Light emitting diode epitaxial wafer and preparation method thereof, LED
By designing alternate stacked quantum wells and quantum barrier layers in the light emitting diode epitaxial sheet, and adjusting the polarization electric field using In component gradient and high-temperature capping layer, the problem of quantum restricted Stark effect in InGaN quantum wells is solved, and the problem of quantum restricted Stark effect in InGaN quantum wells is improved. LED luminous efficiency and radiation recombination rate.
Patent Information
- Application Number
- CN202411223780.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-03
AI Technical Summary
There is a quantum confined Stark effect (QCSE) in the existing InGaN quantum well, resulting in a decrease in the coupling degree of electrons and hole wave functions, thereby reducing the quantum efficiency of LEDs.
Design a light emitting diode epitaxial sheet, including a substrate, a buffer layer, an undoped GaN layer, an N-type GaN layer, an active layer and a P-type GaN layer, an active layer consisting of alternately stacked long-wave, medium-wave and short-wave quantum wells The layer and quantum barrier layer are composed of which adjust the polarization electric field through In component gradient and high-temperature capping layer, reduce lattice mismatch, improve crystal quality and radiation recombination efficiency.
By adjusting the polarization electric field and improving the crystal quality, enhancing the overlap of electrons and holes, improving the luminescence efficiency and radiation recombination rate of LEDs, reducing non-radiation recombination, and achieving efficient preparation of light emitting diode epitaxial sheets.
Smart Images

Figure CN118738241B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optoelectronic technology, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and an LED. Background Art
[0002] The higher In component in the InGaN quantum well increases the lattice mismatch with the GaN barrier, resulting in a huge piezoelectric field in the InGaN quantum well, which produces the so-called quantum confined Stark effect (QCSE). The QCSE effect reduces the coupling between the electron and hole wave functions in the quantum well, thereby reducing the quantum efficiency of the LED. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a light-emitting diode epitaxial wafer, which improves the crystal quality of the quantum well layer, reduces the polarization effect of the quantum well layer, improves the radiation recombination efficiency of carriers in the quantum well, and improves the luminous efficiency of the light-emitting diode.
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a light emitting diode epitaxial wafer, which has a simple process and can stably prepare a light emitting diode epitaxial wafer with good luminous efficiency.
[0005] In order to solve the above technical problems, the present invention provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged;
[0006] The active layer comprises at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers;
[0007] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0008] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0009] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer, which are stacked in sequence.
[0010] In some embodiments, the first N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer;
[0011] The thickness of the first N-type nitride layer is 0.5 nm to 5 nm;
[0012] The Si doping concentration of the first N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ;
[0013] The thickness of the first InGaN layer with a gradient In composition is 0.1 nm to 3 nm;
[0014] The In composition of the first In composition gradient InGaN layer changes gradually from low to high along the growth direction;
[0015] The thickness of the first InGaN layer with a constant In composition is 0.5 nm to 5 nm;
[0016] The In composition of the first InGaN layer having a constant In composition is 0.16 to 0.19;
[0017] The first high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer;
[0018] The thickness of the first high-temperature cover layer is 0.5 nm to 5 nm.
[0019] In some embodiments, the second N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer;
[0020] The thickness of the second N-type nitride layer is 0.5 nm to 5 nm;
[0021] The Si doping concentration of the second N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ;
[0022] The thickness of the second InGaN layer with a gradient In composition is 0.1 nm to 3 nm;
[0023] The In composition of the second In composition gradient InGaN layer changes gradually from low to high along the growth direction;
[0024] The thickness of the second InGaN layer with a constant In composition is 0.5 nm to 5 nm;
[0025] The In composition of the second InGaN layer having a constant In composition is 0.13-0.16;
[0026] The second high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer;
[0027] The thickness of the second high-temperature capping layer is 0.5 nm to 5 nm.
[0028] In some embodiments, the third N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer;
[0029] The thickness of the third N-type nitride layer is 0.5 nm to 5 nm;
[0030] The Si doping concentration of the third N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ;
[0031] The thickness of the third InGaN layer with a gradient In composition is 0.1 nm to 3 nm;
[0032] The In composition of the third In composition gradient InGaN layer changes gradually from low to high along the growth direction;
[0033] The thickness of the third InGaN layer with a constant In composition is 0.5 nm to 5 nm;
[0034] The In composition of the third InGaN layer having a constant In composition is 0.1 to 0.13;
[0035] The third high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer;
[0036] The thickness of the third high-temperature cover layer is 0.5 nm to 5 nm.
[0037] In some embodiments, the In composition content of the first InGaN layer having a constant In composition is greater than the In composition content of the second InGaN layer having a constant In composition and greater than the In composition content of the third InGaN layer having a constant In composition.
