Preparation method of double-layer microstructure array and multi-primary-color LED packaging structure
A double-layer microstructure array is prepared in a multi-primary color LED package through active cooling droplet condensation self-assembly technology, which solves the problem of double-layer microstructure preparation in the existing technology and significantly improves the spatial color uniformity and optical performance of the multi-primary color LED package. .
Patent Information
- Application Number
- CN202410963470.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-18
AI Technical Summary
It is difficult to prepare a double-layer microstructure array with low cost and simple process using the existing technology, resulting in insufficient spatial color uniformity of the multi-primary color LED packaging structure, which limits the quality and application expansion of the light source.
Active refrigeration droplet condensation self-assembly technology is used to form a double-layer microstructure array on the upper and lower surfaces of the second polymer film by using a double-layer polymer material as a sacrificial layer. The temperature and humidity control are used to adjust the morphology to achieve a double-layer microstructure. Preparation and application in multi-primary color LED packages to improve the spatial color uniformity of the light source.
The low-cost, simple-process preparation of double-layer microstructure arrays is achieved, which significantly improves the spatial color uniformity of multi-primary color LED packages and improves optical performance.
Smart Images

Figure CN118738237A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a technology for preparing an organic colloid surface microstructure, and in particular to a method for preparing a double-layer microstructure array and a multi-primary color LED packaging structure. Background Art
[0002] In the scheme of obtaining white light illumination by mixing multi-primary color LEDs, the differences in the spatial distribution of multi-primary color LED chips will cause the light patterns of LED chips of different colors to not match, which in turn causes the light emitted by the LED module to exhibit different correlated color temperatures (CCT) at different viewing angles. That is, multi-primary color LED modules usually have the problem of poor spatial color uniformity, which will greatly reduce the quality of the light source and user experience, and also greatly limit its application expansion.
[0003] In traditional phosphor conversion LEDs, the scattering of phosphors can effectively improve the spatial color uniformity of the light source. However, multi-primary color LEDs usually use transparent packages, and doping with micro-nano particles to achieve mixed light is usually an effective light color mixing solution. This solution uses the scattering effect of micro-nano particles on the light emitted by the LED to change the propagation direction of the light, so that the light emitted by LED chips of different colors is fully mixed, and ultimately improves the spatial color uniformity of the LED light source. However, there will be a certain amount of backscattering from micro-nano scattering particles, and part of the backscattered light is absorbed by the device and cannot be emitted, which ultimately leads to a decrease in the light efficiency of the LED light source. Preparing scattering structures (e.g., microstructure arrays) on the surface of encapsulated colloids is an effective method to improve the spatial color uniformity of multi-primary color LED light sources. Many methods for preparing microstructure arrays have been studied. At present, the method for preparing microstructure arrays on the surface of encapsulated colloids is generally the imprinting method, and the process is generally divided into two parts: mold manufacturing and compression molding. However, the mold making process relies on complex and expensive photolithography technology, which has the problems of complex processing and high cost, especially when preparing non-ordinary single-layer microstructure arrays, the processing complexity and cost are further increased. Droplet imprinting technology, as a common moldless processing technology, has received widespread attention. According to different droplet array acquisition methods, this technology mainly includes droplet printing method and breathing pattern (BF) method. The droplet printing method uses direct writing or laser pulse induction technology to prepare droplet templates and imprint the microstructure array on the surface of the polymer film, but this method still has the disadvantages of low efficiency and high cost. In the breathing pattern method, a solid polymer is dissolved in a volatile solvent, which evaporates quickly, lowering the surface temperature of the solution and causing water vapor in the air to condense into water droplets on the surface of the solution. When the solvent is completely evaporated, a polymer film containing a microstructure array is obtained. However, the surface temperature of the solute polymer is difficult to control during the evaporation of the solvent because it changes the physical properties of the polymer, making the preparation process non-isothermal and non-equilibrium. In addition, the evaporating solvents commonly used in the breathing pattern method are toxic, such as chloroform and carbon disulfide. These shortcomings limit the application of the breathing pattern method in the preparation of microstructure arrays. Therefore, it is still a huge challenge to study the preparation process of microlens arrays with simple process, low cost, flexible and controllable morphology.
[0004] Invention patent CN107188114B proposes a surface microstructure preparation method based on active refrigeration droplet condensation, and directly prepares a microstructure array on the surface of a UV-cured polymer through active refrigeration technology. However, since multi-primary color LEDs contain chips of multiple different wavelengths, the spatial distribution of chips of different colors is very different, resulting in poor spatial color uniformity, which puts higher requirements on light mixing. The scattering performance of the single-layer microstructure prepared by the above method is not able to meet the actual application requirements in terms of improving color uniformity, while the strong scattering effect of the double-layer microstructure array can effectively mix the transmitted light of different colors. Therefore, it is proposed to use a double-layer microstructure in multi-primary color LED packaging, which is expected to achieve a significant improvement in the spatial color uniformity of the light source.
[0005] In summary, how to realize low-cost and simple-process double-layer microstructure preparation technology and apply it to multi-primary color LED packaging to improve spatial color uniformity remains a challenge. Summary of the invention
[0006] In view of the problem that the current traditional surface microstructure preparation technology cannot realize the preparation of double-layer microstructures, the purpose of the present invention is to provide a preparation method of a double-layer microstructure array and a multi-primary color LED packaging structure.
[0007] The first object of the present invention is to provide a method for preparing a double-layer microstructure array, wherein microdroplets formed by active refrigeration droplet condensation self-assembly technology are used as a template for imprinting a microstructure array, a double-layer polymer material is used as a sacrificial layer instead of air, so that the three-phase interface changes from polymer-microdroplets-air to polymer-microdroplets-sacrificial layer, and the imprint preparation of the microstructure is realized on the upper and lower surfaces of the second polymer film, and finally a double-layer microstructure array with controllable morphology is obtained on the double surfaces of the second polymer film. The preparation method has a simple process, and can adjust the temperature, refrigeration time, environmental humidity and other conditions to prepare double-layer microstructure arrays with different morphologies.
