Light emitting diode chip

By adopting a multi-layer insulating layer structure and different deposition processes in the light-emitting diode chip, the stress problem caused by a single layer of silicon oxide insulating layer is solved, the reliability and stability of the chip are improved, and water vapor is blocked from entering, extending the use of the chip life.

CN118738246AActive Publication Date: 2024-10-01XIAMEN SANAN OPTOELECTRONICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410946402.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2021-04-20
Publication Date
2024-10-01
Estimated Expiration
2041-04-20

AI Technical Summary

Technical Problem

The single-layer silicon oxide insulating layer in the light-emitting diode chip has a large slope at the end or through hole, which causes other structural layers to generate large stress during formation, and is prone to cracks or entire layer fractures, reducing the reliability of the chip.

Method used

An insulating layer structure of at least two layers is adopted, in which the first insulating layer exceeds the second insulating layer in the horizontal direction, forming a step structure to reduce the stress inside the second insulating layer, and improve the strength of the insulating layer through different deposition processes and material combinations. reliability.

Benefits of technology

It effectively avoids cracks in the insulation layer or breaks the entire layer, improves the reliability of the light-emitting diode chip, reduces stress through buffering, enhances the stability of the chip, and blocks the entry of water vapor to avoid aging failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738246A_ABST
    Figure CN118738246A_ABST
Patent Text Reader

Abstract

The invention discloses a light emitting diode chip. The light emitting diode chip comprises a semiconductor stacking layer and an insulating layer. The insulating layer at least comprises a first insulating layer and a second insulating layer; the insulating layer is provided with a step structure, the step structure comprises a first step formed by the first insulating layer and a second step formed by the second insulating layer, and the first step exceeds the second step in the horizontal direction. The insulating layer is at least formed by the first insulating layer and the second insulating layer, so that the insulating layer can be prevented from cracking or being fractured, and the reliability of the insulating layer is improved. And the first insulating layer exceeds the second insulating layer by a preset length in the horizontal direction, so that the exceeding part can play a role in buffering when the second structural layer is subsequently formed on the insulating layer, the stress generated in the second structural layer is reduced, and the second structural layer is prevented from cracking or being fractured under the action of the stress; and the reliability of the light-emitting diode chip is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field related to light emitting diodes, and in particular to a light emitting diode chip. Background Art

[0002] Light-emitting diode chips are widely used in various fields due to their high reliability, long life and low power consumption. Among them, the insulating layer in the light-emitting diode chip is mostly a single-layer silicon oxide layer with a large thickness. If other structural layers are formed on the single-layer silicon oxide layer, due to the large slope of the end or through hole of the single-layer silicon oxide layer, when the other structural layers are formed on the single-layer silicon oxide layer, large stress is generated inside the other structural layers, which makes it easy for cracks to appear in the other structural layers or the entire layer to break, thereby reducing the reliability of the light-emitting diode chip. Summary of the invention

[0003] The purpose of the present application is to provide a light-emitting diode chip, wherein the insulating layer is formed by at least a first insulating layer and a second insulating layer, and the first insulating layer exceeds the second insulating layer by a predetermined length in the horizontal direction, so as to reduce the stress generated inside the second insulating layer when the second structural layer is formed on the second insulating layer, avoid cracks in the second insulating layer or breakage of the entire layer under the action of stress, and improve the reliability of the light-emitting diode chip.

[0004] In a first aspect, an embodiment of the present application provides a light-emitting diode chip having a semiconductor stacking layer and an insulating layer, wherein the insulating layer includes at least a first insulating layer and a second insulating layer formed on the upper surface of the first insulating layer; the insulating layer has a step structure, wherein the step structure includes a first step formed by the first insulating layer and a second step formed by the second insulating layer, and the first step exceeds the second step in the horizontal direction.

[0005] In a possible implementation, the thickness of the second insulating layer is greater than that of the first insulating layer, and the thickness of the second insulating layer is equal to or greater than 1 μm.

[0006] In a possible implementation, a length L1 of the first step exceeding the second step is equal to or greater than 50 nm and less than or equal to 5000 nm.

[0007] In a possible implementation, when the first insulating layer is an atomic layer deposition layer, the length L1 of the first step beyond the second step is equal to or greater than 100 nm and less than or equal to 5000 nm.

[0008] In one possible implementation, when the first insulating layer is a high density plasma chemical vapor deposition (HDPCVD) layer, the length L1 of the first step beyond the second step is equal to or greater than 50 nm and less than or equal to 100 nm. In one possible implementation, the angle α1 between the side of the first step and the horizontal direction is smaller than the angle α2 between the side of the second step and the horizontal direction.

[0009] In a possible implementation, the side surface of the second step is a slope surface, and an angle α2 between the slope surface and the horizontal direction is between 20° and 40°, 40° and 60°, or 60° and 70°.

[0010] In a possible implementation, an angle α1 between the side surface of the first step and the horizontal direction decreases in the vertical direction, and the angle α1 is between 10° and 30° or between 30° and 45°.

[0011] In a possible implementation manner, the insulating layer is provided with a through hole penetrating the insulating layer, and the sidewall of the through hole is configured as the above-mentioned step structure; and the end of the insulating layer is configured as the above-mentioned step structure.

[0012] In a possible implementation, when the first insulating layer is an atomic layer deposition layer, the thickness of the first insulating layer is between 30 and 200 nm; the second insulating layer is a high density plasma chemical vapor deposition (HDPCVD) layer, a plasma chemical vapor deposition (PECVD) layer or an evaporation deposition layer.

[0013] In a possible implementation, when the first insulating layer is a high density plasma chemical vapor deposition (HDPCVD) layer, the thickness of the first insulating layer is between 400 and 1000 nm; and the second insulating layer is an evaporation deposition layer.

[0014] In a possible embodiment, the first insulating layer and the second insulating layer are prepared by the same preparation process, and the preparation materials of the first insulating layer and the second insulating layer are different; the preparation materials of the first insulating layer and the second insulating layer include one or more of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide.

[0015] In a possible implementation manner, the first insulating layer is made of aluminum oxide.

[0016] In one possible implementation, the second insulating layer is a distributed Bragg reflector (DBR).

[0017] In a possible embodiment, the insulating layer also includes a third insulating layer formed on the upper surface of the second insulating layer; the step structure also includes a third step formed by the third insulating layer; in the horizontal direction, the length L2 of the second step exceeding the third step is less than the length L1 of the first step exceeding the second step.

[0018] In a possible implementation manner, a second structural layer is formed on a surface of the insulating layer away from the first insulating layer, and the elongation δ of the second structural layer is equal to or less than 50%.

[0019] In a possible implementation, the second structural layer is made of a material selected from the group consisting of nickel, gold, titanium, chromium, indium tin oxide, titanium oxide, silicon oxide, aluminum oxide, silicon nitride, titanium nitride, and aluminum nitride.