[0038] In some embodiments, the long-wave quantum barrier layer, the medium-wave quantum barrier layer, or the short-wave quantum barrier layer is an AlGaN layer or / and a GaN layer.
[0039] To solve the above problems, the present invention also provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0040] S1. providing a substrate;
[0041] S2, depositing a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence;
[0042] The active layer comprises at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers;
[0043] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0044] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0045] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer, which are stacked in sequence.
[0046] In some embodiments, the first InGaN layer with a constant In composition or the second InGaN layer with a constant In composition is prepared by the following method:
[0047] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0048] (2) In N 2 and NH 3Under the atmosphere condition, stop introducing the In source and Ga source for 10s to 60s, then introduce the In source and Ga source again to continue growing the InGaN layer;
[0049] Repeat the above steps (1) and (2) 1 to 10 times to complete the growth of the first InGaN layer with a constant In composition or the second InGaN layer with a constant In composition.
[0050] In some embodiments, the third InGaN layer with a constant In composition is prepared by the following method:
[0051] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, and Ga source to complete the growth of the third InGaN layer with a constant In composition.
[0052] Correspondingly, the present invention further provides an LED, wherein the LED comprises the light emitting diode epitaxial wafer described above.
[0053] The implementation of the present invention has the following beneficial effects:
[0054] The light-emitting diode epitaxial wafer provided by the present invention has an active layer comprising at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0055] Firstly, the present invention arranges quantum well layers of different wavelength bands, utilizes light of different wavelength bands to excite phosphors to produce full-spectrum light, avoids the use of a combination of multiple LED chips of different wavelength bands, and greatly reduces production costs.
[0056] Secondly, the long-wave quantum well layer includes a first N-type nitride layer, a first InGaN layer with a gradient In component, a first InGaN layer with a constant In component, and a first high-temperature cap layer stacked in sequence; the medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In component, a second InGaN layer with a constant In component, and a second high-temperature cap layer stacked in sequence; the short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In component, a third InGaN layer with a constant In component, and a third high-temperature cap layer stacked in sequence. It should be noted that the In content in the InGaN quantum well in the active area is relatively high, and there is a large mismatch stress between the InGaN well and GaN, resulting in a large polarization electric field in the InGaN well. Therefore, depositing an N-type nitride layer can adjust the polarization electric field of the InGaN well, reduce the separation of electron and hole wave functions caused by the polarization effect, and improve the luminous efficiency of the LED. By gradually transitioning the InGaN layer with a gradual change in In composition to the InGaN layer with a constant In composition, the lattice mismatch between the InGaN layer with a constant In composition and the N-type nitride layer can be reduced, the crystal quality of the InGaN layer with a constant In composition can be improved, and the non-radiative recombination of the light-emitting diode can be reduced. The high-temperature cap layer evaporates the In diffused into the quantum barrier layer at high temperature, making the well barrier interface clearer and improving the radiative recombination efficiency of the quantum well layer.
[0057] Finally, by growing multiple periods of the above active layer, the quantum confinement effect is improved, and electrons and holes are localized in multiple quantum wells, thereby increasing the overlap of electron and hole wave functions and further increasing the radiative recombination rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 This is a schematic structural diagram of the light emitting diode epitaxial wafer provided by the present invention. DETAILED DESCRIPTION
[0059] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. In addition, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0060] In the description of the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "left", "right", "horizontal", "top", "bottom", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0061] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0062] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0063] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0064] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific processes and materials provided by the present invention, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0065] In the present invention, "preferred" and "better" are only used to describe implementation methods or embodiments with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features. In the present invention, when involving numerical ranges, unless otherwise specified, the two endpoints of the numerical range are included.
[0066] To solve the above problems, the present invention provides a light emitting diode epitaxial wafer, such as Figure 1 As shown, it includes a substrate 100, on which a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, an active layer 500, an electron blocking layer 600, and a P-type GaN layer 700 are sequentially arranged;
[0067] The active layer 500 includes at least one group of alternately stacked long-wave quantum well layers 511 and long-wave quantum barrier layers 512, at least one group of alternately stacked medium-wave quantum well layers 521 and medium-wave quantum barrier layers 522, and at least one group of alternately stacked short-wave quantum well layers 531 and short-wave quantum barrier layers 532.
[0068] The long-wave quantum well layer 511 includes a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0069] The medium-wave quantum well layer 521 includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0070] The short-wave quantum well layer 531 includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer, which are stacked in sequence.