[0008] The second object of the present invention is to provide a double-layer microstructure array.
[0009] The third object of the present invention is to provide a multi-primary color LED packaging structure. The multi-primary color LED packaging structure uses a high light transmittance polymer layer provided with a double-layer microstructure array to solve the problem of poor light mixing of the multi-primary color LED packaging structure and improve the spatial color uniformity of the multi-primary color LED packaging structure.
[0010] The first object of the present invention is achieved by: A method for preparing a double-layer microstructure array, characterized in that it comprises the following steps: A. preparing a first polymer film on a surface of a first substrate, and placing the first substrate on a temperature controlled platform; B. placing the temperature control platform in a closed environment control box with a constant temperature and humidity and a steam atmosphere, wherein the temperature control platform adjusts the temperature of the first polymer film to be lower than the ambient temperature in the closed environment control box, and the steam in the closed environment control box forms a first droplet array on the surface of the first polymer film; C. Arranging a dam device on the first substrate, preparing a second polymer film on the surface of the first polymer film, and obtaining a three-phase interface of the first polymer film-the first droplet array-the second polymer film; D. adjusting the temperature of the second polymer film to be lower than the ambient temperature in the closed environment control box through the temperature control platform, so that the vapor in the closed environment control box forms a second droplet array on the upper surface of the second polymer film; E. preparing a third polymer film on the surface of the second substrate, and covering the third polymer film on the second substrate on the surface of the second polymer film having the second droplet array; F. Stabilizing to form a three-phase equilibrium state of a second polymer film-a second droplet array-a third polymer film, and solidifying the second polymer film; G. Peeling off the first substrate and the second substrate, removing the first liquid drop array, the second liquid drop array, the first polymer film and the third polymer film, and forming a double-layer microstructure array on the upper and lower surfaces of the second polymer film.
[0011] Furthermore, the materials of the first substrate and the second substrate described in steps A and E are one of glass, silicone, polystyrene, polycarbonate or polymethyl methacrylate high-transmittance materials; the preparation method of the first polymer film and the third polymer film in steps A and E is spin coating, and the first polymer film and the third polymer film are planar films with uniform thickness distribution.
[0012] Furthermore, the temperature control platform is a semiconductor refrigerator; the control range of the ambient temperature of the closed environment control box described in steps B and D is -20-70°C; the cooling temperature of the temperature control platform is 5-40°C lower than the ambient temperature; the concentration range of the vapor atmosphere in the closed environment control box described in steps B and D is 10-90%, and the vapor atmosphere is one of water, methanol, ethanol, ethylene glycol or propylene glycol or one of a mixed solution; the droplet condensation time described in steps C and D is 15s-30min, and the droplet diameter of the first droplet array and the second droplet array is 0.5-100μm.
[0013] Furthermore, the second polymer film is a UV-curable polymer, the first polymer film and the third polymer film are non-UV-curable polymers, the curing method in step F is UV curing, and the curing time is 1-30 minutes; or the second polymer film is a thermally curable polymer, the first polymer film and the third polymer film are non-thermally curable polymers, the curing method in step F is thermally curing, and the curing time is 10-300 minutes.
[0014] Furthermore, the materials of the first polymer film and the third polymer film are liquid polymers at room temperature and pressure; the first polymer film is doped with high thermal conductivity nanoparticles; the second polymer film is a high light transmittance material with a transmittance of >99% and a refractive index of 1.5-1.8; the second polymer film is doped with transparent high thermal conductivity nanoparticles, and the refractive index of the high thermal conductivity nanoparticles is the same as that of the second polymer film.
[0015] Furthermore, in step C, the central area of the dam device is hollowed out, and the geometric relationship between the height h of the dam device and the thickness d1 of the first polymer film and the thickness d2 of the second polymer film is: h≥d1+d2, and the thickness d2 of the second polymer film is 0.05-3mm; the cone angle α of the dam device is equal to the contact angle of the second polymer film on the inner wall of the dam device, and the second polymer film forms a film with uniform thickness inside the dam.
[0016] Furthermore, in step E, the second substrate is limited by the plane on the top of the dam device; and in step G, the size of the double-layer microstructure array is 0.5-100 μm.
[0017] The present invention promotes condensation of water droplets by actively cooling the two interfaces between the second polymer film and the double-layer polymer sacrificial layer, and regulates the morphology of the double-layer microstructure array by controlling parameters such as temperature and time, and finally prepares a double-layer microstructure array with controllable morphology on both surfaces of the second polymer film. The double-layer microstructure array obtained by this method is used as the encapsulation layer of a multi-primary color LED device, which can significantly improve its optical performance.
[0018] The second object of the present invention is achieved by: A double-layer microstructure array prepared according to the preparation method of the double-layer microstructure array.
[0019] The third object of the present invention is achieved by: A multi-primary color LED packaging structure comprises a packaging substrate, a plurality of LED chips of different primary colors, a solid crystal layer, leads, a primary optical lens, a reflective layer and a polymer film with a double-layer microstructure array provided by the invention.
[0020] Furthermore, a primary optical lens is mounted on a packaging substrate, and a number of LED chips, a substrate, a solid crystal layer, and leads are sealed on the substrate; the reflective layer is mounted on the surface of the packaging substrate, and the polymer film with a double-layer microstructure array is mounted on the upper surface of the reflective layer outside the primary optical lens; the LED packaging structure includes ceramic packaging, chip-on-board, system packaging, and silicon-based packaging; the primary optical lens is a spherical cap lens, and the material of the primary optical lens includes silicone, epoxy resin, and polyurethane; the reflectivity of the reflective layer is greater than 95%, and it adopts the form of diffuse reflection or mirror reflection; the height of the reflective layer is H1, the bottom diameter of the reflective layer is D1, the height of the primary optical lens is H2, the diameter of the primary optical lens is D2, H1>H2, D1>D2.
