Negative pole piece, preparation method of negative pole piece, secondary battery and power utilization device

By applying a fluorine-containing compound layer on the surface of the negative electrode sheet of lithium-ion batteries, the problems of uneven reaction activity and excessive by-products on the surface of the negative electrode material are solved, achieving high battery capacity and excellent rate performance.

CN118738276APending Publication Date: 2024-10-01JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949157.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The surface reactivity of the negative electrode material of lithium-ion batteries is uneven, resulting in uneven solid electrolyte phase interface and excessive by-products, resulting in low capacity and poor rate performance.

Method used

A fluorine-containing compound layer is provided on the surface of the negative electrode plate, including fluorine-containing lithium borate salt, fluorobenzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate, to form a uniform solid electrolyte interface, reduce side reactions and Protect the negative active material.

Benefits of technology

It improves the cycle stability and life of the battery, enhances the capacity and rate performance of the battery, and reduces the interface resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738276A_ABST
    Figure CN118738276A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of energy storage. The invention particularly relates to a negative pole piece and a preparation method thereof, a secondary battery and an electric device. The negative electrode plate comprises a negative electrode current collector and a first negative electrode active material layer arranged on at least one surface of the negative electrode current collector, and the first negative electrode active material layer comprises a first negative electrode active substance and a fluorine-containing compound; the fluorine-containing compound comprises one or more of fluorine-containing boric acid lithium salt, fluorobenzene, fluorine-containing siloxane, fluorine-containing phosphate and fluorine-containing carbonate, and the surface of at least part of the first negative electrode active material in the first negative electrode active material layer is coated with the fluorine-containing compound. The negative pole piece provided by the invention is applied to a secondary battery such as a lithium ion battery, an SEI film on the surface of a negative active material can be effectively adjusted, and an interface side reaction can be inhibited, so that the battery has the advantages of high capacity and excellent rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to a negative electrode plate and a preparation method thereof, a secondary battery, and an electrical device. Background Art

[0002] Lithium-ion batteries are rechargeable energy storage systems with the highest energy density among chemical and electrochemical energy storage systems, and therefore they have been used in the field of portable electronic devices, such as laptops, computers or mobile phones, and in the field of transportation, such as electric bicycles or electric cars.

[0003] At present, the negative electrode materials of lithium-ion batteries are usually graphite-based, silicon-based and tin-based negative electrode active materials. The reaction activity of the outer surface of the particles of these negative electrode active materials is uneven, resulting in uneven solid electrolyte interface (SEI) covering the negative electrode surface. At the same time, a large amount of by-products will be produced on the negative electrode surface when the battery is quickly charged, which makes the lithium battery have the disadvantages of low capacity and poor rate performance. Summary of the invention

[0004] Based on this, the present application provides a negative electrode sheet and a preparation method thereof, a secondary battery, and an electric device. The negative electrode sheet provided in the present application is applied to secondary batteries such as lithium-ion batteries, can effectively adjust the SEI film on the surface of the negative electrode active material, and can inhibit the interface side reaction, so that the battery has the advantages of high capacity and excellent rate performance.

[0005] In a first aspect of the present application, a negative electrode sheet is provided, comprising a negative electrode current collector and a first negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the first negative electrode active material layer comprises a first negative electrode active material and a fluorine-containing compound;

[0006] The fluorine-containing compound includes one or more of fluorine-containing lithium borate salt, fluorinated benzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate ester;

[0007] At least a portion of the surface of the first negative electrode active material in the first negative electrode active material layer is coated with the fluorine-containing compound.

[0008] In one embodiment, the structures of the fluorine-containing lithium borate salt, the fluorobenzene, the fluorine-containing siloxane, the fluorine-containing phosphate ester and the fluorine-containing carbonate ester are respectively shown in the following formulas (I-1) to (I-5):

[0009]

[0010] R1 is or ; wherein x1 and x2 are each independently C(=O), S(=O) or S(=O)2; y1 is independently O or C at each occurrence; y2 is independently O or C at each occurrence;

[0011] R2 is an alkyl group having 1 to 8 carbon atoms;

[0012] R 31 is an unsaturated hydrocarbon group having 2 to 5 carbon atoms; R 32 , R 33 , R 34 Each is independently an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms;

[0013] R 41 is an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms, or an alkoxy group having 1 to 5 carbon atoms substituted with one or more fluorine atoms; R 42 , R 43 Each is independently an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms;

[0014] R 51 It is -F or an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms.

[0015] In one embodiment, R1 is any of the following groups:

[0016] ;

[0017] R2 is an alkyl group having 3 to 6 carbon atoms;

[0018] R 31 is vinyl or propenyl; R 32 , R 33 , R 34 Each is independently an alkyl group having 2 to 3 carbon atoms substituted with one or more fluorine atoms;

[0019] R 41 is an alkyl group having 1 to 3 carbon atoms, an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorine atoms, or an alkoxy group having 1 to 3 carbon atoms substituted with one or more fluorine atoms; R 42 , R 43 Each is independently an ethyl group substituted with one or more fluorine atoms or a propyl group substituted with one or more fluorine atoms;

[0020] R 51 It is -F or an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorine atoms.

[0021] In one embodiment, R1 is any of the following groups:

[0022] R2 is cyclohexyl, -C(CH3)3;

[0023] R 31 is vinyl or propenyl; R 32 , R 33 , R 34 Each independently , or ;

[0024] R 41 is an alkyl group having 1 to 3 carbon atoms, , , , , , , , , , , , , , or ;

[0025] R 42 , R 43 Each independently , , , , , , , , , , or ;

[0026] R 51 For -F, , or .

[0027] In one embodiment, the fluorine-containing compound comprises , , , and One or more of .

[0028] In one embodiment, the mass percentage of the fluorine-containing compound in the first negative electrode active material layer is 0.1% to 3.5%.