[0071] In some embodiments, the wavelength range of photons emitted when carriers in the long-wave quantum well layer 511 and the long-wave quantum barrier layer 512 radiate and recombine is 460nm~480nm, the wavelength range of photons emitted when carriers in the medium-wave quantum well layer 521 and the medium-wave quantum barrier layer 522 radiate and recombine is 440nm~460nm, and the wavelength range of photons emitted when carriers in the short-wave quantum well layer 531 and the short-wave quantum barrier layer 532 radiate and recombine is 420nm~440nm.
[0072] The present invention sets quantum well layers of different wavelengths, uses light of different wavelengths to excite phosphors to produce full-spectrum light, avoids the use of multiple LED chips of different wavelengths, and greatly reduces production costs. By growing the above active layer of multiple periods, the quantum confinement effect is improved, and electrons and holes are localized in multiple quantum wells, thereby increasing the overlap of electron and hole wave functions, and further increasing the radiation recombination rate.
[0073] The present invention creatively designs the quantum well layer of the active layer 500. The specific structure of the quantum well layer provided by the present invention is as follows:
[0074] (I) The technical details of the long-wave quantum well layer 511 are as follows:
[0075] In some embodiments, the first N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer. In some embodiments, the thickness of the first N-type nitride layer is 0.5 nm to 5 nm; the exemplary thickness of the first N-type nitride layer is 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but is not limited to the above. In some embodiments, the Si doping concentration of the first N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The exemplary Si doping concentration of the first N-type nitride layer is 2×10 17 atoms / cm 3 , 3×10 17 atoms / cm 3 , 4×10 17 atoms / cm 3 , 5×10 17 atoms / cm 3 , 6×10 17 atoms / cm 3 ,7×10 17 atoms / cm 3, 8×10 17 atoms / cm 3 ,9×10 17 atoms / cm 3 , but not limited to the above.
[0076] In some embodiments, the thickness of the first In composition gradient InGaN layer is 0.1nm-3nm; exemplary thicknesses of the first In composition gradient InGaN layer are 1nm, 1.5nm, 2nm, 2.5nm, but are not limited to the above. In some embodiments, the In composition of the first In composition gradient InGaN layer gradiently changes from low to high along the growth direction.
[0077] In some embodiments, the thickness of the first InGaN layer with a constant In composition is 0.5 nm to 5 nm; exemplary thicknesses of the first InGaN layer with a constant In composition are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, but are not limited to the above. In some embodiments, the In composition of the first InGaN layer with a constant In composition is 0.16 to 0.19.
[0078] In some embodiments, the first InGaN layer with a constant In composition is prepared by the following method:
[0079] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0080] (2) In N 2 and NH 3 Under the atmosphere condition, stop introducing the In source and Ga source for 10s to 60s, then introduce the In source and Ga source again to continue growing the InGaN layer;
[0081] Repeat the above steps (1) and (2) 1 to 10 times to complete the growth of the first InGaN layer with a constant In composition.
[0082] It should be noted that due to the re-volatilization of In atoms and the diffusion of In atoms from the In-rich region to the In-poor region, the growth interruption makes the distribution of In atoms in the quantum well layer more uniform, and makes the quantum well layer have a weaker polarization electric field and less significant In composition fluctuations. In the case of electrical injection, electrons and holes are localized in the multi-quantum wells, thereby increasing the overlap of electron and hole wave functions and thus improving the radiative recombination rate.
[0083] In some embodiments, the first high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer; in some embodiments, the thickness of the first high temperature cap layer is 0.5 nm to 5 nm. Exemplary thicknesses of the first high temperature cap layer are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited to the above.
[0084] It should be noted that the In content in the InGaN quantum well in the active area is relatively high, and there is a large mismatch stress between the InGaN well and GaN, resulting in a large polarization electric field in the InGaN well. Therefore, depositing an N-type nitride layer can adjust the polarization electric field of the InGaN well, reduce the separation of electron and hole wave functions caused by the polarization effect, and improve the luminous efficiency of the LED. By gradually transitioning from an InGaN layer with a gradual In component to an InGaN layer with a constant In component, the lattice mismatch between the InGaN layer with a constant In component and the N-type nitride layer can be reduced, the crystal quality of the InGaN layer with a constant In component can be improved, and the non-radiative recombination of the light-emitting diode can be reduced. The high-temperature cap layer volatilizes the In diffused into the quantum barrier layer through high temperature, making the well-barrier interface clearer and improving the radiative recombination efficiency of the quantum well layer.
