buffer layer on the surface of an electron transport layer of a germanium-selenium solar cell, comprising: an antimony source is potassium antimony tartrate, a selenium source is a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6, and a regulator is thiourea, stirring evenly in deionized water and then transferring to a polytetrafluoroethylene reactor inner tank for hydrothermal heating, the hydrothermal temperature is 100°C, and the time is 60 minutes to obtain an antimony selenide buffer layer;
[0010] The preparation method of Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6 is as follows:
[0011] 3.024 g of anhydrous sodium sulfite Na2SO3 was dissolved in 40 mL of deionized water to form a sodium sulfite solution, and then 0.315 g of selenium Se powder was added to the sodium sulfite solution; after being fully stirred, the mixture was transferred to a polytetrafluoroethylene reactor liner and reacted at a hydrothermal temperature of 135°C for 8 hours to obtain a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6.
[0012] According to an embodiment of the present invention, 0.509 g of potassium antimony tartrate, 2 mL of a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6, 0.2 g of thiourea, and 38 mL of deionized water are stirred evenly and then transferred to a polytetrafluoroethylene reactor for hydrothermal treatment at a temperature of 100° C. for 60 minutes to obtain an antimony selenide buffer layer.
[0013] According to the second aspect of the present invention, the use of the antimony selenide buffer layer of the present invention in the preparation of a germanium-selenium solar cell forms a germanium-selenium solar cell having an antimony selenide buffer layer. The specific method for preparing a germanium-selenium solar cell having an antimony selenide buffer layer comprises:
[0014] Step 1: depositing a cadmium sulfide electron transport layer on a FTO conductive substrate to obtain a FTO / CdS structure;
[0015] Step 2: Prepare an antimony selenide buffer layer by the method described in claim 1 to obtain a FTO / CdS / antimony selenide buffer layer structure;
[0016] Step 3, depositing a germanium-selenium light absorbing layer on the FTO / CdS / antimony selenide buffer layer structure obtained in step 2 to obtain a FTO / CdS / antimony selenide buffer layer / GeSe structure;
[0017] Step 4: spin-coating a hole transport layer on the FTO / CdS / antimony selenide buffer layer / GeSe structure obtained in step 3 to obtain a FTO / CdS / antimony selenide buffer layer / GeSe / P3HT structure;
[0018] Step 5: Scrape a carbon electrode on the FTO / CdS / antimony selenide buffer layer / GeSe / P3HT structure obtained in step 4 to obtain a FTO / CdS / antimony selenide buffer layer / GeSe / P3HT / C structure;
[0019] Thus, a germanium-selenium solar cell with an antimony selenide buffer layer is obtained.
[0020] According to an embodiment of the present invention, in step 1, the method for preparing the FTO / CdS structure is:
[0021] The FTO conductive substrate was soaked in detergent, acetone, isopropanol, ethanol and deionized water in sequence and ultrasonically treated for 30 minutes each, and then dried with nitrogen to obtain a FTO conductive substrate; cadmium sulfide CdS was deposited in a chemical water bath at 70°C for 15 minutes to obtain a FTO / CdS structure.
[0022] Further, according to an embodiment of the present invention, in step three, the antimony selenide buffer layer is used as a substrate, and a germanium selenium absorption layer is deposited on the substrate. The substrate temperature is 270° C., the evaporation source temperature is 420° C., and the evaporation is performed for 30 seconds to prepare a germanium selenium absorption layer with a thickness of 1000 nm.
[0023] Further, according to an embodiment of the present invention, in step 4, 80 μL of P3HT with a concentration of 17 mg / mL is dissolved in a chlorobenzene solution, and is spin-coated on the germanium-selenium absorption layer at 2500 rpm for 60 seconds, and then annealed on a 120° C. flat heating table for 15 minutes to obtain a hole transport layer.
[0024] Compared with the prior art, the present invention has the following beneficial effects: First, the present invention proposes a novel preparation process for a high-quality antimony selenide buffer layer, which is specifically prepared by a hydrothermal method. In addition, the antimony selenide buffer layer prepared by the hydrothermal method has the advantages of thin thickness and uniformity, ensuring uniform coverage of the antimony selenide buffer layer in the germanium-selenium solar cell. Secondly, the antimony selenide buffer layer prepared by the hydrothermal method has a smooth surface, which greatly reduces the presence of interface defects. This smooth and uniform surface of the antimony selenide buffer layer can effectively passivate interface defects, reduce the probability of carrier recombination, and thus improve charge separation and transmission efficiency. In addition, the antimony selenide buffer layer prepared by the hydrothermal method also exhibits excellent interfacial electrical properties. This antimony selenide buffer layer helps to improve the transport path of carriers, so that charges can be more smoothly transferred from the light-absorbing layer to the electrode. This efficient carrier transport not only improves the efficiency of the battery, but also enhances its stability and reliability.