[0021] Compared with the prior art, the technical solution proposed by the present invention has the following advantages: 1. The preparation method of the double-layer microstructure array proposed in the present invention is based on the micro-droplets formed by active cooling as the template for imprinting the microstructure array. By using a double-layer polymer as a sacrificial layer, the droplet array is introduced by active cooling, and the upper and lower double-layer polymer films are introduced to realize the imprint preparation of the microstructure on the upper and lower surfaces of the second polymer film at the same time, so as to obtain a double-layer microstructure array with controllable morphology on both surfaces of the second polymer film. The preparation method of the double-layer microstructure array proposed in the present invention has low cost, and the diameter and spacing of the obtained microstructure can be adjusted by the coagulation time and the cooling temperature, which solves the problem that the traditional photolithography and mold printing method cannot prepare the microstructure array on the upper and lower surfaces of the polymer at one time.
[0022] 2. In the preparation method of the double-layer microstructure proposed in the present invention, the thermal conductivity is improved by doping the first polymer film and the second polymer film with nanoparticles with high thermal conductivity, and a dam device with a certain internal cone angle is provided on the first substrate, and the cone angle of the dam is equal to the contact angle of the second polymer film on the inner wall of the dam. After the second polymer film is added to the dam device, a second polymer film with uniform thickness will be formed inside the dam; at the same time, due to the effect of the top plane of the dam, the second substrate is limited to avoid deformation of the second polymer film caused by the gravity of the second substrate.
[0023] 3. The multi-primary color LED packaging structure proposed in the present invention, by introducing a packaging layer with a double-layer microstructure array, improves the probability of different colors of light propagating in all directions through the strong scattering ability of the double-layer microstructure array, so that the different colors of light emitted from the multi-primary color LED packaging module are better matched and more fully mixed, thereby significantly improving the spatial color uniformity. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Flow chart of the method for preparing the double-layer microstructure array of Example 1 of the present invention.
[0025] Figure 2 This is a structural view of the multi-primary color LED package of the present invention.
[0026] Figure 3 This is a schematic diagram of the arrangement of lamp bead chips in the multi-primary color LED packaging structure of the present invention.
[0027] Figure 4 SEM morphology images of the upper surface of the double-layer microstructure array prepared with different condensation times: (a) the average diameter and spacing of the microstructure array with condensation time of 15s, (b) condensation time of 25s, and (c) condensation time of 45s.
[0028] Figure 5SEM morphology images of the lower surface of the double-layer microstructure array prepared with different condensation times: (a) the average diameter and spacing of the microstructure array with condensation time of 15s, (b) condensation time of 25s, and (c) condensation time of 45s.
[0029] Figure 6 Structural parameters of (a) the upper surface and (b) the lower surface with different coagulation times.
[0030] Figure 7 Figure 2 shows the spatial color temperature distribution of the multi-primary color LED packaging structure: (a) blank multi-primary color LED packaging module, (b) a multi-primary color LED packaging module with only a mirror reflective layer, (c) a multi-primary color LED packaging structure with both a mirror reflective layer and a single-layer microstructure array, and (d) a multi-primary color LED packaging structure with both a mirror reflective layer and a double-layer microstructure array.
[0031] Figure 8 Spatial color temperature distribution diagram of the multi-primary color LED package structure corresponding to the double-layer microstructure array prepared with different condensation times: (a) condensation time is 15s, (b) condensation time is 25s, (c) condensation time is 45s, and (d) the maximum correlated color temperature deviation of samples with different condensation times.
[0032] Fig. 9 This is a flow chart of a method for preparing a double-layer microstructure array according to Example 6 of the present invention. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with embodiments and with reference to the accompanying drawings. However, the following embodiments are only illustrative, and the protection scope of the present invention is not limited to these embodiments. Example 1
[0034] A method for preparing a double-layer microstructure array, characterized in that: Figure 1 As shown, the following steps are included: A. Prepare a semiconductor refrigerator 1 and a first substrate 2. The first substrate 2 is glass. Spin a layer of polymer (OE6636, Dow Corning, USA) on the surface of the first substrate 2 by spin coating. A first polymer film 3 with uniform thickness is obtained on the surface of the first substrate 2. The first substrate 2 is placed on the semiconductor refrigerator 1. The first polymer film 3 is doped with aluminum nitride nanoparticles with high thermal conductivity to increase thermal conductivity and enhance the effect of active refrigeration droplet condensation. The thickness d1 of the first polymer film 3 is 0.5 mm.
[0035] B. Place the semiconductor refrigerator 1 and the first substrate 2 in a closed environment control box 10 with a constant temperature and humidity and a vapor atmosphere, and use the semiconductor refrigerator 1 to actively cool the first substrate 2, so that the surface temperature of the first polymer film 3 is lower than the temperature in the closed environment control box 10, so that the vapor in the closed environment control box 10 nucleates and condenses into droplets on the surface of the first polymer film 3. As time goes by, the droplets on the surface of the first polymer film 3 gradually grow and self-assemble into an ordered array of droplets. Due to the effect of surface tension, part of the droplets enter the interior of the first polymer film 3 and self-assemble into evenly distributed droplets on the upper surface of the first polymer film 3 to obtain a first droplet array 4. Among them, the temperature in the closed environment control box 10 is 25°C, the relative humidity of the environment is 70%, the vapor atmosphere is water vapor, the cooling temperature of the semiconductor refrigerator 1 is 10°C, and the condensation time is 15s.
[0036] C. A dam device 5 with a height of h=1.5 mm is placed at the edge of the first substrate 2, and a layer of UV polymer (NOA61, Norland, USA) is covered on the first polymer film 3 forming the first droplet array 4 to form a second polymer film 6, thereby obtaining a three-phase interface of the first polymer film 3-first droplet array 4-second polymer film 6. The second polymer film 6 is incompatible with the first polymer film 3 and the first droplet array 4. The second polymer film 6 is a highly light-transmitting material with a light transmittance of >99% and a refractive index of 1.52. Transparent high thermal conductivity nanoparticle silica is doped in the second polymer film 6 to increase the thermal conductivity of the second polymer film 6 and enhance the effect of active refrigeration droplet condensation; and the high thermal conductivity nanoparticle silica has the same refractive index as the second polymer film 6 to avoid the reduction of optical performance caused by backscattering. The thickness d2 of the second polymer film 6 is 1 mm. The dam device 5 is a specific structure with a hollow center area. The geometric relationship between the height h of the dam device 5 and the thickness d1 of the first polymer film 3 and the thickness d2 of the second polymer film 6 is h≥d1+d2. The material of the dam device 5 is acrylic. Since the contact angle of the second polymer film 6 on the acrylic surface is 12°, the cone angle α of the dam device 5 is set to 12°. The cone angle α of the dam device 5 is equal to the contact angle of the second polymer film 6 on the inner wall of the dam device 5, and the second polymer film 6 forms a film with uniform thickness inside the dam device 5.