[0085] (ii) The technical details of the medium-wave quantum well layer 521 are as follows:
[0086] In some embodiments, the second N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer. In some embodiments, the thickness of the second N-type nitride layer is 0.5 nm to 5 nm; exemplary thicknesses of the second N-type nitride layer are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited to the above. In some embodiments, the Si doping concentration of the second N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The exemplary Si doping concentration of the second N-type nitride layer is 2×10 17 atoms / cm 3 , 3×10 17 atoms / cm 3 , 4×10 17 atoms / cm 3 , 5×10 17 atoms / cm 3 , 6×10 17atoms / cm 3 ,7×10 17 atoms / cm 3 , 8×10 17 atoms / cm 3 ,9×10 17 atoms / cm 3 , but not limited to the above.
[0087] In some embodiments, the thickness of the second In composition gradient InGaN layer is 0.1nm-3nm; exemplary thicknesses of the second In composition gradient InGaN layer are 1nm, 1.5nm, 2nm, 2.5nm, but are not limited to the above. In some embodiments, the In composition of the second In composition gradient InGaN layer gradiently changes from low to high along the growth direction.
[0088] In some embodiments, the thickness of the second InGaN layer with a constant In composition is 0.5 nm to 5 nm; exemplary thicknesses of the second InGaN layer with a constant In composition are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, but are not limited to the above. In some embodiments, the In composition of the second InGaN layer with a constant In composition is 0.13 to 0.16.
[0089] In some embodiments, the second InGaN layer with a constant In composition is prepared by the following method:
[0090] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0091] (2) In N 2 and NH 3 Under the atmosphere condition, stop introducing the In source and Ga source for 10s to 60s, then introduce the In source and Ga source again to continue growing the InGaN layer;
[0092] Repeat the above steps (1) and (2) 1 to 10 times to complete the growth of the second InGaN layer with a constant In composition.
[0093] It should be noted that due to the re-volatilization of In atoms and the diffusion of In atoms from the In-rich region to the In-poor region, the growth interruption makes the distribution of In atoms in the quantum well layer more uniform, and makes the quantum well layer have a weaker polarization electric field and less significant In composition fluctuations. In the case of electrical injection, electrons and holes are localized in the multi-quantum wells, thereby increasing the overlap of electron and hole wave functions and thus improving the radiative recombination rate.
[0094] In some embodiments, the second high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer; in some embodiments, the thickness of the second high temperature cap layer is 0.5 nm to 5 nm. Exemplary thicknesses of the second high temperature cap layer are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited to the above.
[0095] It should be noted that the In content in the InGaN quantum well in the active area is relatively high, and there is a large mismatch stress between the InGaN well and GaN, resulting in a large polarization electric field in the InGaN well. Therefore, depositing an N-type nitride layer can adjust the polarization electric field of the InGaN well, reduce the separation of electron and hole wave functions caused by the polarization effect, and improve the luminous efficiency of the LED. By gradually transitioning from an InGaN layer with a gradual In component to an InGaN layer with a constant In component, the lattice mismatch between the InGaN layer with a constant In component and the N-type nitride layer can be reduced, the crystal quality of the InGaN layer with a constant In component can be improved, and the non-radiative recombination of the light-emitting diode can be reduced. The high-temperature cap layer volatilizes the In diffused into the quantum barrier layer through high temperature, making the well-barrier interface clearer and improving the radiative recombination efficiency of the quantum well layer.
[0096] (III) The technical details of the short-wave quantum well layer 531 are as follows:
[0097] In some embodiments, the third N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer. In some embodiments, the thickness of the third N-type nitride layer is 0.5 nm to 5 nm; exemplary thicknesses of the third N-type nitride layer are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited to the above. In some embodiments, the Si doping concentration of the third N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 The exemplary Si doping concentration of the third N-type nitride layer is 2×1017 atoms / cm 3 , 3×10 17 atoms / cm 3 , 4×10 17 atoms / cm 3 , 5×10 17 atoms / cm 3 , 6×10 17 atoms / cm 3 ,7×10 17 atoms / cm 3 , 8×10 17 atoms / cm 3 ,9×10 17 atoms / cm 3 , but not limited to the above.
[0098] In some embodiments, the thickness of the third In composition gradient InGaN layer is 0.1nm-3nm; exemplary thicknesses of the third In composition gradient InGaN layer are 1nm, 1.5nm, 2nm, 2.5nm, but are not limited to the above. In some embodiments, the In composition of the third In composition gradient InGaN layer gradiently changes from low to high along the growth direction.
[0099] In some embodiments, the thickness of the third InGaN layer with a constant In composition is 0.5 nm to 5 nm; exemplary thicknesses of the third InGaN layer with a constant In composition are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited to the above. In some embodiments, the In composition of the third InGaN layer with a constant In composition is 0.1 to 0.13.
[0100] In some embodiments, the third InGaN layer with a constant In composition is prepared by the following method:
[0101] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, and Ga source to complete the growth of the third InGaN layer with a constant In composition.
