Pre-lithiation method of silicon negative electrode and assembling method of lithium ion battery
By directly contacting the metallic lithium sheet and the silicon negative electrode sheet in the electrolyte, controlling the contact time to achieve pre-lithiation, the problem of active Li+ loss of the negative electrode material of the lithium-ion battery is solved, the cycle performance and energy density of the battery are improved, and the process is simplified processes and enhanced security.
Patent Information
- Application Number
- CN202410819531.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
AI Technical Summary
The negative electrode material of existing lithium-ion batteries causes the loss of active Li+ due to the formation and volume change of the SEI film during the charge and discharge cycle, which affects the cycle life and energy density of the battery. Moreover, the existing prelithiation method has safety hazards and complicated operations. and the problem of impurity introduction.
By directly contacting the metallic lithium sheet and the silicon anode sheet under the electrolyte, controlling the contact time to achieve pre-lithiation, avoiding the introduction of impurities, preserving the original morphology of the silicon anode active particles, and simplifying the process flow.
It significantly improves the first Coulomb efficiency and cycle performance of lithium-ion batteries, extends battery life, reduces battery internal resistance, increases energy density, while simplifying the process flow and enhancing safety.
Smart Images

Figure CN118738296A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a pre-lithiation method for a silicon negative electrode and an assembly method for a lithium-ion battery. Background Art
[0002] In recent years, electric vehicles have become more and more popular. However, as the core component of electric vehicles, lithium-ion batteries have severely restricted the development of electric vehicles due to their low energy density. There are many ways to improve the energy density of lithium-ion batteries, and the most direct way is to improve the negative electrode active material. For example, increasing the specific surface area of the active material to increase the reaction sites, doping metal or non-metallic elements to improve the transmission of lithium ions, and coating a conductive layer on the surface of the active material particles to promote electron transmission. However, the energy density of lithium-ion batteries prepared by these methods usually decreases during the charge and discharge cycles due to complex side reactions, which is the so-called "aging mechanism."
[0003] Generally speaking, this aging mechanism is due to the active Li + The reduction of the so-called active Li + That is, Li can be reversibly transferred between the positive and negative electrodes. + During the first cycle of lithium-ion batteries, a SEI film will form on the negative electrode surface, consuming the limited active Li inside the battery. + For example, hard carbon, soft carbon, and graphite anodes with high specific surface areas will result in thicker passivation films, resulting in more active Li + For the silicon negative electrode, not only will the SEI layer be formed on the surface of the silicon particles, but also the drastic change in volume during the cycle will cause the SEI film on the surface of the silicon particles to rupture and regenerate repeatedly, resulting in the loss of active Li inside the lithium-ion battery. + The continuous decrease of will seriously affect the cycle life of lithium-ion batteries.
[0004] In lithium-ion batteries, the active Li + They are usually stored in the lithium-rich positive electrode, while the active Li + The retention rate not only determines the utilization rate of the lithium-rich positive electrode, but also determines the total weight of the battery. This is because in order to make up for the active Li lost in the negative electrode, + , and the proportion of lithium-rich positive electrode in the whole battery has to be increased, resulting in an increase in battery weight and a further decrease in energy density. Therefore, researchers proposed the negative electrode pre-lithiation technology, which can be understood as lithium ion doping of negative electrode active particles. By pre-storing a certain amount of active Li in the negative electrode particles + , to compensate for the loss of active Li due to the formation of SEI film on the surface of negative electrode particles during the cycle. +The loss of Li in the battery increases during the subsequent charge and discharge cycles. + The number of cells increases the cycle life of lithium-ion batteries, improves energy density, and reduces battery weight.
[0005] After continuous development, the main pre-lithiation methods are: chemical method, electrochemical method, additive method and direct contact with lithium metal method. However, the chemical method first dissolves lithium ions in a solvent, and then transfers the lithium ions to the negative electrode active particles. The solvent used and the high reactivity of the reaction process will cause safety hazards. At the same time, the solvent residue on the surface of the negative electrode will also affect the lithium-ion battery itself. The assembly principle of the electrochemical method is similar to that of ordinary lithium-ion batteries, except that the positive electrode is replaced with lithium metal. Then, under the action of the external circuit, the lithium ions are transferred from the lithium metal through the diaphragm to the counter electrode to achieve pre-lithiation, but its operation is cumbersome and complicated. The additive method adds lithium active materials to the negative electrode, but due to the high reactivity of the lithium active materials, it is incompatible with the solvents used in the preparation of silicon negative electrodes.