[0020] In a possible implementation manner, a first structural layer is formed on a surface of the insulating layer close to the first insulating layer, and the first structural layer is a transparent insulating layer, a transparent conductive layer or a metal layer.

[0021] In a possible implementation, the semiconductor stack layer serves as the first structural layer, the insulating layer is formed on the semiconductor stack layer, and the second insulating layer is away from the semiconductor stack layer.

[0022] In a possible embodiment, the light-emitting diode chip also includes: a substrate, serving as a first structural layer; a semiconductor stacking layer forming a mesa structure on the substrate, an insulating layer covering at least the side walls of the semiconductor stacking layer and a portion of the substrate other than the semiconductor stacking layer; and a second insulating layer away from the semiconductor stacking layer.

[0023] In the second aspect, an embodiment of the present application provides an insulating layer, which at least includes: a first insulating layer and a second insulating layer formed on the upper surface of the first insulating layer; a step structure, including a first step formed by the first insulating layer and a second step formed by the second insulating layer, and the first step exceeds the second step in the horizontal direction.

[0024] In a possible implementation, the thickness of the second insulating layer is greater than that of the first insulating layer, and the thickness of the second insulating layer is equal to or greater than 1 μm.

[0025] In a possible implementation, a length L1 of the first step exceeding the second step is equal to or greater than 50 nm and less than or equal to 5000 nm.

[0026] In a possible implementation, when the first insulating layer is an atomic layer deposition layer, the length L1 of the first step beyond the second step is equal to or greater than 100 nm and less than or equal to 5000 nm.

[0027] In a possible implementation, when the first insulating layer is a high density plasma chemical vapor deposition (HDPCVD) layer, the length L1 of the first step exceeding the second step is equal to or greater than 50 nm and less than or equal to 100 nm.

[0028] In a possible implementation, an angle α1 between the side surface of the first step and the horizontal direction is smaller than an angle α2 between the side surface of the second step and the horizontal direction.

[0029] In a possible implementation, the side surface of the second step is a slope surface, and an angle α2 between the slope surface and the horizontal direction is between 20° and 40°, 40° and 60°, or 60° and 70°.

[0030] In a possible implementation, an angle α1 between the side surface of the first step and the horizontal direction decreases in the vertical direction, and the angle α1 is between 10° and 30° or between 30° and 45°.

[0031] In a possible implementation manner, the insulating layer is provided with a through hole penetrating the insulating layer, and the sidewall of the through hole is configured as the above-mentioned step structure; and the end of the insulating layer is configured as the above-mentioned step structure.

[0032] In a possible implementation, when the first insulating layer is an atomic layer deposition layer, the thickness of the first insulating layer is between 30 and 200 nm; the second insulating layer is a high-density plasma chemical vapor deposition (HDPCVD) layer, a plasma chemical vapor deposition (PECVD) layer, or an evaporation deposition layer. In a possible implementation, when the first insulating layer is a high-density plasma chemical vapor deposition (HDPCVD) layer, the thickness of the first insulating layer is between 400 and 1000 nm; the second insulating layer is an evaporation deposition layer.

[0033] In a possible embodiment, the first insulating layer and the second insulating layer are prepared by the same preparation process, and the preparation materials of the first insulating layer and the second insulating layer are different; the preparation materials of the first insulating layer and the second insulating layer include one or more of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide.

[0034] In a possible implementation manner, the first insulating layer is made of aluminum oxide.

[0035] In one possible implementation, the second insulating layer is a distributed Bragg reflector (DBR).

[0036] In a possible embodiment, the insulating layer also includes a third insulating layer formed on the upper surface of the second insulating layer; the step structure also includes a third step formed by the third insulating layer; in the horizontal direction, the length L2 of the second step exceeding the third step is less than the length L1 of the first step exceeding the second step.

[0037] Compared with the prior art, the present application has at least the following beneficial effects: the insulating layer in the present application is formed by at least a first insulating layer and a second insulating layer, which can prevent cracks from occurring in the insulating layer or the entire layer from breaking, thereby improving the reliability of the insulating layer. If the first insulating layer exceeds the second insulating layer by a predetermined length in the horizontal direction, the exceeding portion can play a buffering role when the second structural layer is subsequently formed on the insulating layer, thereby reducing the stress generated inside the second structural layer, preventing cracks from occurring in the second structural layer or the entire layer from breaking under the action of stress, thereby improving the reliability of the light-emitting diode chip. In addition, if the portion of the first insulating layer that exceeds the second insulating layer in the horizontal direction is located at the end of the insulating layer, the exceeding portion can also block the entry of water vapor, thereby preventing the light-emitting diode chip from aging and failing. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work. Figure 1 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 2 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 3 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 4 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 5 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 6 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 7 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Figure 8 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Fig. 9 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Fig.10 is a schematic cross-sectional view of a light emitting diode chip according to an embodiment of the present application; Fig.11 is a schematic cross-sectional view of an insulating layer according to an embodiment of the present application; Fig.12 is a schematic cross-sectional view of an insulating layer according to an embodiment of the present application; Fig.13 is a schematic cross-sectional view of an insulating layer according to an embodiment of the present application; Fig.14 It is a schematic cross-sectional view of an insulating layer according to an embodiment of the present application.

[0039] Illustrations: 10 insulating layer; 11 first insulating layer; 12 second insulating layer; 13 third insulating layer; 14 step structure; 20 first structure layer; 30 second structure layer; 40 semiconductor stack layer; 50 substrate; 110 substrate; 120 semiconductor stack layer; 121 first type semiconductor layer; 122 active layer; 123 second type semiconductor layer; 130 current blocking layer; 140 transparent conductive layer; 151 first electrode; 152 second electrode; 160 protective layer; 171 first pad; 172 second pad; 210 substrate bottom; 220 semiconductor stack layer; 221 first type semiconductor layer; 222 active layer; 223 second type semiconductor layer; 230 transparent conductive layer; 240 reflective layer; 251 first electrode; 252 second electrode; 260 first protective layer; 271 first pad; 272 second pad; 280 second protective layer; 310 substrate; 320 semiconductor stack layer; 321 first type semiconductor layer; 322 active layer; 323 second type semiconductor layer; 330 transparent conductive layer; 340 first protective layer; 350 reflective layer; 360 second protective layer; 370 first electrode; 380 second electrode; 390 third protective layer; 410 substrate; 420 semiconductor stack layer; 421 first type semiconductor layer; 422 active layer; 423 second type semiconductor layer; 430 current blocking layer; 440 transparent conductive layer; 451 first electrode; 452 second electrode; 453 interconnecting electrode; 460 protective layer; 471 first pad; 472 second pad. DETAILED DESCRIPTION

[0040] The following describes the implementation of the present application through specific embodiments, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. The present application can also be implemented or operated through other different specific implementations, and the details in the present application can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present application.