[0037] D. Similar to step B, the semiconductor refrigerator 1 is used to actively cool the first substrate 2, and the upper surface temperature of the second polymer film 6 is lower than the temperature in the closed environment control box 10 under the action of heat conduction, so that the vapor in the closed environment control box 10 is nucleated and condensed on the upper surface of the second polymer film 6. After a certain condensation time, the droplets on the upper surface of the second polymer film 6 gradually grow and self-assemble into an orderly and uniformly distributed droplet array. Due to the surface tension, part of the droplets enter the interior of the second polymer film 6, thereby forming a second droplet array 7 on the upper surface of the second polymer film 6. Among them, the cooling temperature of the semiconductor refrigerator 1 is 10°C, and the condensation time is 15s.
[0038] E. Prepare a second substrate 9, the material of the second substrate 9 is glass, and a layer of polymer (OE6636, Dow Corning, USA) is spin-coated on the surface of the second substrate 9 by spin coating, so as to obtain a third polymer film 8 with uniform thickness on the second substrate 9, and place the prepared second substrate 9 with the third polymer film 8 on the second polymer film 6 with the second droplet array 7 formed on the upper surface, and the second substrate 9 is limited by the plane at the top of the dam device 5 to avoid deformation of the second polymer film 6 caused by gravity. The third polymer film 8 is incompatible with the second polymer film 6 and the second droplet array 7, and the thickness of the third polymer film 8 is 0.5 mm.
[0039] F. Stabilize for a certain period of time. When the third polymer film 8, the second droplet array 7 and the second polymer film 6 reach a three-phase equilibrium state, use an ultraviolet lamp to irradiate the second polymer film 6 to form a microstructure array with the first droplet array 4 and the second droplet array 7 as templates on the lower surface and upper surface of the second polymer film 6. The peak wavelength of the ultraviolet lamp is 385nm, and the output light power density is 1.5mW / cm 2 .
[0040] G. Peel off the first substrate 2 and the second substrate 9, and use acetone and deionized water to clean and remove the first polymer film 3, the third polymer film 8, the first droplet array 4 and the second droplet array 7. The cleaning time is 60 seconds and 30 seconds respectively, and a dense double-layer microstructure array 11 is formed on the upper and lower surfaces of the cured second polymer film 6.
[0041] By the above-mentioned double-layer microstructure array preparation method, the first droplet array 4 and the second droplet array 7 are prepared in a closed environment control box 10 at an ambient temperature of 25°C, an ambient relative humidity of 70%, a temperature control platform cooling temperature of 10°C, and a condensation time of 15s, thereby obtaining the double-layer microstructure array prepared in this embodiment. The SEM morphology of the double-layer microstructure array 11 prepared in this embodiment is shown in FIG. Figure 4 (a) and Figure 5As shown in (a), the width D1, average spacing L1, and average depth A1 of the upper surface microstructure array of the double-layer microstructure array 11 are 4.17±0.36, 5.49±0.28, and 2.15±0.24 μm, respectively, and the width D2, average spacing L2, and average depth A2 of the lower surface microstructure array of the double-layer microstructure array 11 are 4.58±0.39, 6.14±0.27, and 2.51±0.21 μm, respectively. For the prepared double-layer microstructure array 11, the aspect ratios of the microstructure arrays on the upper and lower surfaces are 1.82 and 1.93, respectively.
[0042] This embodiment also provides a multi-primary color LED packaging structure, including the double-layer microstructure array prepared above.
[0043] Multi-primary color LED packaging structure, such as Figure 2 As shown, it includes a packaging substrate 101, a plurality of LED chips 102 of different primary colors, a solid crystal layer 103, a lead 104, a primary optical lens 105, and a reflective layer 106. The plurality of LED chips 102 are mechanically connected to the packaging substrate 101 through the solid crystal layer 103, each LED chip 102 is electrically conductive with the packaging substrate 101 through the lead 104, the primary optical lens 105 seals the LED chip 102 on the packaging substrate 101, the reflective layer 106 is installed on the surface of the packaging substrate 101, and the second polymer film 6 having a double-layer microstructure array 11 is installed on the upper surface of the reflective layer 106 outside the primary optical lens 105. The double-layer microstructure array 11 is obtained by the preparation method of the double-layer microstructure array in this embodiment.
[0044] Multi-color LED packaging structure lamp bead chip arrangement Figure 3 shown.
[0045] Among them, the LED chips 102 of different primary colors include several types of red LED chips, orange LED chips, yellow LED chips, green LED chips, cyan LED chips, and blue LED chips. The peak wavelength range of the red LED chip is 615nm~635nm, the peak wavelength range of the orange LED chip is 590nm~610nm, the peak wavelength range of the yellow LED chip is 560nm~580nm, the peak wavelength range of the green LED chip is 510nm~530nm, the peak wavelength range of the cyan LED chip is 480nm~500nm, and the peak wavelength range of the blue LED chip is 445nm~465nm. The LED packaging structure is not limited to ceramic packaging, chip-on-board, system packaging and silicon-based packaging.