[0029] In one embodiment, the first negative electrode active material layer includes a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a mass ratio of (94-96): (1-3): (1-3): (0.1-3.5).

[0030] In one embodiment, the first negative electrode active material includes graphite.

[0031] In one embodiment, the thickness of the first negative electrode active material layer is 95 μm to 115 μm.

[0032] In one embodiment, the negative electrode sheet further includes a second material layer disposed on at least one surface of the first negative electrode active material layer, wherein the second material layer includes a lithium-containing compound.

[0033] The lithium-containing compound includes one or more of lithium phosphorus oxygen nitrogen, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium silicon phosphorus sulfur chlorine.

[0034] In one embodiment, the lithium-containing compound includes Li 11-a Ge 2-a P 1+a S 12 , Li 6-b PS 5-b Cl 1+b , Li 9.54±m1 Si 1.74±m2 P 1.44±m3 S 11.7±m4 Cl 0.3±m5 and Li n1 PO n2 N n3 One or more of;

[0035] Among them, 0.5≤a≤1.5, 0≤b≤0.6, 0≤m1≤2, 0≤m2≤0.3, 0≤m3≤0.4, 0≤m4≤0.2, 0≤m5≤0.2, 0 <n1≤1,0<n2≤1,0<n3≤1。

[0036] In one embodiment, the lithium-containing compound includes Li 10 GeP2S 12 、Li6PS5Cl、Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 and LiPON or more.

[0037] In one embodiment, the second material layer includes a second binder and a lithium-containing compound in a mass ratio of (45-30):(55-70).

[0038] In one embodiment, the thickness of the second negative electrode active material layer is 1 μm to 5 μm.

[0039] In a second aspect of the present application, there is provided a method for preparing the negative electrode sheet according to any one of the embodiments of the first aspect of the present application, comprising the following steps:

[0040] Mixing a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a first solvent to prepare a first active slurry;

[0041] Applying the first active slurry on the surface of the negative electrode current collector and drying it to prepare the first negative electrode active material layer;

[0042] The fluorine-containing compound includes one or more of fluorine-containing lithium borate salt, fluorobenzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate ester.

[0043] In one embodiment, the preparation method further comprises the following steps:

[0044] Mixing a second binder and a lithium-containing compound to prepare a mixture;

[0045] Applying the mixed material on the surface of the first negative electrode active material layer to prepare the second material layer;

[0046] The lithium-containing compound includes one or more of lithium phosphorus oxygen nitrogen, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium silicon phosphorus sulfur chlorine.

[0047] A third aspect of the present application provides a secondary battery, comprising the negative electrode sheet described in any one of the embodiments of the first aspect of the present application.

[0048] A fourth aspect of the present application provides an electrical device comprising the lithium-ion battery described in the third aspect of the present application.

[0049] The present application sets a first negative electrode active material layer including a fluorine-containing compound on the surface of the negative electrode current collector, and the surface of at least part of the first negative electrode active material in the first negative electrode active material layer is coated with the fluorine-containing compound, so that when the first negative electrode active material layer contacts the electrolyte, the fluorine-containing compound therein can react with the lithium ions in the electrolyte to form a uniform and conductive solid electrolyte interface (SEI) film; this helps to reduce the instability of the SEI layer and improve the cycle stability and life of the battery. At the same time, the fluorine-containing compound can protect the first negative electrode active material to reduce side reactions such as the dissolution and precipitation of lithium between negative electrode active materials such as graphite and the electrolyte, which helps to slow down the degradation rate of the electrode material and extend the cycle life of the battery. In addition, the fluorine-containing compound can also improve the interface performance between the electrode and the electrolyte, reduce the interface resistance, and further improve the capacity performance of the battery.

[0050] Furthermore, the fluorine-containing compounds provided in the present application include fluorine-containing lithium borate salts, fluorobenzene, fluorine-containing siloxanes, fluorine-containing phosphates and fluorine-containing carbonates; these fluorine-containing compounds are easy to obtain, which is conducive to the large-scale application of the negative electrode plates of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is the impedance test diagram of Example 2 and Example 3 of the present application. DETAILED DESCRIPTION

[0052] The following is a further complete and clear description of the negative electrode sheet and its preparation method, lithium-ion battery, and electrical device of the present application in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0053] In the present application, "substituted" means that a hydrogen atom in a substituted group is replaced by a substituent.

[0054] In the present application, "alkyl" can represent straight chain, branched and / or cyclic alkyl. Phrases containing this term, for example, "alkyl having 1 to 8 carbon atoms" refer to alkyls containing 1 to 8 carbon atoms, and each occurrence can be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl. Non-limiting examples of alkyl include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, 2-ethylbutyl, 3,3-dimethylbutyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, cyclopentyl, 1-methylpentyl, 3-methylpentyl, 4-methyl-2-pentyl, n-hexyl or cyclohexyl.

[0055] In the present application, "unsaturated hydrocarbon group" refers to a hydrocarbon group containing a double bond or a triple bond. It can be an alkenyl group with one double bond, or a dienyl group, a trienyl group, etc. with two or more double bonds. It can be an alkynyl group with one triple bond, or a dialkynyl group with two or more triple bonds. It can be straight-chain or branched. The "unsaturated hydrocarbon group having 2 to 5 carbon atoms" containing this term means that the number of carbon atoms constituting the unsaturated hydrocarbon group is 2 to 5, and each time it appears, the number of carbon atoms can be 2, 3, 4 or 5 independently of each other. Among them, as a straight-chain unsaturated hydrocarbon group with one double bond in the hydrocarbon group, suitable examples include but are not limited to: vinyl, propenyl, butenyl, pentenyl, etc. As a branched unsaturated hydrocarbon group with one double bond in the hydrocarbon group, suitable examples include but are not limited to: propenyl, etc.