[0041] In the description of the present application, it should be noted that the terms "upper", "lower", "height", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, or are directions or positional relationships in which the products of the present application are usually placed when in use. These directions or positions are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present application.

[0042] According to one aspect of the present application, a light emitting diode chip is provided. Figure 1 and Figure 2 , the light emitting diode chip includes a semiconductor stacking layer 40 and an insulating layer 10. The insulating layer 10 includes at least a first insulating layer 11 and a second insulating layer 12 formed on the upper surface of the first insulating layer 11, and the insulating layer 10 has a step structure 14. The step structure 14 includes a first step formed by the first insulating layer 11 and a second step formed by the second insulating layer 12, and the first step exceeds the second step in the horizontal direction, which can also be described as the first insulating layer 11 exceeding the second insulating layer 12 in the horizontal direction.

[0043] The insulating layer 10 is formed by at least a first insulating layer 11 and a second insulating layer 12, which can prevent cracks from occurring in the insulating layer 10 or the entire layer from breaking, thereby improving the reliability of the insulating layer 10. Furthermore, the first insulating layer 11 exceeds the second insulating layer 12 by a predetermined length in the horizontal direction, and the exceeding portion can play a buffering role when the second structural layer 30 is subsequently formed on the insulating layer 10, thereby reducing the stress generated inside the second structural layer 30, preventing cracks from occurring in the second structural layer 30 or the entire layer from breaking under the action of stress, thereby improving the reliability of the light-emitting diode chip.

[0044] In one embodiment, see Figure 1 and Figure 2 , a first structural layer 20 is formed on the surface of the insulating layer 10 close to the first insulating layer 11, and the first structural layer 20 is a transparent insulating layer, a transparent conductive layer or a metal layer. A second structural layer 30 is formed on the surface of the insulating layer 10 away from the first insulating layer 11, and the second structural layer 30 covers the upper surface of the insulating layer 10 and the step structure 14. The elongation δ of the second structural layer 30 is equal to or less than 50%. According to the relationship between the elongation δ of each metal: aluminum 70.92%, silver 54.38%, copper 53.2%, nickel 48.4%, gold 35%, platinum 24.2%, titanium 24.94%, chromium 20.99%, tungsten 8.84%, the preparation material of the second structural layer 30 is preferably one of nickel, gold, titanium, chromium, indium tin oxide, titanium oxide, silicon oxide, aluminum oxide, silicon nitride, titanium nitride or aluminum nitride.

[0045] As an alternative embodiment, see Figure 5The semiconductor stack layer 40 serves as the first structural layer 20 , the insulating layer 10 is formed on the semiconductor stack layer 40 , and the second insulating layer 12 is away from the semiconductor stack layer 40 .

[0046] As an alternative embodiment, see Figure 6 The light-emitting diode chip further includes a substrate 50. The substrate 50 serves as the first structural layer 20, the semiconductor stacking layer 40 forms a mesa structure on the substrate 50, the insulating layer 10 at least covers the sidewalls of the semiconductor stacking layer 40 and a portion of the substrate 50 except the semiconductor stacking layer 40; the second insulating layer 12 is away from the semiconductor stacking layer 40.

[0047] In one embodiment, the thickness of the second insulating layer 12 is greater than the thickness of the first insulating layer 11, and the thickness of the second insulating layer 12 is equal to or greater than 1 μm. Since the second insulating layer 12 has a greater thickness, the second step has a greater slope. When the second structural layer 30 is formed on the second step, the portion of the first step that exceeds the second step can better buffer the second structural layer 30, reduce the stress generated inside the second structural layer 30, and prevent the second structural layer 30 from cracking or breaking under the stress.

[0048] See also Figure 1 and Figure 2 , the angle α1 between the side of the first step and the horizontal direction is smaller than the angle α2 between the side of the second step and the horizontal direction. Preferably, the angle α1 between the side of the first step and the horizontal direction decreases in the vertical direction, and the angle α1 is between 10° and 30° or between 30° and 45°. The side of the second step is a slope surface, and the angle α2 between the slope surface and the horizontal direction is between 20° and 40°, 40° and 60° or 60° and 70°.

[0049] As an alternative embodiment, see Figure 3 , the side surfaces of the first step and the second step are vertical surfaces.

[0050] In one embodiment, see Figure 1 and Figure 2 The step structure 14 is located at the end or middle part of the insulating layer 10. The insulating layer 10 is provided with a through hole penetrating the insulating layer 10, and the side wall of the through hole is configured as the step structure 14 ( Figure 1 The end of the insulating layer 10 is configured as a step structure 14 ( Figure 2 ). When the step structure 14 is located at the end of the insulating layer 10, the portion of the first insulating layer 11 that exceeds the second insulating layer 12 in the horizontal direction can block the entry of water vapor, thereby preventing the aging failure of the light emitting diode chip.

[0051] In one embodiment, the materials used to prepare the first insulating layer 11 and the second insulating layer 12 include one or more of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. Preferably, the material used to prepare the first insulating layer 11 is aluminum oxide, and the first insulating layer 11 prepared using aluminum oxide has good water resistance. The second insulating layer 12 is a distributed Bragg reflector (DBR).

[0052] When the first insulating layer 11 is an atomic layer deposition layer, the thickness of the first insulating layer 11 is between 30 and 200 nm, preferably, the thickness of the first insulating layer 11 is between 30 and 100 nm; or, the thickness of the first insulating layer 11 is between 100 and 150 nm; or, the thickness of the first insulating layer 11 is between 150 and 200 nm. When the first insulating layer 11 is a high-density plasma chemical vapor deposition (HDPCVD) layer, the thickness of the first insulating layer 11 is between 400 and 1000 nm, preferably, the thickness of the first insulating layer 11 is between 400 and 600 nm; or, the thickness of the first insulating layer 11 is between 600 and 800 nm; or, the thickness of the first insulating layer 11 is between 800 and 1000 nm.

[0053] The density of the first insulating layer 11 is greater than the maximum density of the second insulating layer 12. The first insulating layer 11 and the second insulating layer 12 can be prepared by different processes, and the preparation materials can be the same or different. For example, when the first insulating layer 11 is an atomic layer deposition layer, the second insulating layer 12 is a high density plasma chemical vapor deposition (HDPCVD) layer, a plasma chemical vapor deposition (PECVD) layer or an evaporation deposition layer. When the first insulating layer 11 is a high density plasma chemical vapor deposition (HDPCVD) layer, the second insulating layer 12 is an evaporation deposition layer. The first insulating layer 11 and the second insulating layer 12 can also be prepared by the same preparation process, and the preparation materials of the first insulating layer 11 and the second insulating layer 12 are different. For example, the first insulating layer 11 and the second insulating layer 12 are both atomic layer deposition layers, or the first insulating layer 11 and the second insulating layer 12 are both high density plasma chemical vapor deposition (HDPCVD) layers.

