Preparation method of lithium element high-load negative plate
By using three-dimensional porous copper foil and optimized formula in the lithium battery negative electrode sheet, a three-dimensional conductive network is constructed, which solves the problem of increased resistance caused by the reduction of conductive agent, achieves high energy density and improved lithium element loading capacity, and meets the needs of high energy and Fast charging needs.
Patent Information
- Application Number
- CN202411147591.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-01
AI Technical Summary
When the conductive agent is reduced in the existing lithium battery negative electrode sheet, the resistance increases, resulting in a decrease in capacity, making it difficult to achieve the goals of high energy and fast charging, and at the same time affecting battery safety.
A three-dimensional porous copper foil is used as the negative electrode current collector. A three-dimensional conductive network is constructed by punching holes in the original copper foil to form burrs, and a coating containing active substances, binders and thickeners is coated on it to reduce the conductive agent. content to increase the lithium element loading capacity.
It effectively improves the capacity/energy density and lithium element loading capacity of the negative electrode, while reducing the mass of the negative electrode piece, increasing the energy density, and achieving a higher lithium element loading design without affecting the conductivity.
Smart Images

Figure CN118738290A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to a method for preparing a lithium element high-load negative electrode sheet. Background Art
[0002] As a green energy storage technology, lithium battery technology plays a vital role in achieving the goals of carbon peak and carbon neutrality. At present, social development requires lithium batteries to have higher energy, faster charging speed and better safety performance. Therefore, it is necessary to improve various key indicators of batteries on the basis of traditional lithium batteries. The core is to effectively improve the transmission and load capacity of lithium elements in the battery pole while maintaining the safety of the battery, so as to achieve the goal of high energy or faster charging rate of the battery.
[0003] The basic requirement for high-energy batteries is to effectively increase the lithium element load of the positive and negative electrodes of the battery under the same battery size, thereby achieving the goal of high-energy batteries.
[0004] A Chinese patent with application number CN200710115517.5 discloses a high-capacity lithium iron phosphate power battery and its manufacturing process. The positive electrode material of the high-capacity lithium iron phosphate power battery is lithium iron phosphate, the positive electrode current collector is aluminum foil, the conductive agent is superconducting carbon black, conductive graphite, or no conductive agent is used, the positive electrode material binder is polyvinylidene fluoride, and the negative electrode material is natural or artificial graphite; the negative electrode current collector is copper foil, the conductive agent is superconducting carbon black, conductive graphite, and the negative electrode material binder is polyvinylidene fluoride or carboxymethyl cellulose sodium, styrene butadiene rubber.
[0005] It provides a solution to increase the battery capacity by not using conductive agents, but in fact, directly reducing the conductive agent and increasing the amount of other materials will not only fail to increase the capacity, but will reduce the capacity due to resistance. Therefore, it needs to be improved. Summary of the invention
[0006] In order to solve the defects of the prior art, the present invention discloses a method for preparing a negative electrode sheet with a high load of lithium, wherein the negative electrode sheet comprises a negative electrode current collector and negative electrode coatings on both sides of the current collector, wherein the current collector is a three-dimensional porous copper foil, and burrs are formed by punching holes on the original copper foil to form a three-dimensional structure, and a three-dimensional conductive network is constructed by the three-dimensional porous copper foil; The negative electrode coating comprises an active material, a binder, a thickener and a conductive agent; The conductive agent is one or more of conductive carbon black, carbon nanotubes, and graphene, and the added amount of the conductive agent accounts for 0% to 2%.
[0007] Preferably, the thickness of the three-dimensional porous copper foil is 3-40 μm.
[0008] Preferably, the surface density of the three-dimensional porous copper foil is not less than 95% of the surface density of the original copper foil.
[0009] Preferably, the components of the active material include artificial graphite, natural graphite, and silicon oxide, and the amount of the active material added accounts for 95% to 99%. Preferably, the binder component includes styrene-butadiene rubber latex (SBR), and the added amount of the binder accounts for 0.5% to 2.5%.
[0010] Preferably, the thickener component includes sodium carboxymethyl cellulose (CMC), and the added amount of the thickener accounts for 0.5% to 2.5%.
[0011] Preferably, the addition ratio of the binder to the thickener is 1:1.
[0012] Preferably, the negative electrode coating is coated on the three-dimensional porous copper foil using a conventional coating process, and the baking temperature during coating is controlled between 70 and 105°C.
[0013] Compared with the prior art, the present invention has the following beneficial effects: the present invention improves the structure of the negative electrode current collector, optimizes the traditional negative electrode formula, and indirectly increases the percentage content of the negative electrode active material by reducing the content of the conductive agent to the limit, or even not using the conductive agent, thereby increasing the capacity / energy density of the negative electrode; At the same time, by constructing a three-dimensional conductive network with three-dimensional porous copper foil, the possibility of reduced conductivity caused by the reduction of conductive agent is compensated, so as to better achieve the goal of high load design of negative electrode lithium element, thereby preparing high-energy batteries; Three-dimensional porous copper foil can reduce the mass of the negative electrode sheet to a certain extent and further improve the energy density of the negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic diagram of the three-dimensional porous copper foil structure of the present invention. DETAILED DESCRIPTION
[0015] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] The present invention provides a technical solution: a method for preparing a lithium high-load negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode current collector and negative electrode coatings on both sides of the current collector, wherein the current collector is a three-dimensional porous copper foil.
[0017] The negative electrode coating comprises an active material, a binder, a thickener and a conductive agent.