[0046] The primary optical lens 105 is a spherical cap lens made of silicone (OE6636, Dow Corning, USA), with a light transmittance of 99% and a refractive index of 1.54; the reflective layer 106 adopts a diffuse reflection form or a mirror reflection form, with a reflectivity of >95%, and the geometric relationship among the height H1 of the reflective layer 106, the bottom diameter D1 of the reflective layer 106, the height H2 of the primary optical lens 105, and the diameter D2 of the primary optical lens 105 is H1>H2, D1>D2. Example 2
[0047] The preparation methods of the double-layer microstructure arrays of Example 2 and Example 1 are basically the same, except that: The coagulation time in step C is different from that in step D, and the coagulation time is 25 s.
[0048] The SEM morphology of the double-layer microstructure array 11 prepared in this embodiment is as follows: Figure 4 (b) and Figure 5 As shown in (b), the width D1, average spacing L1, and average depth A1 of the upper surface microstructure array of the double-layer microstructure array 11 are 7.81±1.04, 8.31±0.49, and 4.19±0.34 μm, respectively, and the width D2, average spacing L2, and average depth A2 of the lower surface microstructure array of the double-layer microstructure array 11 are 8.01±0.94, 8.48±0.50, and 4.08±0.39 μm, respectively. For the prepared double-layer microstructure array 11, the width-to-depth ratios of the microstructure arrays on the upper and lower surfaces are 1.91 and 1.91, respectively. Example 3
[0049] The preparation method of the double-layer microstructure array of Example 3 is basically the same as that of Example 1, except that: The coagulation time in step C is different from that in step D, and the coagulation time is 45s.
[0050] The SEM morphology of the double-layer microstructure array 11 prepared in this embodiment is as follows: Figure 4 As shown in (c) and 5(c), the width D1, average spacing L1, and average depth A1 of the upper surface microstructure array of the double-layer microstructure array 11 are 11.16±1.04, 11.67±0.31, and 5.07±0.54 μm, respectively, and the width D2, average spacing L2, and average depth A2 of the lower surface microstructure array of the double-layer microstructure array 11 are 10.79±1.04, 11.56±0.43, and 4.96±0.55 μm, respectively. For the prepared double-layer microstructure array 11, the width-to-depth ratios of the microstructure arrays on the upper and lower surfaces are 2.17 and 2.20, respectively.
[0051] Image Pro software was used to perform data statistics and analysis on the surface and cross-sectional SEM images of a large number of double-layer microstructure arrays 11 prepared at different coagulation times, and the statistical average width and statistical average depth of the upper and lower surfaces of each group of double-layer microstructure array structures were obtained. Figure 6 As shown, the morphology is semicircular. For the double-layer microstructure array 11 with condensation time of 15s, 25s and 45s, the width of the microstructure array on the upper surface is 4.17±0.36, 7.81±1.04 and 11.16±1.04μm, and the depth is 2.15±0.24, 4.19±0.34 and 5.07±0.54μm; the width of the microstructure array on the lower surface is 4.58±0.39, 8.01±0.94 and 10.79±1.04μm, and the depth is 2.51±0.21, 4.08±0.39 and 4.96±0.55μm. The aspect ratio is used to evaluate the change of the cross-sectional profile. For the microstructure arrays with different diameters, the aspect ratios of the upper surface are 1.82, 1.91 and 2.17, and the aspect ratios of the lower surface are 1.93, 1.91 and 2.20, respectively. It can be seen that the present method realizes a double-layer microstructure array 11 with uniform distribution, consistent morphology and close arrangement on the upper and lower surfaces.
[0052] The spatial spectrum distribution tester was used to further study the effect of different condensation times on the optical properties of the prepared double-layer microstructure array 11. The spatial color temperature distribution test was conducted on the multi-primary color LED package module with a double-layer microstructure array 11 obtained with condensation times of 15s, 25s, and 45s, respectively. The test input current was set to 80mA, and the distance between the detector test probe and the multi-primary color LED package module was 1m. The test results are shown in Figure 1. Figure 7 and Figure 8 As shown. As can be seen from the figure, the maximum color temperature deviation of the blank multi-primary color LED packaging module measured is 1183.9K, the maximum color temperature deviation of the multi-primary color LED packaging module with only a mirror reflective layer is 3115K, the maximum color temperature deviation of the multi-primary color LED packaging module with a mirror reflective layer and a single-layer microstructure array is 728.6K, and the maximum color temperature deviation of the multi-primary color LED packaging module with a mirror reflective layer and a double-layer microstructure array prepared under three different condensation times is reduced to 211.2K, 165.4K, and 169.9K, respectively. In this embodiment, the average diameter of the single-layer microstructure array is about 8μm. This shows that the introduction of a microstructure array structure on the surface of a multi-primary color LED packaging module can significantly improve its spatial color uniformity, and the array size of the double-layer microstructure array 11 prepared under different condensation time conditions has little effect on the spatial color uniformity in the multi-primary color LED packaging module, and the improvement of the spatial color uniformity by the double-layer microstructure array 11 is very stable. Example 4
[0053] A method for preparing a double-layer microstructure array, characterized in that: Figure 1 As shown, the following steps are included: A. Prepare a semiconductor refrigerator 1 and a first substrate 2. The first substrate 2 is polystyrene. Spin-coat a layer of polymer (EP1026, Resinlab, USA) on the surface of the first substrate 2 by spin coating to obtain a first polymer film 3 with uniform thickness on the surface of the first substrate 2. Place the first substrate 2 on the semiconductor refrigerator 1. The first polymer film 3 is doped with high thermal conductivity nanoparticle boron nitride to increase thermal conductivity and enhance the effect of active refrigeration droplet condensation. The thickness d1 of the first polymer film 3 is 1.5 mm.
[0054] B. Place the semiconductor refrigerator 1 and the first substrate 2 in a closed environment control box 10 with a constant temperature and humidity and a vapor atmosphere, and use the semiconductor refrigerator 1 to actively cool the first substrate 2, so that the surface temperature of the first polymer film 3 is lower than the temperature in the closed environment control box 10, so that the vapor in the closed environment control box 10 nucleates and condenses on the surface of the first polymer film 3. As time goes by, the droplets on the surface of the first polymer film 3 gradually grow and self-assemble into an ordered array of droplets. Due to the surface tension, part of the droplets enter the interior of the first polymer film 3 and self-assemble into uniformly distributed droplets on the upper surface of the first polymer film 3 to obtain a first droplet array 4. Among them, the temperature in the closed environment control box 10 is 40°C, the relative humidity of the environment is 75%, the vapor atmosphere is a mixed solution vapor of water and ethylene glycol in a ratio of 1:1, and the cooling temperature of the semiconductor refrigerator 1 is 0°C.