[0054] Since the density of the first insulating layer 11 is greater than the maximum density of the second insulating layer 12, when the insulating layer 10 is etched by dry etching or wet etching, the etching rate of the first insulating layer 11 is lower than the etching rate of the second insulating layer 12, so a step structure 14 is formed on the insulating layer 10. Preferably, the dry etching method is an inductively coupled plasma method (ICP).

[0055] In one embodiment, see Figure 1~Figure 3, the length L1 of the first step exceeding the second step in the horizontal direction is equal to or greater than 50nm and less than or equal to 5000nm. The size of the length L1 is related to the density between the first insulating layer 11 and the second insulating layer 12. The greater the difference in density between the first insulating layer 11 and the second insulating layer 12, the greater L1. For example, when the first insulating layer 11 is an atomic layer deposition layer, L1 is equal to or greater than 100nm and less than or equal to 5000nm. When the first insulating layer 11 is a high-density plasma chemical vapor deposition (HDPCVD) layer, L1 is equal to or greater than 50nm and less than or equal to 100nm.

[0056] In one embodiment, see Figure 4 The insulating layer 10 further includes a third insulating layer 13 formed on the upper surface of the second insulating layer 12. Correspondingly, the step structure 14 further includes a third step formed by the third insulating layer 13. In the horizontal direction, the length L2 of the second step beyond the third step is less than the length L1 of the first step beyond the second step.

[0057] The thickness of the third insulating layer 13 is equal to or greater than the thickness of the second insulating layer 12, and the density of the third insulating layer 13 is equal to or less than the minimum density of the second insulating layer 12. The third insulating layer 13 and the first insulating layer 11 and the second insulating layer 12 can be prepared by different processes. For example, the first insulating layer 11 is an atomic layer deposition layer, the second insulating layer 12 is a high-density plasma chemical vapor deposition (HDPCVD) layer, and the third insulating layer 13 is an evaporation deposition layer. The third insulating layer 13 and the first insulating layer 11 and the second insulating layer 12 can also be prepared by the same preparation process, and the preparation materials of the third insulating layer 13 and the first insulating layer 11 and the second insulating layer 12 are different.

[0058] The light emitting diode chip provided in this embodiment was tested under different conditions to verify the reliability of the light emitting diode chip: The light-emitting diode chips provided in this embodiment are subjected to aging tests under different conditions: 1) 85°C+1500mA; 2) 115°C+1500mA; 3) high temperature and high humidity; 4) double 85°C+15mA and 5) -45°C~125°C hot and cold cycle. The light-emitting diode chips after the tests all have high reliability.

[0059] The following is an example of the specific implementation structure of the light emitting diode chip: Example 1

[0060] See also Figure 7, this embodiment provides a flip-chip structured light-emitting diode chip. Figure a is an overall structural diagram of the light-emitting diode chip, and Figure b is an enlarged diagram of the black frame area in Figure a. The light-emitting diode chip includes a substrate 110 and a semiconductor stack layer 120 located on the upper surface of the substrate 110. The semiconductor stack layer 120 forms a mesa structure on the upper surface of the substrate 110. The semiconductor stack layer 120 includes a first-type semiconductor layer 121, an active layer 122, and a second-type semiconductor layer 123 arranged in sequence from bottom to top, and is provided with a groove extending from the second-type semiconductor layer 123 to the inside of the first-type semiconductor layer 121, and the groove exposes a portion of the first-type semiconductor layer 121.

[0061] Preferably, the first type semiconductor layer 121 is an N-type semiconductor layer, the second type semiconductor layer 123 is a P-type semiconductor layer, and the active layer 122 is a multi-layer quantum well layer. The substrate 110 is a sapphire flat substrate or a sapphire patterned substrate.

[0062] In one embodiment, the light emitting diode chip further comprises a current blocking layer 130, a transparent conductive layer 140, an electrode layer, a protective layer 160 and a pad layer which are sequentially arranged. The current blocking layer 130 is formed on the upper surface of the second type semiconductor layer 123, and the length of the transparent conductive layer 140 is greater than the length of the current blocking layer 130, so that the transparent conductive layer 140 covers the upper surface and sidewall of the current blocking layer 130. The electrode layer comprises a first electrode 151 electrically connected to the first type semiconductor layer 121, and a second electrode 152 electrically connected to the second type semiconductor layer 123. The pad layer comprises a first pad 171 electrically connected to the first electrode 151, and a second pad 172 electrically connected to the second electrode 152. The protective layer 160 covers the upper surface and sidewall of the semiconductor stack layer 120 and the area on the upper surface of the substrate 110 except the semiconductor stack layer 120.

[0063] Among them, the electrode layer is equivalent to the above-mentioned first structural layer, the pad layer is equivalent to the above-mentioned second structural layer, and the protective layer 160 is equivalent to the above-mentioned insulating layer. Through holes are respectively opened at positions corresponding to the first electrode 151 and the second electrode 152 in the protective layer 160, the first pad 171 fills the through hole and is electrically connected to the first electrode 151, and the second pad 172 fills the through hole and is electrically connected to the second electrode 152. As shown in Figure b, the sidewall of the through hole in the protective layer 160 is configured as the above-mentioned step structure.

[0064] Preferably, the current blocking layer 130 is made of silicon oxide, specifically including one or more of silicon oxide, silicon nitride, silicon carbide or silicon oxynitride.

[0065] Preferably, the transparent conductive layer 140 is made of a conductive material with a transparent property. In the present embodiment, the transparent conductive layer 140 is made of indium tin oxide, which mainly plays the role of ohmic contact and lateral current expansion.

[0066] Preferably, the materials used to make the first electrode 151 and the second electrode 152 both include Au or an alloy of Au. The structure and materials used to make the protective layer 160 are the same as those used to make the insulating layer in the above embodiment.

[0067] Example 2 See also Figure 8 , this embodiment provides a flip-chip structured light-emitting diode chip. Figure a is an overall structural diagram of the light-emitting diode chip, and Figure b is an enlarged diagram of the black frame area in Figure a. The light-emitting diode chip includes a substrate 210 and a semiconductor stack layer 220 located on the upper surface of the substrate 210. The semiconductor stack layer 220 forms a mesa structure on the upper surface of the substrate 210. The semiconductor stack layer 220 includes a first-type semiconductor layer 221, an active layer 222, and a second-type semiconductor layer 223 arranged in sequence from bottom to top, and is provided with a groove extending from the second-type semiconductor layer 223 to the inside of the first-type semiconductor layer 221, and the groove exposes a portion of the first-type semiconductor layer 221.