[0056] In the present application, "alkoxy" refers to a group having -O-alkyl, i.e., an alkyl group as defined above is connected to a parent core structure via an oxygen atom. Phrases containing the term, for example, "alkoxy having 1 to 5 carbon atoms" means that the alkyl portion contains 1 to 5 carbon atoms, and each occurrence may be independently C1 alkoxy, C4 alkoxy, or C5 alkoxy. Suitable examples include, but are not limited to, methoxy (-O-CH3 or -OMe), ethoxy (-O-CH2CH3 or -OEt) and tert-butoxy (-OC(CH3)3 or -OtBu).

[0057] In this application, " " represents a connection site or a fusion site. In the present application, when a connection site is not specified in a group, it means that an optional connection site in the group is used as a connection site; in the present application, when a fusion site is not specified in a group, it means that an optional fusion site in the group is used as a fusion site, and preferably two or more sites in adjacent positions in the group are fusion sites.

[0058] In the present application, when a linking site is not specified in a group, it means that an optional linking site in the group can be used as a linking site.

[0059] In the present application, the single bond to which the substituent is connected runs through the corresponding ring, indicating that the substituent can be connected to any position of the ring, for example R is connected to any substitutable site of the benzene ring. The particle reactivity of graphite, silicon-based and tin-based negative electrode materials is uneven, the grain size is large, the surface crystal structure is easily destroyed during charging and discharging, and the SEI covering the surface is uneven, which makes the lithium battery have the disadvantages of low capacity and poor rate performance.

[0060] At present, in order to improve the uniformity of the reaction activity of the negative electrode material and enhance the electrochemical performance of the battery, the relevant technology usually requires the modification of the negative electrode active material. Taking graphite-based negative electrode active materials as an example, the current methods for modifying graphite mainly include the following: (1) First, the graphite is crushed and graded to obtain a shaped graphite material, and then high-temperature oxidation, hot pressing, static impregnation, granulation, and graphitization are performed to obtain modified graphite. (2) The graphite is dried, ball-milled and sieved, and then silicon nanofibers and amorphous carbon are deposited on the surface of natural graphite particles by chemical vapor deposition. (3) Composite modifiers such as strongly oxidizing acids, gases, and ionic liquids are used to modify graphite. (4) Add easily graphitizable adhesives such as petroleum asphalt, coal tar, phenolic resin, epoxy resin, furan resin, etc. to the graphite raw material, and then perform low-temperature heat treatment at 300℃~800℃ for 10h~20h, and then perform high-temperature treatment at 2800℃~3000℃ for 24h~48h.

[0061] As can be seen from the above, the main modification methods currently focus on the raw materials of negative electrode active materials, and most of them require cumbersome processes, such as drying, ball milling and screening, high-temperature oxidation and graphitization, etc. These steps are time-consuming and it is difficult to achieve the goal of large-scale application of lithium-ion batteries by relying on large-scale production.

[0062] Based on this, the present application provides a negative electrode plate, in which the selected fluorine-containing compounds can protect the surface of negative electrode active material particles such as graphite. At the same time, these fluorine-containing compounds are easy to obtain, which is conducive to large-scale application.

[0063] In a first aspect of the present application, a negative electrode sheet is provided, comprising a negative electrode current collector and a first negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the first negative electrode active material layer comprises a first negative electrode active material and a fluorine-containing compound;

[0064] The fluorine-containing compound includes one or more of fluorine-containing lithium borate salt, fluorinated benzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate ester;

[0065] At least a portion of the surface of the first negative electrode active material in the first negative electrode active material layer is coated with the fluorine-containing compound.

[0066] The present application sets a first negative electrode active material layer including a fluorine-containing compound on the surface of the negative electrode current collector, and the surface of at least part of the first negative electrode active material in the first negative electrode active material layer is coated with the fluorine-containing compound, so that when the first negative electrode active material layer contacts the electrolyte, the fluorine-containing compound therein can react with the lithium ions in the electrolyte to form a uniform and conductive solid electrolyte interface (SEI) film; this helps to reduce the instability of the SEI layer and improve the cycle stability and life of the battery. At the same time, the fluorine-containing compound can protect the negative electrode active particles to reduce side reactions such as the dissolution and precipitation of lithium between the negative electrode active materials such as graphite and the electrolyte, which helps to slow down the degradation rate of the electrode material and extend the cycle life of the battery. In addition, the fluorine-containing compound can also improve the interface performance between the electrode and the electrolyte, reduce the interface resistance, and further improve the capacity performance of the battery.

[0067] Furthermore, the fluorine-containing compounds provided in the present application include fluorine-containing lithium borate salts, fluorobenzenes, fluorine-containing siloxanes, fluorine-containing phosphates and fluorine-containing carbonates; these fluorine-containing compounds are easily available and are conducive to large-scale applications.

[0068] In one example, the structures of the fluorine-containing lithium borate salt, the fluorobenzene, the fluorine-containing siloxane, the fluorine-containing phosphate ester and the fluorine-containing carbonate ester are respectively shown in the following formulas (I-1) to (I-5): .

[0069] In one example, in formula (I-1),

[0070] R1 is or ; wherein x1 and x2 are each independently C(=O), S(=O) or S(=O)2; y1 is independently O or C each time it appears; y2 is independently O or C each time it appears.

[0071] In one example, R1 is any of the following groups:

[0072]

[0073] .

[0074] Furthermore, in formula (I-1), R1 is any of the following groups:

[0075] Furthermore, in formula (I-1), R1 is any of the following groups: .

[0076] In one specific example, the fluorine-containing compound represented by formula (I-1) includes one or more of the following compounds:

[0077]

[0078] .

[0079] In a more specific example, the fluorine-containing compound represented by formula (I-1) includes one or more of the following compounds: .

[0080] In one example, in formula (I-2), R2 is an alkyl group having 1 to 8 carbon atoms.

[0081] Furthermore, in formula (I-2), R2 is an alkyl group having 3 to 6 carbon atoms.

[0082] Furthermore, R2 is cyclohexyl or -C(CH3)3.