[0025] In summary, the present invention provides a new way to effectively improve the performance of germanium-selenium solar cells by using an antimony selenide buffer layer prepared by a hydrothermal method. The introduction of the antimony selenide buffer layer improves the photoelectric conversion efficiency of the cell and has important application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the reaction of preparing an antimony selenide buffer layer by a hydrothermal method in an embodiment of the present invention;
[0027] Figure 2 This is a SEM image of the surface of the antimony selenide buffer layer prepared by the hydrothermal method in an embodiment of the present invention;
[0028] Figure 3 This is a thickness distribution diagram of an antimony selenide buffer layer prepared by a hydrothermal method in an embodiment of the present invention;
[0029] Figure 4 This is the JV curve of the antimony selenide buffer layer prepared by the hydrothermal method in the embodiment of the present invention and applied to the germanium-selenium solar cell. DETAILED DESCRIPTION
[0030] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments. Those skilled in the art should understand that the specific description below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0031] The following experimental methods and detection methods, unless otherwise specified, are conventional methods; the following reagents and raw materials, unless otherwise specified, are commercially available.
[0032] The application of the antimony selenide buffer layer of the present invention in the preparation of a germanium-selenium solar cell forms a germanium-selenium solar cell having an antimony selenide buffer layer. The specific method for preparing a germanium-selenium solar cell having an antimony selenide buffer layer comprises:
[0033] (1) soaking the FTO conductive substrate in acetone, isopropanol, ethanol and deionized water for 30 minutes each, and then drying it with nitrogen; using the treated FTO conductive substrate as a substrate, depositing a cadmium sulfide (CdS) electron transport layer on the substrate to prepare a 60 nm thin film, thereby obtaining a FTO / CdS substrate;
[0034] (2) A Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6 was synthesized by a hydrothermal method as a selenium source: 3.024 g of anhydrous sodium sulfite (Na2SO3) was dissolved in 40 mL of deionized water to form a sodium sulfite solution, and then 0.315 g of selenium powder (Se powder) was added to the sodium sulfite solution; after being fully stirred, the mixture was transferred to a polytetrafluoroethylene reactor and reacted at a hydrothermal temperature of 135°C for 8 h to obtain a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6;
[0035] (3) Depositing an antimony selenide buffer layer by a hydrothermal method, the antimony source is 0.509 g of potassium antimony tartrate, the selenium source is 2 mL of a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6, the regulator is 0.2 g of thiourea, and 38 mL of deionized water. After stirring evenly, a precursor solution is obtained and transferred to a polytetrafluoroethylene reactor for hydrothermal treatment at a temperature of 100 ° C for 60 minutes to obtain an antimony selenide buffer layer;
[0036] (4) using the antimony selenide buffer layer as a substrate, depositing a germanium-selenium light absorption layer on the substrate, with the substrate temperature at 270° C. and the evaporation source temperature at 420° C. for 30 seconds to prepare a germanium-selenium light absorption layer with a thickness of 1000 nm;
[0037] (5) 80 μL of P3HT with a concentration of 17 mg / mL was dissolved in chlorobenzene solution and spin-coated on the germanium-selenium absorption layer at 2500 rpm for 60 seconds, and then annealed on a flat heating table at 120°C for 5 minutes to obtain a hole transport layer; then a carbon electrode was scraped on the hole transport layer to obtain a germanium-selenium thin film solar cell with an antimony selenide buffer layer with a molar ratio of Se and Na2SO3 of 1:6.
[0038] Schematic diagram of antimony selenide buffer layer Figure 1 As shown, the FTO / CdS substrate is placed obliquely in the precursor liquid in the polytetrafluoroethylene reactor, with the cadmium sulfide CdS facing downward. The precursor liquid in the reactor contains sufficient precursors, first (SbO) + and SeSO3 2- The reaction generates antimony selenide. As the ion reaction in the solution proceeds, (SbO) + Also with SeSO3 2- HSe generated by hydrolysis -The reaction continues to generate Sb2Se3. The ions of the two pathways react fully and synergistically promote the growth of a uniform and dense antimony selenide buffer layer on the surface of cadmium sulfide CdS. Figure 2 The SEM image of the antimony selenide buffer layer is shown. The surface of the antimony selenide buffer layer is smooth and free of impurities, and the grain size is uniform and closely arranged. Figure 3 The thickness distribution of the antimony selenide buffer layer measured by ellipsometer is uniform, and the thickness is stable between 7.90nm and 8.39nm, showing high uniformity and dense structure. Figure 4 The current-voltage curve of the germanium-selenium solar cell prepared with an antimony selenide buffer layer is shown in Table 1. As can be seen from Table 1, the open circuit voltage (V OC ) is 0.31V, the short-circuit current density (J SC ) is 24.63 mA cm -2 , the fill factor (FF) is 43.67%, and the photoelectric conversion efficiency (PCE) is 2.31%. The germanium-selenium solar cell prepared based on the antimony selenide buffer layer has excellent photoelectric performance. This shows that the antimony selenide buffer layer has excellent heterojunction quality due to its uniform thickness and dense and smooth surface, which is conducive to the transport of carriers, thereby improving the device performance. This study provides technical support for the further preparation of high-performance germanium-selenium thin film optoelectronic devices.