[0055] C. A dam device 5 with a height of h=4.5 mm is placed at the edge of the first substrate 2, and a layer of UV polymer (NOA61, Norland, USA) is covered on the first polymer film 3 forming the first droplet array 4 to form a second polymer film 6, thereby obtaining a three-phase interface of the first polymer film 3-first droplet array 4-second polymer film 6. The condensation time is 2 min, the second polymer 6 is incompatible with the first polymer film 3 and the first droplet array 4, the second polymer film 6 is a highly light-transmitting material with a light transmittance of >99% and a refractive index of 1.52, and transparent high thermal conductivity nanoparticle silica is doped in the second polymer film 6 to increase the thermal conductivity of the second polymer film 6 and enhance the effect of active refrigeration droplet condensation; and the high thermal conductivity nanoparticle silica has the same refractive index as the second polymer film 6 to avoid the reduction of optical performance caused by backscattering. The thickness d2 of the second polymer film 6 is 3 mm. The dam device 5 is a specific structure with a hollow central area. The geometric relationship between the height h of the dam device 5 and the thickness d1 of the first polymer film 3 and the thickness d2 of the second polymer film 6 is h≥d1+d2. The material of the dam device 5 is PCT plastic. Since the contact angle of the second polymer film 6 on the surface of the PCT plastic is 19°, the cone angle α of the dam device 5 is set to 19°. The cone angle α of the dam device 5 is equal to the contact angle of the second polymer film 6 on the inner wall of the dam device 5, and the second polymer film 6 forms a film with uniform thickness inside the dam device 5.
[0056] D. Similar to step B, the semiconductor refrigerator 1 is used to actively cool the first substrate 2, and the upper surface temperature of the second polymer film 6 is lower than the temperature in the closed environment control box 10 under the action of heat conduction, so that the vapor in the closed environment control box 10 is nucleated and condensed on the upper surface of the second polymer film 6. After a certain condensation time, the droplets on the upper surface of the second polymer film 6 gradually grow and self-assemble into an orderly and uniformly distributed droplet array. Due to the surface tension, part of the droplets enter the interior of the second polymer film 6, thereby forming a second droplet array 7 on the upper surface of the polymer 6. Among them, the cooling temperature of the semiconductor refrigerator 1 is 0°C, and the condensation time is 2 min.
[0057] E. Prepare a second substrate 9, the material of the second substrate 9 is polystyrene, and a layer of polymer (EP1026, Resinlab, USA) is spin-coated on the surface of the second substrate 9 by spin coating, and a third polymer film 8 with uniform thickness is obtained on the second substrate 9. The prepared second substrate 9 with the third polymer film 8 is placed on the second polymer film 6 with the second droplet array 7 formed on the upper surface, and the second substrate 9 is limited by the plane at the top of the dam device 5 to avoid deformation of the second polymer film 6 caused by gravity. Among them, the third polymer film 8 is incompatible with the second polymer film 6 and the second droplet array 7, and the thickness of the third polymer film 8 is 1.5 mm.
[0058] F. After stabilization for a certain period of time, when the third polymer film 8, the second droplet array 7 and the second polymer film 6 reach a three-phase equilibrium state, the second polymer film 6 is irradiated with an ultraviolet lamp to form a microstructure array on the surface of the second polymer film 6 with the first droplet array 4 and the second droplet array 7 as templates. The peak wavelength of the ultraviolet lamp is 385 nm, and the output light power density is 1.5 mW / cm 2 .
[0059] G. Peel off the first substrate 2 and the second substrate 9, and use acetone and deionized water to clean and remove the first polymer film 3, the third polymer film 8, the first droplet array 4 and the second droplet array 7. The cleaning time is 60 seconds and 30 seconds respectively, and a dense double-layer microstructure array 11 is formed on the upper and lower surfaces of the cured second polymer film 6.
[0060] A double-layer microstructure array prepared by the double-layer microstructure array preparation method.
[0061] This embodiment also provides a multi-primary color LED packaging structure, including the double-layer microstructure array prepared above.
[0062] Multi-primary color LED packaging structure, such as Figure 2 and Figure 3 As shown, it includes a packaging substrate 101, a plurality of LED chips 102 of different primary colors, a solid crystal layer 103, a lead 104, a primary optical lens 105, and a reflective layer 106. The plurality of LED chips 102 are mechanically connected to the packaging substrate 101 through the solid crystal layer 103, each LED chip 102 is electrically conductive with the packaging substrate 101 through the lead 104, the primary optical lens 105 seals the LED chip 102 on the packaging substrate 101, the reflective layer 106 is installed on the surface of the packaging substrate 101, and the second polymer film 6 having a double-layer microstructure array 11 is installed on the upper surface of the reflective layer 106 outside the primary optical lens 105. The double-layer microstructure array 11 is obtained by the preparation method of the double-layer microstructure array in this embodiment.
[0063] Among them, the LED chips 102 of different primary colors include a blue light LED chip with a main wavelength of 455 nm, a cyan LED chip with a main wavelength of 490 nm, a green light LED chip with a main wavelength of 520 nm, a yellow light LED chip with a main wavelength of 560 nm, and a red light LED chip with a main wavelength of 620 nm. The LED packaging structure is not limited to ceramic packaging, chip-on-board, system packaging, and silicon-based packaging.