[0083] In one specific example, the fluorine-containing compound represented by formula (I-2) includes one or more of the following compounds: , .

[0084] In a more specific example, the fluorine-containing compound represented by formula (I-2) includes one or more of the following compounds: 1-fluoro-2-cyclohexylbenzene , 1-Fluoro-3-cyclohexylbenzene , 1-Fluoro-4-cyclohexylbenzene , 1-Fluoro-2-tert-butylbenzene , 1-Fluoro-3-tert-butylbenzene , 1-Fluoro-4-tert-butylbenzene .

[0085] In one example, in formula (I-3), R 31 is an unsaturated hydrocarbon group having 2 to 5 carbon atoms; R 32 , R 33 , R 34 Each is independently an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms.

[0086] Furthermore, in formula (I-3), R 31 is vinyl or propenyl; R 32 , R 33 , R 34 Each is independently an alkyl group having 2 to 3 carbon atoms substituted with one or more fluorine atoms.

[0087] Furthermore, R 31 is vinyl or propenyl; R 32 , R 33 , R 34 Each independently , or .

[0088] In one specific example, the fluorine-containing compound represented by formula (I-3) includes one or more of the following compounds: .

[0089] In one example, in formula (I-4), R 41 is an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms, or an alkoxy group having 1 to 5 carbon atoms substituted with one or more fluorine atoms; R 42 , R 43 Each is independently an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms.

[0090] Furthermore, in formula (I-4), R 41 is an alkyl group having 1 to 3 carbon atoms, an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorine atoms, or an alkoxy group having 1 to 3 carbon atoms substituted with one or more fluorine atoms; R 42 , R 43 Each independently represents an ethyl group substituted with one or more fluorine atoms or a propyl group substituted with one or more fluorine atoms.

[0091] Furthermore, in formula (I-4), R 41is an alkyl group having 1 to 3 carbon atoms, , or , , , , , , , , , , , or ; R 42 , R 43 Each independently , , , , , , , , , , or .

[0092] In one specific example, the fluorine-containing compound represented by formula (I-4) includes one or more of tris(2,2,2-trifluoroethyl) phosphate, bis(2,2,2-trifluoroethyl) methyl phosphate, bis(2,2,2-trifluoroethyl) ethyl phosphate, bis(2,2-difluoroethyl) 2,2,2-trifluoroethyl phosphate, bis(2,2,2-trifluoroethyl) 2,2-difluoroethyl phosphate, bis(2,2,3,3-tetrafluoropropyl) 2,2,2-trifluoroethyl phosphate, bis(2,2,2-trifluoroethyl) 2,2,3,3-tetrafluoropropyl phosphate and (2,2,2-trifluoroethyl) (2,2,3,3-tetrafluoropropyl) methyl phosphate.

[0093] In one specific example, the fluorine-containing compound represented by formula (I-4) includes one or more of the following compounds:

[0094]

[0095] .

[0096] In one example, in formula (I-5), R 51 It is -F or an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms.

[0097] Furthermore, in formula (I-5), R 51 It is -F or an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorine atoms.

[0098] Furthermore, in formula (I-5), R 51 For -F, , or .

[0099] In one specific example, the fluorine-containing compound represented by formula (I-5) includes one or more of the following compounds: .

[0100] In a more specific example, the fluorine-containing compound includes , , , and One or more of .

[0101] The content of fluorine-containing compounds plays an important role in helping to form a more stable SEI film and preventing it from reacting adversely with the electrolyte, thereby extending the cycle life of the battery. In one example, the mass percentage of the fluorine-containing compound in the first negative electrode active material layer is 0.1% to 3.5%. It is understandable that the mass percentage of the fluorine-containing compound in the first negative electrode active material layer includes but is not limited to 0.2%, 0.5%, 0.6%, 0.7%, 0.8%, 1%, 1.1%, 1.2%, 1.3%, 1.5%, 1.7%, 2%, 2.1%, 2.2%, 2.3%, 2.5%, 2.8%, 3%, 3.2% or 3.5%.

[0102] Limiting the amount of conductive agent added can improve the conductivity of the electrode and reduce the internal resistance of the electrode; in addition, the binder can enhance the bonding force between the active material particles and the electrode current collector, and improve the mechanical strength and cycle stability of the electrode. Therefore, precisely controlling the ratio of the first negative electrode active material, the conductive agent, the binder and the fluorine-containing compound can optimize the performance of the battery. In one example, the first negative electrode active material layer includes a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a mass ratio of (94~96): (1~3): (1~3): (0.1~3.5). Specifically, the mass ratio of the first negative electrode active material, the first conductive agent, the first binder and the fluorine-containing compound includes but is not limited to 94:1.5:0.8:3, 94.5:1:0.8:3, 94.9:1.2:1:2.2, 95:1.1:1:2.2, 94.9:1.2:2:1.2, 95:1.1:2:1.2, 95:1:2:1.3, 95:1.6:2:0.7, 95.3:1.3:2:0.7, 95.4:1.2:2:0.6, 95.5:1.5:1.6:0.7, 95.7:2:0.9:0.7 or 96:1:0.3:2. In a more specific example, the first negative electrode active material layer includes a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a mass ratio of (94.9-95.4): (1-1.5): (1.5-2.5): (0.5-1.5).

[0103] In one example, the first negative electrode active material layer also includes a thickener. For example, the types of thickeners include but are not limited to sodium carboxymethyl cellulose. Specifically, the first negative electrode active material layer includes a first negative electrode active material, a first conductive agent, a first binder, a fluorine-containing compound and a thickener in a mass ratio of (94~96): (1~3): (1~3): (0.1~3.5): (1~1.5). Specifically, the mass ratio of the first negative electrode active material, the first conductive agent, the first binder, the fluorine-containing compound and the thickener includes but is not limited to 94:1.5:0.8:3:0.7, 94.5:1:0.8:3:0.7, 94.9:1.2:1:2.2:0.7, 95:1.1:1:2.2:0.7, 94.9:1.2:2:1.2:0.7, 95:1 .1:2:1.2:0.7, 95:1:2:1.3:0.7, 95:1.6:2:0.7:0.7, 95.3:1.3:2:0.7:0.7, 95.4:1.2:2:0.6:0.7, 95.5:1.5:1.6:0.7:0.7, 95.7:2:0.9:0.7:0.7 or 96:1:0.3:2:0.7.