[0039] Table 1
[0040] Examples <![CDATA[V OC ]]> <![CDATA[J SC ]]> FF PCE 1 0.31 24.63 43.67 3.33
Claims
1. A method for preparing an antimony selenide buffer layer in a germanium-selenium solar cell by a hydrothermal method, characterized in that: The method uses a hydrothermal method to deposit an antimony selenide buffer layer on the surface of the electron transport layer of a germanium-selenium solar cell, comprising: an antimony source is potassium antimony tartrate, a selenium source is a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6, and a regulator is thiourea. The precursor solution is uniformly stirred in deionized water and transferred to a polytetrafluoroethylene reactor for hydrothermal treatment at a temperature of 100°C for 60 minutes to obtain an antimony selenide buffer layer. The preparation method of Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6 is as follows: 3.024 g of anhydrous sodium sulfite Na2SO3 was dissolved in 40 mL of deionized water to form a sodium sulfite solution, and then 0.315 g of selenium Se powder was added to the sodium sulfite solution; after being fully stirred, the mixture was transferred to a polytetrafluoroethylene reactor liner and reacted at a hydrothermal temperature of 135°C for 8 hours to obtain a Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:
6.
2. The method for preparing an antimony selenide buffer layer in a germanium-selenium solar cell by a hydrothermal method according to claim 1, characterized in that: 0.509g potassium antimony tartrate, 2mL Na2SeSO3 solution with a molar ratio of Se to Na2SO3 of 1:6, 0.2g thiourea, 38mL deionized water, after stirring evenly, transferred to the inner liner of a polytetrafluoroethylene reactor for hydrothermal treatment at a temperature of 100°C for 60 minutes to obtain an antimony selenide buffer layer.
3. A method for preparing a germanium-selenium solar cell having an antimony selenide buffer layer, characterized in that: include: Step 1: depositing a cadmium sulfide electron transport layer on a FTO conductive substrate to obtain a FTO / CdS structure; Step 2: Prepare an antimony selenide buffer layer by the method described in claim 1 to obtain a FTO / CdS / antimony selenide buffer layer structure; Step 3, depositing a germanium-selenium light absorbing layer on the FTO / CdS / antimony selenide buffer layer structure obtained in step 2 to obtain a FTO / CdS / antimony selenide buffer layer / GeSe structure; Step 4: spin-coating a hole transport layer on the FTO / CdS / antimony selenide buffer layer / GeSe structure obtained in step 3 to obtain a FTO / CdS / antimony selenide buffer layer / GeSe / P3HT structure; Step 5: Scrape a carbon electrode on the FTO / CdS / antimony selenide buffer layer / GeSe / P3HT structure obtained in step 4 to obtain a FTO / CdS / antimony selenide buffer layer / GeSe / P3HT / C structure; Thus, a germanium-selenium solar cell with an antimony selenide buffer layer is obtained.
4. The method for preparing a germanium-selenium solar cell having an antimony selenide buffer layer according to claim 3, characterized in that: In step 1, the FTO / CdS structure preparation method is: The FTO conductive substrate was sequentially soaked in acetone, isopropanol, ethanol and deionized water for 30 minutes each, and then dried with nitrogen to obtain a FTO conductive substrate; Cadmium sulfide (CdS) was deposited by chemical water bath at 70° C. for 15 minutes to obtain a FTO / CdS structure.
5. The method for preparing a germanium-selenium solar cell having an antimony selenide buffer layer according to claim 4, characterized in that: In step three, the antimony selenide buffer layer is used as a substrate, and a germanium-selenium light absorption layer is deposited on the substrate. The substrate temperature is 270° C., the evaporation source temperature is 420° C., and the evaporation is performed for 30 seconds to prepare a germanium-selenium light absorption layer with a thickness of 1000 nm.
6. The method for preparing a germanium-selenium solar cell having an antimony selenide buffer layer according to claim 5, characterized in that: In step 4, 80 μL of 17 mg / mL P3HT was dissolved in chlorobenzene solution and spin-coated on the germanium-selenium absorption layer at 2500 rpm for 60 seconds, and then annealed on a 120° C. flat heating table for 15 minutes to obtain a hole transport layer.