[0018] The conductive agent is one or more of conductive carbon black, carbon nanotubes, and graphene, and the added amount of the conductive agent is 0% to 2%, preferably 0 to 0.5%.
[0019] The components of the active material include artificial graphite, natural graphite and silicon oxide, and the added amount of the active material accounts for 95% to 99%, preferably 98% to 99%.
[0020] By reducing the content of conductive agent in the negative electrode formula, or even not using conductive agent, the content of active material can be indirectly increased, thereby increasing the capacity / energy density of the negative electrode.
[0021] The components of the binder include styrene-butadiene rubber latex (SBR), and the added amount of the binder accounts for 0.5% to 2.5%.
[0022] The components of the thickener include sodium carboxymethyl cellulose (CMC), and the added amount of the thickener accounts for 0.5% to 2.5%.
[0023] The addition ratio of binder to thickener is 1:1.
[0024] The three-dimensional porous copper foil is formed by punching holes on the original copper foil to form burrs, thereby forming a three-dimensional structure, and constructing a three-dimensional conductive network through the three-dimensional porous copper foil.
[0025] The thickness of the original copper foil is 6 μm, and the maximum thickness of the three-dimensional porous copper foil is about 25 μm.
[0026] The advantages of three-dimensional porous copper foil are uniform pore size and pore distribution, and slight punching burrs make it easier to construct three-dimensional foil and improve current distribution in the negative electrode sheet.
[0027] The surface density of the three-dimensional porous copper foil is 99.1% of the surface density of the original copper foil. This data should not be less than 95% to avoid affecting the tensile strength of the porous copper foil.
[0028] A three-dimensional conductive network is constructed using three-dimensional porous copper foil, thereby compensating for the possible decrease in conductivity caused by the reduction of conductive agent, avoiding the impact on the conductivity of the negative electrode due to the reduction in the content of conductive agent, and thus achieving the goal of having a higher lithium element loading capacity for the negative electrode with the same surface density.
[0029] After the negative electrode coating is made into a slurry, the negative electrode coating is coated on the three-dimensional porous copper foil using a traditional coating process. The baking temperature during coating is controlled between 70 and 105°C. Controlling this temperature range can effectively avoid cracking of the electrode.
[0030] Embodiment 1: The preferred formula range of the negative electrode used in this embodiment is as follows: the active material content is 98.5%, the binder content is 1.2%, the thickener content is 1.2%, and the conductive agent content is 0.3%.
[0031] Comparative Example 1: The preferred formula range of the negative electrode used in this comparative example is as follows: the active material content is 97.2%, the binder content is 1.2%, the thickener content is 1.2%, and the conductive agent content is 1.6%.
[0032] By comparing the resistivity and charge capacity of the negative electrode of Example 1 with that of the negative electrode of Comparative Example 1, the following conclusions are obtained: Sheet resistance (mΩ / cm2) Capacity of negative electrode of buckled battery / mAh Optimized negative electrode 45.2 3.478 Reference group negative electrode 44.9 3.309 Comparing Example 1 with Comparative Example 1, the surface resistance of the negative electrode in Example 1 increased by 0.67%, and the lithium element loading capacity increased by 5.11%. This shows that the patent solution can effectively improve the lithium element loading capacity of the negative electrode without affecting the conductivity of the negative electrode.
[0033] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-restrictive, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all changes within the meaning and range of equivalents of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0034] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a lithium high-load negative electrode sheet, Features: The negative electrode sheet includes a negative electrode current collector and negative electrode coatings on both sides of the current collector. The current collector is a three-dimensional porous copper foil. Burrs are formed by punching holes on the original copper foil to form a three-dimensional structure. A three-dimensional conductive network is constructed by the three-dimensional porous copper foil. The negative electrode coating comprises an active material, a binder, a thickener and a conductive agent; The conductive agent is one or more of conductive carbon black, carbon nanotubes, and graphene, and the added amount of the conductive agent accounts for 0% to 2%.
2. The method for preparing the lithium high-load negative electrode sheet according to claim 1, Features: The thickness of the three-dimensional porous copper foil is 3 to 40 μm.
3. The method for preparing the lithium high-load negative electrode sheet according to claim 2, Features: The surface density of the three-dimensional porous copper foil is not less than 95% of the surface density of the original copper foil.
4. The method for preparing the lithium high-load negative electrode sheet according to claim 1, Features: The components of active substances include artificial graphite, natural graphite, and silicon oxide, and the added amount of active substances accounts for 95% to 99%.
5. The method for preparing the lithium high-load negative electrode sheet according to claim 4, Features: The components of the binder include styrene-butadiene rubber latex (SBR), and the added amount of the binder accounts for 0.5% to 2.5%.
6. The method for preparing the lithium high-load negative electrode sheet according to claim 5, Features: The components of the thickener include sodium carboxymethyl cellulose (CMC), and the added amount of the thickener accounts for 0.5% to 2.5%.
7. The method for preparing the lithium high-load negative electrode sheet according to claim 6, Features: The addition ratio of binder to thickener is 1:
1.
8. The method for preparing the lithium high-load negative electrode sheet according to claim 7, Features: The negative electrode coating is coated on the three-dimensional porous copper foil using a traditional coating process, and the baking temperature during coating is controlled between 70 and 105°C.
Citation Information
Patent Citations
High capacity lithium iron phosphate power cell and production technique thereof
CN101183729A
Cited By
Low-temperature sodium-ion battery pole piece, battery cell and preparation method of low-temperature sodium-ion battery pole piece
CN119153707A