[0102] It should be noted that since the In component of the short-wave quantum well is lower, its In atomic distribution is also higher and the In component is more uniform, and the lattice mismatch of GaN is smaller, the third InGaN layer with a constant In component of the short-wave quantum well is not set with growth interruption, which can reduce deposition time and improve production capacity.
[0103] In some embodiments, the third high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer; in some embodiments, the thickness of the third high temperature cap layer is 0.5 nm to 5 nm. Exemplary thicknesses of the third high temperature cap layer are 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, and 4.5 nm, but are not limited to the above.
[0104] It should be noted that the In content in the InGaN quantum well in the active area is relatively high, and there is a large mismatch stress between the InGaN well and GaN, resulting in a large polarization electric field in the InGaN well. Therefore, depositing an N-type nitride layer can adjust the polarization electric field of the InGaN well, reduce the separation of electron and hole wave functions caused by the polarization effect, and improve the luminous efficiency of the LED. By gradually transitioning from an InGaN layer with a gradual In component to an InGaN layer with a constant In component, the lattice mismatch between the InGaN layer with a constant In component and the N-type nitride layer can be reduced, the crystal quality of the InGaN layer with a constant In component can be improved, and the non-radiative recombination of the light-emitting diode can be reduced. The high-temperature cap layer volatilizes the In diffused into the quantum barrier layer through high temperature, making the well-barrier interface clearer and improving the radiative recombination efficiency of the quantum well layer.
[0105] Comparing the long-wave quantum well layer 511, the medium-wave quantum well layer 521 and the short-wave quantum well layer 531, the following characteristics are found:
[0106] In some embodiments, the In composition content of the first InGaN layer having a constant In composition is greater than the In composition content of the second InGaN layer having a constant In composition and greater than the In composition content of the third InGaN layer having a constant In composition.
[0107] In addition to the quantum well layer, other technical features of the active layer 500 are described below.
[0108] In some embodiments, the long-wave quantum barrier layer 512, the medium-wave quantum barrier layer 522, or the short-wave quantum barrier layer 532 is an AlGaN layer or / and a GaN layer. Suitable quantum barrier layers can reduce the non-radiative recombination caused by the overflow of electrons to the P-type layer and improve the recombination efficiency of electrons and holes in the quantum well.
[0109] In some embodiments, the active layer 500 includes, in sequence:
[0110] h alternately stacked long-wave quantum well layers 511 and long-wave quantum barrier layers 512,
[0111] j alternately stacked medium-wave quantum well layers 521 and medium-wave quantum barrier layers 522,
[0112] k alternately stacked short-wave quantum well layers 531 and short-wave quantum barrier layers 532;
[0113] h≥1, j≥1, k≥1.
[0114] Preferably, 1≤h≤20, 1≤j≤20, and 1≤k≤20.
[0115] Accordingly, the present invention provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0116] S1, providing a substrate 100;
[0117] In some embodiments, the substrate 100 may be a sapphire substrate, a SiO 2 One of sapphire composite substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate. Preferably, the substrate 100 is a sapphire substrate, which is a commonly used GaN-based LED substrate material. The sapphire substrate has a mature preparation process, a low price, is easy to clean and handle, and has good stability at high temperatures.
[0118] S2, depositing a buffer layer 200, a non-doped GaN layer 300, an N-type GaN layer 400, an active layer 500, an electron blocking layer 600, and a P-type GaN layer 700 in sequence on the substrate 100.
[0119] Specifically, the above preparation method comprises the following steps:
[0120] S21 , depositing the buffer layer 200 on the substrate 100 .
[0121] In some embodiments, the buffer layer 200 is an AlN buffer layer.
[0122] S22 , depositing the undoped GaN layer 300 on the buffer layer 200 .
[0123] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, N source and Ga source are introduced, and a non-doped GaN layer with a thickness of 1 μm to 5 μm is grown.
[0124] S23 , depositing the N-type GaN layer 400 on the undoped GaN layer 300 .
[0125] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Ga source, and a Si source are introduced to grow the N-type GaN layer.
[0126] S24 , depositing the active layer 500 on the N-type GaN layer 400 .
[0127] The structure of the active layer is as described above and will not be repeated here.
[0128] In some embodiments, the first InGaN layer with a constant In composition or the second InGaN layer with a constant In composition is prepared by the following method:
[0129] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0130] (2) In N 2 and NH 3 Under the atmosphere condition, stop introducing the In source and Ga source for 10s to 60s, then introduce the In source and Ga source again to continue growing the InGaN layer;
[0131] Repeat the above steps (1) and (2) 1 to 10 times to complete the growth of the first InGaN layer with a constant In composition or the second InGaN layer with a constant In composition.