[0068] Preferably, the first type semiconductor layer 221 is an N-type semiconductor layer, the second type semiconductor layer 223 is a P-type semiconductor layer, and the active layer 222 is a multi-layer quantum well layer. The substrate 210 is a sapphire flat substrate or a sapphire patterned substrate.

[0069] In one embodiment, the light emitting diode chip further includes a transparent conductive layer 230, a reflective layer 240, an electrode layer, a first protective layer 260, a first pad 271, a second protective layer 280, and a second pad 272 arranged in sequence. The transparent conductive layer 230 is formed on the upper surface of the second type semiconductor layer 223, and the length of the reflective layer 240 is greater than the length of the transparent conductive layer 230, so that the reflective layer 240 covers the upper surface and sidewall of the transparent conductive layer 230. The electrode layer includes a first electrode 251 electrically connected to the first type semiconductor layer 221, and a second electrode 252 electrically connected to the second type semiconductor layer 223.

[0070] The first pad 271 is electrically connected to the first electrode 251, and the second pad 272 is electrically connected to the second electrode 252. The upper surface height of the first pad 271 is less than the upper surface height of the second pad 272, and a second protective layer 280 is formed between the first pad 271 and the second pad 272. The second pad 272 is continuously or discontinuously arranged on the upper surface of the second protective layer 280. The first protective layer 260 and the second protective layer 280 both cover the upper surface, the sidewall of the semiconductor stack layer 220, and the upper surface of the substrate 210 except the semiconductor stack layer 220.

[0071] Among them, the electrode layer is equivalent to the above-mentioned first structural layer, the pad layer is equivalent to the above-mentioned second structural layer, and the first protective layer 260 and the second protective layer 280 are equivalent to the above-mentioned insulating layer. A through hole is opened at the position of the first protective layer 260 corresponding to the first electrode 251, and the first pad 271 fills the through hole and is electrically connected to the first electrode 251. A through hole is opened at the position of the second protective layer 280 corresponding to the second electrode 252, and the second pad 272 fills the through hole and is electrically connected to the second electrode 252. As shown in Figure b, the side wall of the through hole in the second protective layer 280 is configured as the above-mentioned step structure. Similarly, the side wall of the through hole in the first protective layer 260 is also configured as the above-mentioned step structure.

[0072] Preferably, the transparent conductive layer 230 is made of a conductive material with a transparent property. In the present embodiment, the transparent conductive layer 230 is made of indium tin oxide, which mainly plays the role of ohmic contact and lateral current expansion.

[0073] Preferably, the reflective layer 240 is made of silver. The first electrode 251 and the second electrode 252 are made of Au or an alloy of Au. The structure and material of the first protective layer 260 and the second protective layer 280 are the same as those of the insulating layer provided in the above embodiment.

[0074] Example 3 See also Fig. 9 , this embodiment provides a vertically structured light-emitting diode chip. Figure a is an overall structural diagram of the light-emitting diode chip, and Figure b is an enlarged diagram of the black frame area in Figure a. The light-emitting diode chip includes a substrate 310, a semiconductor stack layer 320, and a functional layer located between the substrate 310 and the semiconductor stack layer 320. The two sides of the semiconductor stack layer 320 are staggered with the two sides of the substrate 310, and the two sides of the functional layer are aligned with the two sides of the substrate 310, that is, the semiconductor stack layer 320 forms a mesa structure on the upper surface of the substrate 310. Part of the surface, sidewalls of the semiconductor stack layer 320, and the area on the upper surface of the substrate 310 except the semiconductor stack layer 320 are covered with a third protective layer 390, and the third protective layer 390 can adopt the insulating layer provided in the above embodiment.

[0075] The semiconductor stacked layer 320 includes a first type semiconductor layer 321 , an active layer 322 , and a second type semiconductor layer 323 arranged in sequence from top to bottom, and is provided with a groove extending from the second type semiconductor layer 323 to the inside of the first type semiconductor layer 321 , wherein the groove exposes a portion of the first type semiconductor layer 321 .

[0076] Preferably, the first type semiconductor layer 321 is an N-type semiconductor layer, the second type semiconductor layer 323 is a P-type semiconductor layer, and the active layer 322 is a multi-layer quantum well layer. The substrate 310 is made of a material selected from GaAs, Ge, Si, Cu, Mo, WCu or MoCu.

[0077] In one embodiment, the functional layer includes a transparent conductive layer 330, a first protective layer 340, a reflective layer 350, a second protective layer 360, and a first electrode 370 electrically connected to the first type semiconductor layer 321, which are arranged in sequence. The transparent conductive layer 330 is connected to the second type semiconductor layer 323, and the first electrode 370 is connected to the substrate 310. A second electrode 380 is provided in the region above the functional layer except for the semiconductor stack layer 320, and the first protective layer 340 is provided with an opening connecting the reflective layer 350 and the second electrode 380, and the reflective layer 350 fills the opening and is electrically connected to the second electrode 380.

[0078] Among them, the transparent conductive layer 330 is equivalent to the above-mentioned first structural layer, the reflective layer 350 is equivalent to the above-mentioned second structural layer, and the first protective layer 340 is equivalent to the above-mentioned insulating layer. The height of the first protective layer 340 is greater than the height of the transparent conductive layer 330, and it is coated on the periphery of the transparent conductive layer 330 to electrically isolate the transparent conductive layer 340 from the reflective layer 350. A through hole connecting the reflective layer 350 and the transparent conductive layer 330 is provided at the bottom of the first protective layer 340, and the reflective layer 350 fills the through hole and is electrically connected to the transparent conductive layer 330. As shown in Figure b, the side wall of the through hole in the first protective layer 340 is configured as the above-mentioned step structure. Similarly, the side wall of the opening in the first protective layer 340 connecting the reflective layer 350 and the second electrode 380 is also configured as the above-mentioned step structure.

[0079] The semiconductor stacking layer 320 may be equivalent to the above-mentioned first structural layer, the third protective layer 390 may be equivalent to the above-mentioned insulating layer, and other structural layers may be continuously deposited on the third protective layer 390 .

[0080] Preferably, the transparent conductive layer 330 is made of a conductive material with a transparent property. In the present embodiment, the transparent conductive layer 330 is made of indium tin oxide, which mainly plays the role of ohmic contact and lateral current expansion.

[0081] Preferably, the second electrode 360 ​​is made of any combination of Au, Ti, Al, Cr, Pt, TiW alloy or Ni. The first electrode 380 is made of Au or an alloy of Au.

[0082] Preferably, the structure and preparation materials of the first protective layer 340 and the second protective layer 370 are the same as the structure and preparation materials of the insulating layer provided in the above embodiment.