[0064] The primary optical lens 105 is a spherical cap lens made of silicone (OE6636, Dow Corning, USA), with a light transmittance of 99% and a refractive index of 1.54; the reflective layer 106 adopts a diffuse reflection form or a mirror reflection form, with a reflectivity of >95%, and the geometric relationship among the height H1 of the reflective layer 106, the bottom diameter D1 of the reflective layer 106, the height H2 of the primary optical lens 105, and the diameter D2 of the primary optical lens 105 is H1>H2, D1>D2. Example 5
[0065] The preparation methods of the double-layer microstructure arrays of Example 5 and Example 4 are basically the same, except that: The cooling temperature of the semiconductor refrigerator 1 is different from the ambient temperature and vapor atmosphere in the closed environment control box 10: in steps B and D, the temperature in the closed environment control box 10 is 15°C, the relative humidity of the environment is 90%, the vapor atmosphere is a 1:1 mixed solution vapor of water and propylene glycol, the cooling temperature of the semiconductor refrigerator 1 is -5°C, and the condensation time is 3 minutes.
[0066] The multi-primary color LED package module of Example 5 is basically the same as that of Example 4, except that the double-layer microstructure array 11 of the multi-primary color LED package module in this embodiment is prepared by the preparation method of the double-layer microstructure array in this embodiment. Example 6
[0067] A method for preparing a double-layer microstructure array, characterized in that: Fig. 9 As shown, the following steps are included: A. Prepare a semiconductor refrigerator 1 and a first substrate 2. The first substrate 2 is glass. Spin a layer of non-thermosetting polymer (NOA61, NORLAND, USA) on the surface of the first substrate 2 by spin coating. Obtain a first polymer film 3 with uniform thickness on the surface of the first substrate 2. Place the first substrate 2 on the semiconductor refrigerator 1. The first polymer film 3 is doped with high thermal conductivity nanoparticle graphene to increase thermal conductivity and enhance the effect of active refrigeration droplet condensation. The thickness d1 of the first polymer film 3 is 1 mm.
[0068] B. Use the semiconductor refrigerator 1 to actively cool the first substrate 2, so that the surface temperature of the first polymer film 3 is lower than the ambient temperature, so that the water vapor in the air nucleates and condenses on the surface of the first polymer film 3. As time goes by, the droplets on the surface of the first polymer film 3 gradually grow and self-assemble into an ordered array of droplets. Due to the surface tension, part of the droplets enter the interior of the first polymer film 3 and self-assemble into evenly distributed droplets on the upper surface of the first polymer film 3 to obtain a first droplet array 4. Among them, the ambient temperature is 25°C, the relative humidity is 50%, and the cooling temperature of the semiconductor refrigerator 1 is 0°C.
[0069] C. A dam device 5 with a height of h=3 mm is placed at the edge of the first substrate 2, and a layer of heat-cured polymer silicone (OE6636, Dow Corning, USA) with a transmittance of 99% is covered on the first polymer film 3 forming the first droplet array 4 to form a second polymer film 6, thereby obtaining a three-phase interface of the first polymer film 3-first droplet array 4-second polymer film 6. The condensation time is 5 minutes, and the second polymer film 6 is incompatible with the first polymer film 3 and the droplets 4. The second polymer film 6 is a highly light-transmitting material with a refractive index of 1.54. Transparent high thermal conductivity nanoparticle aluminum oxide is doped in the second polymer 6 to increase the thermal conductivity of the second polymer film 6 and enhance the effect of active refrigeration droplet condensation; and the high thermal conductivity nanoparticle aluminum oxide has the same refractive index as the second polymer film 6 to avoid the reduction of optical performance caused by backscattering. The thickness d2 of the second polymer film 6 is 2 mm. The dam device 5 is a specific structure with a hollow central area. The geometric relationship between the height h of the dam device 5 and the thickness d1 of the first polymer film 3 and the thickness d2 of the second polymer film 6 is h≥d1+d2. The material of the dam device 5 is a silicon wafer. Since the contact angle of the second polymer film 6 on the surface of the silicon wafer is 17°, the cone angle α of the dam device 5 is set to 17°. The cone angle α of the dam device 5 is equal to the contact angle of the second polymer film 6 on the inner wall of the dam device 5, and the second polymer film 6 forms a film with uniform thickness inside the dam device 5.
[0070] D. Similar to step B, the semiconductor refrigerator 1 is used to actively cool the first substrate 2, and the upper surface temperature of the second polymer film 6 is lower than the ambient temperature under the action of heat conduction, so that the water vapor in the air nucleates and condenses on the upper surface of the second polymer film 6. After a certain condensation time, the droplets on the upper surface of the second polymer film 6 gradually grow and self-assemble into an orderly and evenly distributed droplet array. Due to the surface tension, part of the droplets enter the interior of the second polymer film 6, thereby forming a second droplet array 7 on the upper surface of the polymer 6. Among them, the cooling temperature of the semiconductor refrigerator 1 is 0°C, and the condensation time is 5 minutes.
[0071] E. Prepare a second substrate 9, the material of the second substrate 9 is glass, and a layer of non-thermosetting polymer (NOA61, NORLAND, USA) is spin-coated on the surface of the substrate 9 by spin coating, and a third polymer film 8 with uniform thickness is obtained on the second substrate 9. The prepared second substrate 9 with the third polymer film 8 is placed on the second polymer film 6 with the second droplet array 7 formed on the upper surface. The second substrate 9 is limited by the plane at the top of the dam device 5 to avoid deformation of the second polymer film 6 caused by gravity. The third polymer film 8 is incompatible with the second polymer film 6 and the second droplet array 7, and the thickness of the third polymer film 8 is 1 mm.
[0072] F. After stabilization for a certain period of time, when the third polymer film 8, the second droplet array 7 and the second polymer film 6 reach a three-phase equilibrium state, the device is placed on a hot stage 12 to achieve complete curing of the second polymer film 6, and a microstructure array with the first droplet array 4 and the second droplet array 7 as templates is formed on the surface of the second polymer film 6. The curing temperature of the hot stage 12 is 80°C and the curing time is 90 minutes.
[0073] G. Peel off the first substrate 2 and the second substrate 9, remove the first polymer film 3, the third polymer film 8, the first droplet array 4 and the second droplet array 7, and form a dense double-layer microstructure array 11 corresponding to the droplet arrays on the upper and lower surfaces of the solidified second polymer film 6.