[0132] In some embodiments, the third InGaN layer with a constant In composition is prepared by the following method:
[0133] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, and Ga source to complete the growth of the third InGaN layer with a constant In composition.
[0134] S25, depositing the electron blocking layer 600 on the active layer 500;
[0135] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1000° C., the pressure is controlled at 100 torr to 300 torr, N source, Al source, Ga source, and In source are introduced, and an AlInGaN electron blocking layer with a thickness of 10 nm to 40 nm is grown.
[0136] S26 , depositing the P-type GaN layer 700 on the electron blocking layer 600 .
[0137] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1050° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Mg source, and a Ga source are introduced to grow the P-type GaN layer.
[0138] Accordingly, the present invention further provides an LED, which comprises the above-mentioned light-emitting diode epitaxial wafer, wherein the photoelectric efficiency of the LED is effectively improved and other electrical properties are good.
[0139] The present invention is further described below with specific embodiments:
[0140] Example 1
[0141] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0142] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0143] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0144] The first N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0145] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0146] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0147] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0148] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0149] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0150] The second N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0151] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0152] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0153] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0154] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0155] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0156] The third N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0157] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0158] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0159] Example 2
[0160] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0161] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0162] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0163] The first N-type nitride layer is an N-type GaN layer with a thickness of 1.5 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.7nm, and the In component gradient changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.5nm, and the In component is 0.18; the first high-temperature cap layer is a GaN layer with a thickness of 2nm.
[0164] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0165] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0166] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0167] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0168] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0169] The second N-type nitride layer is an N-type GaN layer with a thickness of 1.5 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.7nm, and the In component gradient changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.5nm, and the In component is 0.15; the second high-temperature cap layer is a GaN layer with a thickness of 2nm.
[0170] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0171] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0172] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0173] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0174] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0175] The third N-type nitride layer is an N-type GaN layer with a thickness of 1.5 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.7nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.5nm, and the In component is 0.11; the third high-temperature cap layer is a GaN layer with a thickness of 2nm.
[0176] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0177] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0178] Example 3
[0179] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0180] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0181] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0182] The first N-type nitride layer is an N-type AlInGaN layer with a thickness of 1 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.3nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3nm, and the In component is 0.18; the first high-temperature cap layer is an AlInGaN layer with a thickness of 1.2nm.
[0183] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0184] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0185] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0186] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0187] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0188] The second N-type nitride layer is an N-type AlInGaN layer with a thickness of 1 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.3nm, and the In component gradient changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3nm, and the In component is 0.15; the second high-temperature cap layer is an AlInGaN layer with a thickness of 1.2nm.
[0189] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0190] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0191] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0192] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0193] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0194] The third N-type nitride layer is an N-type AlInGaN layer with a thickness of 1 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.3nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3nm, and the In component is 0.11; the third high-temperature cap layer is an AlInGaN layer with a thickness of 1.2nm.
[0195] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0196] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0197] Example 4
[0198] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0199] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0200] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0201] The first N-type nitride layer is an N-type InGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.7×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradient changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is an InGaN layer with a thickness of 1.5nm.
[0202] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0203] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0204] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0205] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0206] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0207] The second N-type nitride layer is an N-type InGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.7×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradient changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is an InGaN layer with a thickness of 1.5nm.
[0208] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0209] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0210] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0211] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0212] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0213] The third N-type nitride layer is an N-type InGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.7×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is an InGaN layer with a thickness of 1.5nm.
[0214] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0215] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0216] Example 5
[0217] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0218] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0219] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0220] The first N-type nitride layer is an N-type BGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.1×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is a BGaN layer with a thickness of 1.5nm.
[0221] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0222] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0223] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0224] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0225] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0226] The second N-type nitride layer is an N-type BGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.1×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is a BGaN layer with a thickness of 1.5nm.
[0227] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0228] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0229] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0230] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0231] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0232] The third N-type nitride layer is an N-type BGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.1×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is a BGaN layer with a thickness of 1.5nm.
[0233] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0234] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0235] Example 6
[0236] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0237] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0238] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0239] The first N-type nitride layer is an N-type BInGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is a BInGaN layer with a thickness of 1.5nm.
[0240] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0241] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0242] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 25 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0243] Repeat the above steps (1) and (2) 6 times to complete the growth.
[0244] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0245] The second N-type nitride layer is an N-type BInGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is a BInGaN layer with a thickness of 1.5nm.
[0246] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0247] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0248] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 25 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0249] Repeat the above steps (1) and (2) 6 times to complete the growth.