[0083] Example 4 See also Fig.10 , this embodiment provides a high-voltage structure light-emitting diode chip. FIG. a is an overall structure diagram of the light-emitting diode chip, and FIG. b is an enlarged view of the black frame area in FIG. a. The light-emitting diode chip includes a substrate 410 and a plurality of semiconductor stacking layers 420 arranged at intervals, and adjacent semiconductor stacking layers 420 are connected by a semiconductor stacking layer 420 disposed at an interval. Fig.10 , this embodiment provides a light-emitting diode chip with a high-voltage structure. Figure a is an overall structural diagram of the light-emitting diode chip, and Figure b is an enlarged diagram of the black frame area in Figure a. The light-emitting diode chip includes a substrate 410 and a plurality of semiconductor stack layers 420 arranged at intervals, and adjacent semiconductor stack layers 420 are separated by cutting paths. Each semiconductor stack layer 420 includes a first-type semiconductor layer 421, an active layer 422, and a second-type semiconductor layer 423 arranged in sequence from bottom to top, and is provided with a groove extending from the second-type semiconductor layer 423 to the inside of the first-type semiconductor layer 421, and the groove exposes a portion of the first-type semiconductor layer 421.

[0084] In one embodiment, the light-emitting diode chip further includes a current blocking layer 430, a transparent conductive layer 440, an electrode layer, a protective layer 460, and a pad layer arranged in sequence. The current blocking layer 430 covers the upper surface of the second type semiconductor layer 123, the sidewalls of the semiconductor stack layer 420, and a portion of the cutting path. The transparent conductive layer 44 covers a portion of the current blocking layer 430. The electrode layer includes a first electrode 451 electrically connected to the first type semiconductor layer 421, a second electrode 452 electrically connected to the second type semiconductor layer 423, and an interconnection electrode 453 connecting adjacent semiconductor stack layers 420. The pad layer includes a first pad 471 electrically connected to the first electrode 451, and a second pad 472 electrically connected to the second electrode 452. The protective layer 460 covers the upper surface, sidewalls, and cutting paths of the semiconductor stack layer 420.

[0085] The substrate 410 is equivalent to the first structural layer, the interconnection electrode 453 is equivalent to the second structural layer, and the current blocking layer 430 is equivalent to the insulating layer. As shown in FIG. b, the end of the current blocking layer 430 is configured as the step structure.

[0086] The first electrode 451 and the second electrode 452 in the electrode layer are equivalent to the first structural layer, the pad layer is equivalent to the second structural layer, and the protective layer 460 is equivalent to the insulating layer. Through holes are respectively opened in the protective layer 460 at positions corresponding to the first electrode 451 and the second electrode 452, the first pad 471 fills the through hole and is electrically connected to the first electrode 451, and the second pad 472 fills the through hole and is electrically connected to the second electrode 452. Similarly, the sidewalls of the through hole in the protective layer 460 are also configured as the above-mentioned step structure.

[0087] Preferably, the current blocking layer 430 is made of silicon oxide, specifically including one or more of silicon oxide, silicon nitride, silicon carbide or silicon oxynitride.

[0088] Preferably, the transparent conductive layer 440 is made of a conductive material having a transparent property. In the present embodiment, the transparent conductive layer 440 is made of indium tin oxide, which mainly plays the role of ohmic contact and lateral current expansion.

[0089] Preferably, the materials of the first electrode 451, the second electrode 452 and the interconnection electrode 453 all include Au or an alloy of Au. The structure and material of the protective layer 460 are the same as those of the insulating layer provided in the above embodiment.

[0090] It should be noted that the structures of the LED chips involved in Example 1, Example 2, Example 3 and Example 4 are merely exemplary. In addition to the above-mentioned flip-chip structure LED chips, vertical structure LED chips and high-voltage structure LED chips, the LED chips claimed for protection in this application are also applicable to LED chips of other structures.

[0091] According to one aspect of the present application, an insulating layer is provided. Fig.11 and Fig.12 The insulating layer 10 at least includes a first insulating layer 11 and a second insulating layer 12 formed on the upper surface of the first insulating layer 11. The insulating layer 10 has a step structure 14, and the step structure 14 includes a first step formed by the first insulating layer 11 and a second step formed by the second insulating layer 12. The first step exceeds the second step in the horizontal direction, which can also be described as the first insulating layer 11 exceeding the second insulating layer 12 in the horizontal direction.

[0092] The insulating layer 10 is formed by at least a first insulating layer 11 and a second insulating layer 12, which can prevent cracks from occurring in the insulating layer 10 or the entire layer from breaking, thereby improving the reliability of the insulating layer 10. In addition, the first insulating layer 11 exceeds the second insulating layer 12 by a predetermined length in the horizontal direction, and the exceeding portion can play a buffering role for the second structural layer 30 in the subsequent process of forming the second structural layer 30 on the insulating layer 10, thereby reducing the stress generated inside the second structural layer 30, preventing cracks from occurring in the second structural layer 30 or the entire layer from breaking under the action of stress, thereby improving the reliability of the light-emitting diode chip using the insulating layer.

[0093] In one embodiment, the thickness of the second insulating layer 12 is greater than the thickness of the first insulating layer 11, and the thickness of the second insulating layer 12 is equal to or greater than 1 μm. Since the second insulating layer 12 has a greater thickness, the second step has a greater slope. When the second structural layer 30 is formed on the second step, the portion of the first step that exceeds the second step can better buffer the second structural layer 30, reduce the stress generated inside the second structural layer 30, and prevent the second structural layer 30 from cracking or breaking under the stress.

[0094] See also Fig.11 and Fig.12 , the angle α1 between the side of the first step and the horizontal direction is smaller than the angle α2 between the side of the second step and the horizontal direction. Preferably, the angle α1 between the side of the first step and the horizontal direction decreases in the vertical direction, and the angle α1 is between 10° and 30° or between 30° and 45°. The side of the second step is a slope surface, and the angle α2 between the slope surface and the horizontal direction is between 20° and 40°, 40° and 60° or 60° and 70°.

[0095] As an alternative embodiment, see Fig.13 , the side surfaces of the first step and the second step are vertical surfaces.

[0096] In one embodiment, see Fig.11 and Fig.12 The step structure 14 is located at the end or middle part of the insulating layer 10. The insulating layer 10 is provided with a through hole penetrating the insulating layer 10, and the side wall of the through hole is configured as the step structure 14 ( Fig.11 The end of the insulating layer 10 is configured as a step structure 14 ( Fig.12 ). When the step structure 14 is located at the end of the insulating layer 10, the portion of the first insulating layer 11 that exceeds the second insulating layer 12 in the horizontal direction can block the entry of water vapor, thereby preventing the aging failure of the light emitting diode chip.