[0104] The surface crystal structure of natural graphite powder is easily destroyed during the charging and discharging process, and the SEI covering the surface is uneven, which will result in low initial coulombic efficiency and poor rate performance, so the application of natural graphite in lithium battery materials is showing a downward trend. In one example, the first negative electrode active material includes graphite. Fluorine-containing compounds can protect natural graphite particles to reduce side reactions such as dissolution and precipitation of lithium between graphite negative electrode active materials and electrolytes, which helps to slow down the degradation rate of electrode materials and extend the cycle life of batteries.

[0105] In one example, the thickness of the first negative electrode active material layer is 95 μm to 115 μm. Specifically, the thickness of the first negative electrode active material layer includes but is not limited to 98 μm, 100 μm, 105 μm, 108 μm, 110 μm, 112 μm or 115 μm.

[0106] In one example, the negative electrode sheet further includes a second material layer disposed on at least one surface of the first negative electrode active material layer, the second material layer includes a lithium-containing compound,

[0107] The lithium-containing compound includes one or more of lithium phosphorus oxygen nitrogen, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium silicon phosphorus sulfur chlorine.

[0108] The addition of different types of lithium-containing compounds to the second material layer can also improve the cycle stability of the battery, which increases the diversity and flexibility of battery design. However, the addition of the second material layer may lead to interface effects between the first negative electrode active material layer and the second material layer, such as reduced electrolyte permeability, obstruction of electronic conduction, etc. These effects will lead to a slight decrease in battery capacity and a slight decrease in capacity retention rate; however, compared with the negative electrode sheet that does not include lithium-containing compounds and fluorine-containing compounds, the addition of the second material layer can still significantly improve the battery capacity and retention rate.

[0109] In one example, the lithium-containing compound includes Li 11-a Ge 2-a P 1+a S 12 , Li 6-b PS 5-b Cl 1+b , Li 9.54±m1 Si 1.74±m2 P 1.44±m3 S 11.7±m4 Cl 0.3±m5 and Li n1 PO n2 N n3 One or more of;

[0110] Among them, 0.5≤a≤1.5, 0≤b≤0.6, 0≤m1≤2, 0≤m2≤0.3, 0≤m3≤0.4, 0≤m4≤0.2, 0≤m5≤0.2, 0 <n1≤1,0<n2≤1,0<n3≤1。

[0111] Specifically, the value of a includes, but is not limited to, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, or 1.5. The value of b includes, but is not limited to, 0, 0.1, 0.2, 0.3, 0.4, 0.5, or 0.6. The value of m1 includes, but is not limited to, 0, 0.1, 0.3, 0.5, 0.7, 0.9, 1.1, 1.3, 1.5, 1.7, or 2. The value of m2 includes, but is not limited to, 0, 0.1, 0.2, 0.3. The value of m3 includes, but is not limited to, 0, 0.1, 0.2, 0.3, or 0.4. The value of m4 includes, but is not limited to, 0, 0.1, or 0.2. The value of m5 includes, but is not limited to, 0, 0.1, or 0.2. The value of n1 includes, but is not limited to, 0.1, 0.3, 0.5, 0.7, 0.8, 0.9, or 1. The value of n2 includes, but is not limited to, 0.1, 0.3, 0.5, 0.7, 0.8, 0.9 or 1. The value of n3 includes, but is not limited to, 0.1, 0.3, 0.5, 0.7, 0.8, 0.9 or 1.

[0112] In one example, the lithium-containing compound includes Li 10 GeP2S 12 、Li6PS5Cl、Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 and LiPON or more.

[0113] In one example, the second material layer includes a second binder and a lithium-containing compound in a mass ratio of (45-30):(55-70). Specifically, the mass ratio of the second binder and the lithium-containing compound includes but is not limited to 45:55, 40:60, 35:65, and 30:70.

[0114] In the present application, the negative electrode current collector may be copper, and the shape of the negative electrode current collector is not particularly limited, and may be a rod, plate, sheet, or foil, and may vary depending on the shape of the lithium ion secondary battery.

[0115] It is understandable that the first conductive agent of the present application can be selected from common conductive agents in the art. For example, the first conductive agent is selected from one or more of conductive carbon black, Ketjen black, graphene carbon fiber, acetylene black and carbon nanotubes.

[0116] It is understandable that the first binder and the second binder of the present application can be selected from commonly used binders in the art. For example, the types of binders include butadiene styrene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0117] In one specific example, the first binder and the second binder are each independently selected from polyacrylic acid. More specifically, the viscosity of polyacrylic acid is 4000 mPa·s to 22000 mPa·s. The viscosity of polyacrylic acid includes but is not limited to 4000 mPa·s, 6000 mPa·s, 8000 mPa·s, 10000 mPa·s, 12000 mPa·s, 14000 mPa·s, 16000 mPa·s, 18000 mPa·s, 20000 mPa·s, and 22000 mPa·s.

[0118] In one example, the thickness of the second material layer is 1 μm to 5 μm. Specifically, the thickness of the second material layer includes but is not limited to 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.8 μm, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm, 3.2 μm, 3.5 μm, 3.8 μm, 4 μm, 4.2 μm, 4.5 μm, 4.8 μm or 5 μm.

[0119] In a second aspect of the present application, there is provided a method for preparing a negative electrode sheet as described in any example of the first aspect of the present application, comprising the following steps:

[0120] a1. Mixing a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a first solvent to prepare a first active slurry;

[0121] a2. Applying the first active slurry on the surface of the negative electrode current collector and drying it to prepare the first negative electrode active material layer;

[0122] The fluorine-containing compound includes one or more of fluorine-containing lithium borate salt, fluorobenzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate ester.