[0250] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0251] The third N-type nitride layer is an N-type BInGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is a BInGaN layer with a thickness of 1.5nm.
[0252] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0253] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0254] Example 7
[0255] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0256] The active layer includes 3 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 4 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0257] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0258] The first N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0259] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0260] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0261] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source were stopped for 35 seconds and then the In source and Ga source were introduced again to continue growing the InGaN layer;
[0262] Repeat the above steps (1) and (2) 4 times to complete the growth.
[0263] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0264] The second N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0265] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0266] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0267] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source were stopped for 35 seconds and then the In source and Ga source were introduced again to continue growing the InGaN layer;
[0268] Repeat the above steps (1) and (2) 4 times to complete the growth.
[0269] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0270] The third N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0271] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0272] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0273] Example 8
[0274] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0275] The active layer includes 2 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 3 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 5 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0276] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0277] The first N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0278] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0279] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0280] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0281] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0282] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0283] The second N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0284] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0285] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0286] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0287] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0288] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0289] The third N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0290] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0291] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0292] Example 9
[0293] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0294] The active layer includes 4 groups of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, 3 groups of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and 3 groups of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers.
[0295] The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence;
[0296] The first N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the first In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the first In component constant InGaN layer is 3.2nm, and the In component is 0.18; the first high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0297] Wherein, the first InGaN layer with a constant In composition is prepared by the following method:
[0298] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0299] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0300] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0301] The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence;
[0302] The second N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the second In component gradient InGaN layer is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the second In component constant InGaN layer is 3.2nm, and the In component is 0.15; the second high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0303] Wherein, the second InGaN layer with a constant In composition is prepared by the following method:
[0304] (1) Control the temperature of the reaction chamber at 700℃~900℃, the pressure at 50torr~300torr, and introduce N 2 NH 3 , In source, Ga source, grow InGaN layer;
[0305] (2) In N 2 and NH 3 Under the atmosphere condition, the In source and Ga source are stopped for 30 seconds and then the In source and Ga source are introduced again to continue growing the InGaN layer;
[0306] Repeat the above steps (1) and (2) 5 times to complete the growth.
[0307] The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence;
[0308] The third N-type nitride layer is an N-type AlGaN layer with a thickness of 1.2 nm and a Si doping concentration of 2.5×10 17 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In component is 0.5nm, and the In component gradually changes from low to high along the growth direction; the thickness of the third InGaN layer with a constant In component is 3.2nm, and the In component is 0.11; the third high-temperature cap layer is an AlGaN layer with a thickness of 1.5nm.
[0309] Wherein, the third InGaN layer with a constant In composition is prepared by the following method:
[0310] The temperature of the reaction chamber was controlled at 700°C~900°C, the pressure was controlled at 50torr~300torr, and N 2 NH 3 , In source, Ga source to complete the growth.
[0311] Comparative Example 1
[0312] This comparative example provides a light emitting diode epitaxial wafer, which is different from Example 1 in that its active layer includes 10 periods of alternately stacked InGaN quantum well layers and AlGaN quantum barrier layers, and the rest is the same as Example 1.
[0313] The light-emitting diode epitaxial wafers prepared in Examples 1 to 9 and Comparative Example 1 were prepared into 10 mil×24 mil chips using the same chip process conditions. 300 LED chips were respectively extracted and tested at a current of 120 mA. Compared with the LED prepared in Comparative Example 1, the luminous efficiency improvement rate of each example was calculated. The specific test results are shown in Table 1.
[0314] Table 1 Performance test results of LEDs obtained from Examples 1 to 9
[0315]
[0316] From the above results, it can be seen that the light-emitting diode epitaxial wafer provided by the present invention, by designing a high-quality quantum well layer, electrons and holes are localized in the quantum well layer, thereby improving the radiation recombination efficiency of the quantum well layer. The multi-period active layer is grown to improve the quantum confinement effect, and electrons and holes are localized in the multi-quantum well, thereby increasing the overlap of the electron and hole wave functions, thereby increasing the radiation recombination rate. The present invention sets different band barrier layers to reduce the polarization effect of the active layer, increase the barrier height, reduce electron overflow, promote uniform distribution of carriers in the active layer, improve the recombination efficiency of carriers in the active layer, and improve the luminous efficiency of the light-emitting diode.