[0097] In one embodiment, the materials used to prepare the first insulating layer 11 and the second insulating layer 12 include one or more of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. Preferably, the material used to prepare the first insulating layer 11 is aluminum oxide, and the first insulating layer 11 prepared using aluminum oxide has good water resistance. The second insulating layer 12 is a distributed Bragg reflector (DBR).

[0098] When the first insulating layer 11 is an atomic layer deposition layer, the thickness of the first insulating layer 11 is between 30 and 200 nm, preferably, the thickness of the first insulating layer 11 is between 30 and 100 nm; or, the thickness of the first insulating layer 11 is between 100 and 150 nm; or, the thickness of the first insulating layer 11 is between 150 and 200 nm. When the first insulating layer 11 is a high-density plasma chemical vapor deposition (HDPCVD) layer, the thickness of the first insulating layer 11 is between 400 and 1000 nm, preferably, the thickness of the first insulating layer 11 is between 400 and 600 nm; or, the thickness of the first insulating layer 11 is between 600 and 800 nm; or, the thickness of the first insulating layer 11 is between 800 and 1000 nm.

[0099] The density of the first insulating layer 11 is greater than the maximum density of the second insulating layer 12. The first insulating layer 11 and the second insulating layer 12 can be prepared by different processes, and the preparation materials can be the same or different. For example, when the first insulating layer 11 is an atomic layer deposition layer, the second insulating layer 12 is a high density plasma chemical vapor deposition (HDPCVD) layer, a plasma chemical vapor deposition (PECVD) layer or an evaporation deposition layer. When the first insulating layer 11 is a high density plasma chemical vapor deposition (HDPCVD) layer, the second insulating layer 12 is an evaporation deposition layer. The first insulating layer 11 and the second insulating layer 12 can also be prepared by the same preparation process, and the preparation materials of the first insulating layer 11 and the second insulating layer 12 are different. For example, the first insulating layer 11 and the second insulating layer 12 are both atomic layer deposition layers, or the first insulating layer 11 and the second insulating layer 12 are both high density plasma chemical vapor deposition (HDPCVD) layers.

[0100] Since the density of the first insulating layer 11 is greater than the maximum density of the second insulating layer 12, when the insulating layer 10 is etched by dry etching or wet etching, the etching rate of the first insulating layer 11 is lower than the etching rate of the second insulating layer 12, so a step structure 14 is formed on the insulating layer 10. Preferably, the dry etching method is an inductively coupled plasma method (ICP).

[0101] In one embodiment, see Figure 11~Figure 13, the length L1 of the first step exceeding the second step in the horizontal direction is equal to or greater than 50nm, and less than or equal to 5000nm. The size of the length L1 is related to the density between the first insulating layer 11 and the second insulating layer 12. The greater the difference in density between the first insulating layer 11 and the second insulating layer 12, the greater L1. For example, when the first insulating layer 11 is an atomic layer deposition layer, L1 is equal to or greater than 100nm, and less than or equal to 5000nm. When the first insulating layer 11 is a high-density plasma chemical vapor deposition (HDPCVD) layer, L1 is equal to or greater than 50nm, and less than or equal to 100nm.

[0102] In one embodiment, see Fig.14 The insulating layer 10 further includes a third insulating layer 13 formed on the upper surface of the second insulating layer 12. Correspondingly, the step structure 14 further includes a third step formed by the third insulating layer 13. In the horizontal direction, the length L2 of the second step beyond the third step is less than the length L1 of the first step beyond the second step.

[0103] The thickness of the third insulating layer 13 is equal to or greater than the thickness of the second insulating layer 12, and the density of the third insulating layer 13 is equal to or less than the minimum density of the second insulating layer 12. The third insulating layer 13 and the first insulating layer 11 and the second insulating layer 12 can be prepared by different processes. For example, the first insulating layer 11 is an atomic layer deposition layer, the second insulating layer 12 is a high-density plasma chemical vapor deposition (HDPCVD) layer, and the third insulating layer 13 is an evaporation deposition layer. The third insulating layer 13 and the first insulating layer 11 and the second insulating layer 12 can also be prepared by the same preparation process, and the preparation materials of the third insulating layer 13 and the first insulating layer 11 and the second insulating layer 12 are different.

[0104] According to one aspect of the present application, a method for preparing the insulating layer in the above embodiment is provided. The preparation method comprises the following steps: S1. Prepare a first insulating layer 11 and a second insulating layer 12. The thickness of the second insulating layer 12 is greater than that of the first insulating layer 11, and the thickness of the second insulating layer 12 is equal to or greater than 1 μm.

[0105] The density of the first insulating layer 11 is greater than the maximum density of the second insulating layer 12. The first insulating layer 11 and the second insulating layer 12 can be prepared by different processes, and their preparation materials include one or more of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide. For example, the first insulating layer 11 is prepared by atomic layer deposition, and the second insulating layer 12 is prepared by high-density plasma chemical vapor deposition (HDPCVD), plasma chemical vapor deposition (PECVD) or evaporation deposition. Alternatively, the first insulating layer 11 is prepared by high-density plasma chemical vapor deposition (HDPCVD), and the second insulating layer 12 is prepared by evaporation deposition.

[0106] The first insulating layer 11 and the second insulating layer 12 may also be prepared by the same preparation process, and the first insulating layer 11 and the second insulating layer 12 may be prepared by different materials. For example, the first insulating layer 11 and the second insulating layer 12 are both prepared by atomic layer deposition, or the first insulating layer 11 and the second insulating layer 12 are both prepared by high-density plasma chemical vapor deposition (HDPCVD).

[0107] Preferably, the first insulating layer 11 is made of aluminum oxide, and the first insulating layer 11 made of aluminum oxide has good water resistance. The second insulating layer 12 is a distributed Bragg reflector (DBR).

[0108] S2. Etch the insulating layer 10 and form a step structure 14 on the insulating layer 10; the step structure 14 includes a first step formed by the first insulating layer 11 and a second step formed by the second insulating layer 12. The first step exceeds the second step in the horizontal direction, which can also be described as the first insulating layer 11 exceeding the second insulating layer 12 in the horizontal direction.

[0109] The angle α1 between the side of the first step and the horizontal direction is smaller than the angle α2 between the side of the second step and the horizontal direction. Preferably, the angle α1 between the side of the first step and the horizontal direction decreases in the vertical direction, and the angle α1 is between 10° and 30° or between 30° and 45°. The side of the second step is a slope surface, and the angle α2 between the slope surface and the horizontal direction is between 20° and 40°, 40° and 60° or 60° and 70°.

[0110] As an alternative embodiment, the side surfaces of the first step and the second step are vertical surfaces.