[0123] In one example, the preparation method further includes the following steps:

[0124] b1, mixing the second binder and the lithium-containing compound to prepare a mixture;

[0125] b2, coating the mixed material on the surface of the first negative electrode active material layer to prepare the second negative material layer;

[0126] The lithium-containing compound includes one or more of lithium phosphorus oxygen nitrogen, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium silicon phosphorus sulfur chlorine.

[0127] In one example, the solid content of the first active slurry is 40% to 70%. Specifically, the solid content of the first active slurry includes but is not limited to 45%, 50%, 55%, 60%, 65% or 70%.

[0128] In addition, in the step of preparing the first active slurry in step a1, a thickener may also be added. For example, the types of thickeners include but are not limited to sodium carboxymethyl cellulose.

[0129] In one example, in step b1, the process parameters for drying include: a drying temperature of 70°C to 90°C.

[0130] In a third aspect of the present application, a secondary battery is provided, comprising the negative electrode sheet described in any example of the first aspect of the present application. In one example, the secondary battery comprises: the negative electrode sheet described in any example of the first aspect of the present application, and

[0131] The positive electrode plate is arranged opposite to the negative electrode plate.

[0132] Without limitation, the positive electrode sheet can be selected from commonly used positive electrode sheets of technicians in this field. For example, the positive electrode sheet includes a positive current collector and a positive active material layer located on the positive current collector. Specifically, the positive current collector includes an aluminum foil current collector. Further, the composition of the positive active material layer includes a positive active material, a conductive agent and a binder. The positive active material can be, for example, lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material, lithium manganese oxide (LiMn2O4), lithium nickel manganese oxide (LiNi 0.5 Mn 1.5 O4) and lithium iron phosphate (LiFePO4) or more.

[0133] In addition, the secondary battery may further include a diaphragm and an electrolyte, which are disposed between the positive electrode and the negative electrode. Without limitation, the diaphragm may be selected from diaphragms commonly used in lithium-ion secondary batteries, such as polyolefin films, including microporous films made of polyethylene and polypropylene; multilayer films of porous polyethylene and polypropylene; non-woven fabrics formed of polyester fibers, aramid fibers, glass fibers, etc.; and base films formed of ceramic particles such as silicon dioxide, aluminum oxide, and titanium dioxide attached to their surfaces. In some embodiments, the diaphragm is a three-layer film of PP / PE / PP coated with aluminum oxide on both sides.

[0134] The electrolyte may include an electrolyte and a non-aqueous organic solvent. The electrolyte is preferably LiPF6, LiBF4, LiSbF6, LiAsF6. The non-aqueous organic solvent may be a carbonate, an ester, and an ether. Among them, carbonates such as ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) may be preferably used.

[0135] In a fourth aspect of the present application, there is provided an electrical device, comprising the lithium-ion battery described in the third aspect of the present application. Specifically, the electrical device may be, for example, a smart wearable device, a computer, a smart phone, a camera, a drone, an electric car, etc.

[0136] The following further specific examples are provided to explain the present application in detail. It should also be understood that the following examples are only used to further explain the present application and cannot be understood as limiting the scope of protection of the present application. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present application belong to the scope of protection of the present application. The specific process parameters of the following embodiments are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not necessarily limited to the specific values ​​of the embodiments below.

[0137] [Binder]

[0138] Polyacrylic acid, viscosity: about 21000 mPa·s.

[0139] Example 1

[0140] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (a mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing compound fluorine-containing boric acid lithium salt (the specific structure of the fluorine-containing boric acid lithium salt is shown in Table 1) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 95.4%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorine-containing boric acid lithium salt is 0.7%.

[0141] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of the components in the first negative electrode active material layer were as shown in Table 1, and a graphite electrode was obtained.

[0142] Example 2

[0143] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing compound fluorine-containing boric acid lithium salt (the specific structure of the fluorine-containing boric acid lithium salt is shown in Table 1) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 94.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorine-containing boric acid lithium salt is 1.2%.

[0144] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of the components in the first negative electrode active material layer were as shown in Table 1, and a graphite electrode was obtained.

[0145] Example 3

[0146] (1) The first active material graphite and the first conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the first binder polyacrylic acid is added and stirred for another 2 hours; some deionized water can be added to adjust the consistency of the slurry. Finally, the fluorine-containing compound fluorine-containing boric acid lithium salt (the specific structure of the fluorine-containing boric acid lithium salt is shown in Table 1) is added and stirred for about 30 minutes to form a first active material slurry; wherein the solid content of the first active slurry is 50%. In the solid of the first active slurry, the mass fraction of the active material graphite is 94.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorine-containing boric acid lithium salt is 1.2%.

[0147] (2) coating the first active slurry of step (1) on both sides of the copper foil, and then drying at 80° C. to form a first negative electrode active material layer with a thickness of 107 μm;

[0148] (3) Mixing the lithium-containing compound LiPON and the second binder polyacrylic acid for about 30 minutes to prepare a mixture; coating the mixture on the surface of the first negative electrode active material layer to prepare a second material layer. In the second material layer, the mass fraction of the second binder polyacrylic acid is 45%, and the mass fraction of the lithium-containing compound LiPON is 55%.

[0149] (4) The second active slurry of step (3) was coated on both sides of the first negative electrode active material layer, and then dried at 80° C. to form a second material layer with a thickness of 3 μm; the contents of each component in the first negative electrode active material layer and the second material layer were as shown in Table 1, and a graphite electrode was obtained.

[0150] Example 4

[0151] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; some deionized water can be added to adjust the consistency of the slurry. Finally, the fluorinated additive fluorobenzene (the specific structure of fluorobenzene is shown in Table 1) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 94.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorinated compound fluorobenzene is 1.2%.