[0317] In the description of this specification, the description with reference to the terms "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0318] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, on which a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged; The active layer comprises at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers; The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence; The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence; The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer stacked in sequence; The first N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer; The In composition of the first In composition gradient InGaN layer changes gradually from low to high along the growth direction; The In composition of the first InGaN layer having a constant In composition is 0.16 to 0.19; The first high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer; The second N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer; The In composition of the second In composition gradient InGaN layer changes gradually from low to high along the growth direction; The In composition of the second InGaN layer having a constant In composition is 0.13-0.16; The second high temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer; The third N-type nitride layer is one of an N-type GaN layer, an N-type AlGaN layer, an N-type AlInGaN layer, an N-type InGaN layer, an N-type BGaN layer, and an N-type BInGaN layer; The In composition of the third In composition gradient InGaN layer changes gradually from low to high along the growth direction; The In composition of the third InGaN layer having a constant In composition is 0.1 to 0.13; The third high-temperature cap layer is one of a GaN layer, an AlGaN layer, an AlInGaN layer, an InGaN layer, a BGaN layer, and a BInGaN layer.
2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the first N-type nitride layer is 0.5 nm to 5 nm; The Si doping concentration of the first N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The thickness of the first InGaN layer with a gradient In composition is 0.1 nm to 3 nm; The thickness of the first InGaN layer with a constant In composition is 0.5 nm to 5 nm; The thickness of the first high-temperature cover layer is 0.5 nm to 5 nm.
3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the second N-type nitride layer is 0.5 nm to 5 nm; The Si doping concentration of the second N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The thickness of the second InGaN layer with a gradient In composition is 0.1 nm to 3 nm; The thickness of the second InGaN layer with a constant In composition is 0.5 nm to 5 nm; The thickness of the second high-temperature capping layer is 0.5 nm to 5 nm.
4. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the third N-type nitride layer is 0.5 nm to 5 nm; The Si doping concentration of the third N-type nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 ; The thickness of the third InGaN layer with a gradient In composition is 0.1 nm to 3 nm; The thickness of the third InGaN layer with a constant In composition is 0.5 nm to 5 nm; The thickness of the third high-temperature cover layer is 0.5 nm to 5 nm.
5. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The In composition content of the first InGaN layer having a constant In composition>the In composition content of the second InGaN layer having a constant In composition>the In composition content of the third InGaN layer having a constant In composition.
6. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The long-wave quantum barrier layer, the medium-wave quantum barrier layer, or the short-wave quantum barrier layer is an AlGaN layer or / and a GaN layer.
7. A method for preparing a light emitting diode epitaxial wafer according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. providing a substrate; S2, depositing a buffer layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence; The active layer comprises at least one group of alternately stacked long-wave quantum well layers and long-wave quantum barrier layers, at least one group of alternately stacked medium-wave quantum well layers and medium-wave quantum barrier layers, and at least one group of alternately stacked short-wave quantum well layers and short-wave quantum barrier layers; The long-wave quantum well layer comprises a first N-type nitride layer, a first InGaN layer with a gradient In composition, a first InGaN layer with a constant In composition, and a first high-temperature cap layer stacked in sequence; The medium-wave quantum well layer includes a second N-type nitride layer, a second InGaN layer with a gradient In composition, a second InGaN layer with a constant In composition, and a second high-temperature cap layer stacked in sequence; The short-wave quantum well layer includes a third N-type nitride layer, a third InGaN layer with a gradient In composition, a third InGaN layer with a constant In composition, and a third high-temperature cap layer, which are stacked in sequence.
8. The method for preparing a light emitting diode epitaxial wafer according to claim 7, characterized in that: The first InGaN layer with a constant In composition or the second InGaN layer with a constant In composition is prepared by the following method: (1) Control the temperature of the reaction chamber at 700°C~900°C and the pressure at 50torr~300torr, introduce N2, NH3, In source and Ga source, and grow an InGaN layer; (2) Under the conditions of N2 and NH3 atmosphere, stop introducing In source and Ga source for 10s to 60s, then introduce In source and Ga source again to continue growing the InGaN layer; Repeat the above steps (1) and (2) 1 to 10 times to complete the growth of the first InGaN layer with a constant In composition or the second InGaN layer with a constant In composition.
9. The method for preparing a light emitting diode epitaxial wafer according to claim 7, characterized in that: The third InGaN layer with a constant In composition is prepared by the following method: The temperature of the reaction chamber is controlled at 700° C. to 900° C., the pressure is controlled at 50 torr to 300 torr, and N2, NH3, In source, and Ga source are introduced to complete the growth of the third InGaN layer with a constant In composition.
10. An LED, characterized in that: The LED comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Light-emitting diode epitaxial wafer, preparation method thereof and LED
CN117393667A
High-luminous-efficiency LED epitaxial wafer, preparation method thereof and high-luminous-efficiency LED
CN118099307A
Nitride light emitting diode and manufacturing method thereof
WO2015085803A1
Semiconductor epitaxial wafer and manufacturing method therefor
WO2023092717A1