[0074] A double-layer microstructure array prepared by the double-layer microstructure array preparation method.
[0075] The multi-primary color LED package module of Example 6 is basically the same as that of Example 4, except that the double-layer microstructure array 11 of the multi-primary color LED package module in this embodiment is prepared by the preparation method of the double-layer microstructure array in this embodiment.
Claims
1. A method for preparing a double-layer microstructure array, characterized in that: The following steps are involved: A. preparing a first polymer film on a surface of a first substrate, and placing the first substrate on a temperature controlled platform; B. placing the temperature control platform in a closed environment control box with a constant temperature and humidity and a steam atmosphere, wherein the temperature control platform adjusts the temperature of the first polymer film to be lower than the ambient temperature in the closed environment control box, and the steam in the closed environment control box forms a first droplet array on the surface of the first polymer film; C. Arranging a dam device on the first substrate, preparing a second polymer film on the surface of the first polymer film, and obtaining a three-phase interface of the first polymer film-the first droplet array-the second polymer film; D. adjusting the temperature of the second polymer film to be lower than the ambient temperature in the closed environment control box through the temperature control platform, so that the vapor in the closed environment control box forms a second droplet array on the upper surface of the second polymer film; E. preparing a third polymer film on the surface of the second substrate, and covering the third polymer film on the second substrate on the surface of the second polymer film having the second droplet array; F. Stabilizing to form a three-phase equilibrium state of a second polymer film-a second droplet array-a third polymer film, and solidifying the second polymer film; G. Peeling off the first substrate and the second substrate, removing the first liquid drop array, the second liquid drop array, the first polymer film and the third polymer film, and forming a double-layer microstructure array on the upper and lower surfaces of the second polymer film.
2. The method for preparing a double-layer microstructure array according to claim 1, characterized in that: The first substrate and the second substrate materials described in steps A and E are one of glass, silicone, polystyrene, polycarbonate or polymethyl methacrylate high light transmittance materials; the preparation method of the first polymer film and the third polymer film in steps A and E is spin coating, and the first polymer film and the third polymer film are planar films with uniform thickness distribution.
3. The method for preparing a double-layer microstructure array according to claim 1, characterized in that: The temperature control platform is a semiconductor refrigerator; the control range of the ambient temperature of the closed environment control box described in steps B and D is -20-70°C; the refrigeration temperature of the temperature control platform is 5-40°C lower than the ambient temperature; the concentration range of the vapor atmosphere in the closed environment control box described in steps B and D is 10-90%, and the vapor atmosphere is one of water, methanol, ethanol, ethylene glycol or propylene glycol or one of a mixed solution; the droplet condensation time described in steps C and D is 15s-30min, and the droplet diameter of the first droplet array and the second droplet array is 0.5-100μm.
4. The method for preparing a double-layer microstructure array according to claim 1, characterized in that: The second polymer film is a UV-curable polymer, the first polymer film and the third polymer film are non-UV-curable polymers, the curing method in step F is UV curing, and the curing time is 1-30 minutes; or the second polymer film is a heat-curable polymer, the first polymer film and the third polymer film are non-heat-curable polymers, the curing method in step F is heat curing, and the curing time is 10-300 minutes.
5. The method for preparing a double-layer microstructure array according to claim 1, characterized in that: The materials of the first polymer film and the third polymer film are liquid polymers at room temperature and pressure; the first polymer film is doped with high thermal conductivity nanoparticles; the second polymer film is a high light transmittance material with a transmittance of >99% and a refractive index of 1.5-1.8; the second polymer film is doped with transparent high thermal conductivity nanoparticles, and the refractive index of the transparent high thermal conductivity nanoparticles is the same as that of the second polymer film.
6. The method for preparing a double-layer microstructure array according to claim 1, characterized in that: In step C, the central area of the dam device is hollowed out, and the geometric relationship between the height h of the dam device and the thickness d1 of the first polymer film and the thickness d2 of the second polymer film is: h≥d1+d2, and the thickness d2 of the second polymer film is 0.05-3mm; the cone angle α of the dam device is equal to the contact angle of the second polymer film on the inner wall of the dam device, and the second polymer film forms a film with uniform thickness inside the dam.
7. The method for preparing a double-layer microstructure array according to claim 1, characterized in that: In step E, the second substrate is limited by the plane on the top of the dam device; in step G, the size of the double-layer microstructure array is 0.5-100 μm.
8. A double-layer microstructure array prepared according to the preparation method according to any one of claims 1 to 7.
9. A multi-primary color LED packaging structure, characterized in that: Comprising the double-layer microstructure array as described in claim 8.
10. The multi-primary color LED packaging structure according to claim 9, characterized in that: include: A packaging substrate, a plurality of LED chips of different primary colors, a solid crystal layer, leads, a primary optical lens, a reflective layer and a polymer film with a double-layer microstructure array, wherein the primary optical lens is mounted on the packaging substrate, and a plurality of LED chips, the substrate, the solid crystal layer and the leads are sealed on the substrate, the reflective layer is mounted on the surface of the packaging substrate, and the polymer film with a double-layer microstructure array is mounted on the upper surface of the reflective layer outside the primary optical lens; the LED packaging structure includes ceramic packaging, chip on board, system packaging and silicon-based packaging; the primary optical lens is a spherical cap lens, and the material of the primary optical lens includes silicone, epoxy resin and polyurethane; the reflectivity of the reflective layer is greater than 95%, and it adopts the form of diffuse reflection or mirror reflection; the height of the reflective layer is H1, the bottom diameter of the reflective layer is D1, the height of the primary optical lens is H2, the diameter of the primary optical lens is D2, H1>H2, D1>D2.
Citation Information
Patent Citations
Surface microstructure preparation method based on active refrigeration liquid droplet coagulation
CN107188114A
Full-inorganic LED packaging structure and preparation method thereof
CN109786537A
Surface microstructure preparation method for morphology regulation and control based on electric field
CN111170270A