[0152] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of the components in the first negative electrode active material layer were as shown in Table 1, and a graphite electrode was obtained.

[0153] Example 5

[0154] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing additive fluorinated silicone (the specific structure of the fluorinated silicone is shown in Table 1) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 94.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorinated compound fluorinated silicone is 1.2%.

[0155] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of the components in the first negative electrode active material layer were as shown in Table 1, and a graphite electrode was obtained.

[0156] Example 6

[0157] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing additive fluorine-containing phosphate (the specific structure of the fluorine-containing phosphate is shown in Table 2) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 94.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorine-containing phosphate is 1.2%.

[0158] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of each component in the first negative electrode active material layer were as shown in Table 2, and a graphite electrode was obtained.

[0159] Example 7

[0160] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing additive fluorocarbonate (the specific structure of the fluorocarbonate is shown in Table 2) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 94.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorocarbonate is 1.2%.

[0161] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of each component in the first material layer were as shown in Table 2, and a graphite electrode was obtained.

[0162] Example 8

[0163] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing additive fluorocarbonate (the specific structure of the fluorocarbonate is shown in Table 2) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 92.6%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorocarbonate is 3.5%.

[0164] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of each component in the first material layer were as shown in Table 2, and a graphite electrode was obtained.

[0165] Example 9

[0166] (1) The active material graphite and the conductive agent conductive carbon black are dry mixed by slow stirring for about 10 minutes; then, sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) is added and dispersed for about 60 minutes, and after being fully stirred, the binder polyacrylic acid is added and stirred for another 2 hours; according to the consistency of the slurry, some deionized water can be added for adjustment. Finally, the fluorine-containing additive fluorocarbonate (the specific structure of the fluorocarbonate is shown in Table 2) is added and stirred for about 30 minutes to form an active material slurry; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 95.9%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, the mass fraction of the binder polyacrylic acid is 2.0%, and the mass fraction of the fluorine-containing compound fluorocarbonate is 0.2%.

[0167] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of each component in the first material layer were as shown in Table 2, and a graphite electrode was obtained.

[0168] Comparative Example 1

[0169] (1) Dry-mix the active material graphite and the conductive agent conductive carbon black by slow stirring for about 10 minutes; then add sodium carboxymethyl cellulose glue (mixed solution of thickener sodium carboxymethyl cellulose and deionized water) and disperse for about 60 minutes. After fully stirring, add the binder polyacrylic acid and stir for another 2 hours; according to the consistency of the slurry, some deionized water can be added to adjust. Active material slurry is formed; wherein the solid content of the active slurry is 50%. In the solid of the active slurry, the mass fraction of the active material graphite is 96.1%, the mass fraction of the conductive agent conductive carbon black is 1.2%, the mass fraction of the thickener sodium carboxymethyl cellulose is 0.7%, and the mass fraction of the binder polyacrylic acid is 2.0%.

[0170] (2) The active slurry of step (1) was coated on both sides of the copper foil, and then dried at 80° C. to form a first negative electrode active material layer with a thickness of 110 μm; the contents of each component in the first negative electrode active material layer were as shown in Table 2, and a graphite electrode was obtained.

[0171] The graphite pole pieces prepared in the above-mentioned embodiments and comparative examples are assembled into lithium-ion batteries according to the following steps.

[0172] (1) Preparation of positive electrode sheet

[0173] Lithium iron phosphate positive electrode active material, conductive carbon black and polyvinylidene fluoride are dispersed in N-methylpyrrolidone at a weight ratio of 94:2:4, and mixed evenly to prepare positive electrode slurry. The uniform positive electrode slurry is evenly coated on the aluminum foil current collector and dried at 55°C to obtain a 130µm positive electrode active material layer; a positive electrode sheet is prepared.

[0174] (2) Assembling lithium-ion batteries

[0175] The graphite pole piece prepared in the above-mentioned embodiment and comparative example is used as the negative electrode of the battery, and a three-layer film of PP / PE / PP coated with aluminum oxide on both sides is placed between the positive pole piece and the negative electrode as a separator, and a conventional carbonate electrolyte is added dropwise. The positive pole piece prepared in step (1) is used as the positive electrode to assemble into a lithium-ion battery.

[0176] The following tests were performed on the lithium-ion batteries assembled from the graphite pole pieces prepared in the examples and comparative examples: the lithium-ion batteries were placed in a 25°C constant temperature chamber for 6 hours to allow the lithium-ion batteries to reach a constant temperature. The constant temperature lithium-ion batteries were cycled at 1C within the range of 3.65V-2V, the corresponding cycle data were recorded, and the capacity retention rate of the corresponding lithium-ion batteries after 1000 cycles was calculated.

[0177] The corresponding performance test results of the lithium-ion batteries assembled from the graphite pole pieces in the embodiments and comparative examples are shown in Table 3.

[0178] Table 1

[0179]

[0180] Table 2

[0181]

[0182] Table 3

[0183]

[0184] From the comparison between the above embodiments and the comparative examples, it can be seen that by adding fluorine-containing compounds to the first negative electrode active material, the capacity and cycle performance of the lithium-ion battery can be effectively improved. The addition of the second material layer in Example 3 results in slightly lower initial capacity and capacity retention rate than in Example 2, but its performance is better than that of Comparative Example 1; this shows that the provision of the first negative electrode active material layer of the present application can increase the diversity and flexibility of battery design, for example, it can be redesigned based on the first negative electrode active material layer of the present application.

[0185] in addition, Figure 1 The impedance test diagrams of Example 2 and Example 3 are shown in FIG. Figure 1It can be seen that the impedance value of Example 2 is greater than that of Example 3, which indicates that the interface impedance of the second material layer containing LiPON is slightly larger, which has a slight impact on the cycle performance (capacity and retention rate), but is still better than Examples 4, 5, 7, 8, and 9.