[0111] Preferably, the length L1 of the first step exceeding the second step in the horizontal direction is equal to or greater than 50nm and less than or equal to 5000nm. The length L1 is related to the density between the first insulating layer 11 and the second insulating layer 12. The greater the difference in density between the first insulating layer 11 and the second insulating layer 12, the greater L1. For example, when the first insulating layer 11 is an atomic layer deposition layer, L1 is equal to or greater than 100nm and less than or equal to 5000nm. When the first insulating layer 11 is a high-density plasma chemical vapor deposition (HDPCVD) layer, L1 is equal to or greater than 50nm and less than or equal to 100nm.

[0112] In one embodiment, in step S1, a first insulating layer 10, a second insulating layer 12, and a third insulating layer 13 are prepared; in step S2, the insulating layer 10 is etched, and a step structure 14 is formed on the insulating layer 10, wherein the step structure 14 further includes a third step formed by the third insulating layer 13. In the horizontal direction, a length L2 of the second step exceeding the third step is less than a length L1 of the first step exceeding the second step.

[0113] It can be seen from the above technical solutions that the insulating layer 10 in the present application is formed by at least the first insulating layer 11 and the second insulating layer 12, which can prevent cracks from occurring in the insulating layer or the entire layer from breaking, thereby improving the reliability of the insulating layer. Furthermore, if the first insulating layer 11 exceeds the second insulating layer 12 by a predetermined length in the horizontal direction, the exceeding portion can play a buffering role when the second structural layer 30 is subsequently formed on the insulating layer 10, thereby reducing the stress generated inside the second structural layer 30, thereby preventing cracks from occurring in the second structural layer 30 or the entire layer from breaking under the action of stress, thereby improving the reliability of the light-emitting diode chip. In addition, if the portion of the first insulating layer 11 that exceeds the second insulating layer 12 in the horizontal direction is located at the end of the insulating layer 10, the exceeding portion can also block the entry of water vapor, thereby preventing the aging failure of the light-emitting diode chip.

[0114] The above is only a preferred implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present application. These improvements and substitutions should also be regarded as the scope of protection of the present application.

Claims

1. A light-emitting diode chip comprising a semiconductor stack layer, a transparent conductive layer and an insulating layer, It is characterized in that The insulating layer is formed on the transparent conductive layer, and the insulating layer at least includes a first insulating layer and a second insulating layer formed on the upper surface of the first insulating layer; the insulating layer is provided with a through hole penetrating the insulating layer, and the through hole has a metal layer; The thickness of the second insulating layer is greater than that of the first insulating layer, and the thickness of the second insulating layer is equal to or greater than 1 μm, and the thickness of the first insulating layer is 30 nm to 200 nm or 400 nm to 1000 nm; The orthographic projection of the side surface of the second insulating layer on the first plane is located within the orthographic projection of the first insulating layer on the first plane, and the angle α between the side surface of the first insulating layer and the horizontal direction is 1 is smaller than the angle α between the side surface of the second insulating layer and the horizontal direction 2 The first plane is the plane where the lower surface of the first insulating layer is located.

2. The light emitting diode chip according to claim 1, It is characterized in that The length L of the lower surface of the first insulating layer beyond the lower surface of the second insulating layer 1 Equal to or greater than 50nm and less than or equal to 5000nm.

3. The light emitting diode chip according to claim 1, It is characterized in that When the first insulating layer is an atomic layer deposition layer, the lower surface of the first insulating layer exceeds the lower surface of the second insulating layer by a length L 1 Equal to or greater than 100nm and less than or equal to 5000nm.

4. The light emitting diode chip according to claim 1, It is characterized in that When the first insulating layer is a high-density plasma chemical vapor deposition layer, the lower surface of the first insulating layer exceeds the lower surface of the second insulating layer by a length L 1 Equal to or greater than 50nm and less than or equal to 100nm.

5. The light emitting diode chip according to claim 1, It is characterized in that The side surface of the second insulating layer is a slope surface, and the angle α between the slope surface and the horizontal direction is 2 Between 20°~40°, 40°~60° or 60°~70°.

6. The light emitting diode chip according to claim 1, It is characterized in that The angle α between the side surface of the first insulating layer and the horizontal direction 1 Decreases in the vertical direction, and the angle α 1 Between 10°~30° or 30°~45°.

7. The light emitting diode chip according to claim 1, It is characterized in that When the first insulating layer is an atomic layer deposition layer, the thickness of the first insulating layer is between 30 and 200 nm; The second insulating layer is a plasma chemical vapor deposition layer or an evaporation deposition layer.

8. The light emitting diode chip according to claim 1, It is characterized in that When the first insulating layer is a high-density plasma chemical vapor deposition layer, the thickness of the first insulating layer is between 400 and 1000 nm; The second insulating layer is an evaporation deposition layer.

9. The light emitting diode chip according to claim 1, It is characterized in that The first insulating layer and the second insulating layer are prepared by the same preparation process, and the preparation materials of the first insulating layer and the second insulating layer are different; the preparation materials of the first insulating layer and the second insulating layer include one or more of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide or titanium oxide.

10. The light emitting diode chip according to claim 1, It is characterized in that The first insulating layer is made of aluminum oxide.

11. The light emitting diode chip according to claim 1, It is characterized in that The second insulating layer is a distributed Bragg reflector.

12. The light emitting diode chip according to claim 1, It is characterized in that The insulating layer further includes a third insulating layer formed on the upper surface of the second insulating layer; in the horizontal direction, the lower surface of the second insulating layer exceeds the lower surface of the third insulating layer by a length L 2 less than the length L of the lower surface of the first insulating layer extending beyond the second step 1 .

13. The light emitting diode chip according to claim 1, It is characterized in that A first structural layer is formed on a surface of the insulating layer close to the first insulating layer, and the first structural layer is a transparent insulating layer, a transparent conductive layer or a metal layer.

14. The light emitting diode chip according to claim 1, It is characterized in that The semiconductor stacking layer serves as a first structural layer, the insulating layer is formed on the semiconductor stacking layer, and the second insulating layer is away from the semiconductor stacking layer.

15. The light emitting diode chip according to claim 1, It is characterized in that Also includes: A substrate, serving as a first structural layer; The semiconductor stacking layer forms a mesa structure on the substrate, and the insulating layer at least covers the sidewalls of the semiconductor stacking layer and a portion of the substrate except the semiconductor stacking layer; The second insulating layer is far away from the semiconductor stacking layer.

Citation Information

Patent Citations

  • LED (Light Emitting Diode) chip provided with stepped current blocking structure and fabricating method thereof

    CN102751410A

  • Oxide semiconductor devices, methods of manufacturing oxide semiconductor devices, display devices having oxide semiconductor devices, methods of manufacturing display devices having oxide semiconductor devices

    CN102820330A

  • An OLED light emitting device and a preparation method thereof

    CN109103223A

  • Display device and its manufacturing method