[0186] Among all the embodiments, the performance of embodiment 6 is the best, which is mainly due to the combination of "phosphoric acid" and "fluorine".

[0187] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0188] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A negative electrode plate, characterized in that: The invention comprises a negative electrode current collector and a first negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the first negative electrode active material layer comprises a first negative electrode active material and a fluorine-containing compound; The fluorine-containing compound includes one or more of fluorine-containing lithium borate salt, fluorinated benzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate ester; At least a portion of the surface of the first negative electrode active material in the first negative electrode active material layer is coated with the fluorine-containing compound.

2. The negative electrode sheet according to claim 1, characterized in that: The structures of the fluorine-containing lithium borate salt, the fluorobenzene, the fluorine-containing siloxane, the fluorine-containing phosphate ester and the fluorine-containing carbonate ester are respectively shown in the following formulas (I-1) to (I-5): R1 is or ; wherein x1 and x2 are each independently C(=O), S(=O) or S(=O)2; y1 is independently O or C at each occurrence; y2 is independently O or C at each occurrence; R2 is an alkyl group having 1 to 8 carbon atoms; R 31 is an unsaturated hydrocarbon group having 2 to 5 carbon atoms; R 32 , R 33 , R 34 Each is independently an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms; R 41 is an alkyl group having 1 to 5 carbon atoms, an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms, or an alkoxy group having 1 to 5 carbon atoms substituted with one or more fluorine atoms; R 42 , R 43 Each is independently an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms; R 51 It is -F or an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms.

3. The negative electrode sheet according to claim 2, characterized in that: R1 is any of the following groups: ; R2 is an alkyl group having 3 to 6 carbon atoms; R 31 is vinyl or propenyl; R 32 , R 33 , R 34 Each is independently an alkyl group having 2 to 3 carbon atoms substituted with one or more fluorine atoms; R 41 is an alkyl group having 1 to 3 carbon atoms, an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorine atoms, or an alkoxy group having 1 to 3 carbon atoms substituted with one or more fluorine atoms; R 42 , R 43 Each is independently an ethyl group substituted with one or more fluorine atoms or a propyl group substituted with one or more fluorine atoms; R 51 It is -F or an alkyl group having 1 to 3 carbon atoms substituted with one or more fluorine atoms.

4. The negative electrode sheet according to claim 2, characterized in that: R1 is any of the following groups: R2 is cyclohexyl, -C(CH3)3; R 31 is vinyl or propenyl; R 32 , R 33 , R 34 Each independently , or ; R 41 is an alkyl group having 1 to 3 carbon atoms, , , , , , , , , , , , , , or ; R 42 , R 43 Each independently , , , , , , , , , , or ; R 51 For -F, , or .

5. The negative electrode sheet according to claim 4, characterized in that: The fluorine-containing compound includes , , , and One or more of .

6. The negative electrode sheet according to any one of claims 1 to 5, characterized in that: The negative electrode sheet comprises one or more of the following features: (1) The mass percentage of the fluorine-containing compound in the first negative electrode active material layer is 0.1% to 3.5%; (2) the first negative electrode active material layer includes a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a mass ratio of (94-96): (1-3): (1-3): (0.1-3.5); (3) The thickness of the first negative electrode active material layer is 95 μm to 115 μm; (4) The first negative electrode active material includes graphite.

7. The negative electrode sheet according to any one of claims 1 to 5, characterized in that: The negative electrode sheet further includes a second material layer disposed on at least one surface of the first negative electrode active material layer, the second material layer including a lithium-containing compound, The lithium-containing compound includes one or more of lithium phosphorus oxygen nitrogen, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium silicon phosphorus sulfur chlorine.

8. The negative electrode sheet according to claim 7, characterized in that: The lithium-containing compound includes Li 11-a Ge 2-a P 1+ a S 12 , Li 6-b PS 5-b Cl 1+b , Li 9.54±m1 Si 1.74±m2 P 1.44±m3 S 11.7±m4 Cl 0.3±m5 and Li n1 PO n2 N n3 One or more of; Among them, 0.5≤a≤1.5, 0≤b≤0.6, 0≤m1≤2, 0≤m2≤0.3, 0≤m3≤0.4, 0≤m4≤0.2, 0≤m5≤0.2, 0 <n1≤1,0<n2≤1,0<n3≤1。 9. The negative electrode sheet according to claim 8, characterized in that: The lithium-containing compound includes Li 10 GeP2S 12 、Li6PS5Cl、Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 and LiPON or more.

10. The negative electrode sheet according to claim 8 or 9, characterized in that: The negative electrode sheet comprises one or more of the following features: (1) The second material layer includes a second binder and a lithium-containing compound in a mass ratio of (45-30):(55-70); (2) The thickness of the second negative electrode active material layer is 1 μm to 5 μm.

11. A method for preparing a negative electrode sheet according to any one of claims 1 to 10, characterized in that: The following steps are involved: Mixing a first negative electrode active material, a first conductive agent, a first binder and a fluorine-containing compound in a first solvent to prepare a first active slurry; Applying the first active slurry on the surface of the negative electrode current collector and drying it to prepare the first negative electrode active material layer; The fluorine-containing compound includes one or more of fluorine-containing lithium borate salt, fluorinated benzene, fluorine-containing siloxane, fluorine-containing phosphate ester and fluorine-containing carbonate ester.

12. The method for preparing a negative electrode sheet according to claim 11, characterized in that: The following steps are also included: Mixing a second binder and a lithium-containing compound to prepare a mixture; Applying the mixed material on the surface of the first negative electrode active material layer to prepare a second material layer; The lithium-containing compound includes one or more of lithium phosphorus oxygen nitrogen, lithium germanium phosphorus sulfur, lithium phosphorus sulfur chlorine and lithium silicon phosphorus sulfur chlorine.

13. A secondary battery, characterized in that: A negative electrode sheet comprising the negative electrode sheet according to any one of claims 1 to 11.