[0006] Direct contact with lithium metal method, such as uniformly coating or spraying a layer of stable lithium metal powder (SLMP) on the surface of the negative electrode, and then breaking the Li2CO3 shell outside the SLMP under appropriate pressure, so that the internal lithium metal is in direct contact with the negative electrode active particles, thereby achieving pre-lithiation of the negative electrode. However, this method is not only cumbersome and complicated to operate, but it is also very difficult to evenly distribute SLMP on the surface of the negative electrode. At the same time, the action of external force may also damage the structure of the silicon negative electrode active particles. Summary of the invention
[0007] In view of this, the purpose of the present application is to provide a pre-lithiation method for silicon negative electrode, so that the method can achieve pre-lithiation of silicon negative electrode in a safer and simpler way, without introducing impurities, preserving the original morphology of active particles of silicon negative electrode, and successfully achieving the purpose of improving the first efficiency, rate performance and cycle performance of lithium-ion batteries.
[0008] In order to solve the above technical problem / achieve the above purpose or at least partially solve the above technical problem / achieve the above purpose, as a first aspect of the present application, a pre-lithiation method of a silicon negative electrode is provided, comprising:
[0009] Provide silicon negative electrode sheet;
[0010] Placing the silicon negative electrode plate on the first bottom plate, with the side of the silicon negative electrode plate containing the active material facing upward; then adding the electrolyte to the silicon negative electrode plate, and covering the silicon negative electrode plate with a lithium sheet;
[0011] Cover the lithium sheet with a second bottom plate, apply force to the first bottom plate and the second bottom plate to make the lithium sheet fully contact with the silicon negative electrode plate, and control the degree of pre-lithiation by controlling the time for which the lithium sheet and the silicon negative electrode plate are fully in contact. After the pre-lithiation is completed, separate the silicon negative electrode plate.
[0012] Optionally, the active material of the silicon negative electrode plate includes one or more of silicate mineral-derived silicon, nano silicon, micro silicon and spherical silicon. Further optionally, the active material also includes a conductive agent and a binder.
[0013] Optionally, the top surfaces of the first bottom plate and the second bottom plate are both provided with raised side guard plates, and the side guard plates extend along the circumference of the bottom plate and are connected end to end.
[0014] Optionally, the inner side of the side guard plate of the first base plate is adjacent to the outer side of the side guard plate of the second base plate.
[0015] Optionally, acetonitrile solvent is used to assist in separating the pre-lithiated silicon negative electrode sheet.
[0016] Optionally, the lithium sheet is in full contact with the silicon negative electrode sheet for 10-30 minutes.
[0017] As a second aspect of the present application, a method for assembling a lithium ion battery is provided, comprising:
[0018] The pre-lithiation silicon negative electrode plate is obtained according to the pre-lithiation method described in the present application, and then assembled into a lithium-ion battery with an electrolyte, a separator and a positive electrode plate according to the lithium-ion battery assembly process.
[0019] This application achieves pre-lithiation of the silicon negative electrode sheet by allowing the metal lithium sheet to directly contact the silicon negative electrode sheet under the infiltration of the electrolyte, and controls the degree of pre-lithiation by controlling the contact time. This application can achieve simple and convenient pre-lithiation of the silicon negative electrode sheet without introducing impurities, preserving the original morphology of the silicon negative electrode active particles, and reducing the internal resistance of the battery, significantly improving the first coulomb efficiency, and at the same time, the silicon negative electrode after pre-lithiation has better rate performance and cycle performance due to the relief of volume expansion during the cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Shown is a physical display diagram of the pre-lithiation process of the present application;
[0021] Figure 2The figure shows a schematic diagram of the process of the pre-lithiation process of the present application; ① substrate (such as a glass plate); ② second bottom plate (such as a buckled negative electrode shell, with the concave surface facing upward); ③ lithium sheet (silver-white, smooth, and without black spots); ④ electrolyte (the electrolyte can be an electrolyte for pre-assembled batteries); ⑤ silicon negative electrode sheet to be pre-lithiated; ⑥ first bottom plate (such as a buckled positive electrode shell, with the concave surface facing upward); ⑦ fixing clip;
[0022] Figure 3 The figure shows the comparison of the first cycle charge and discharge curves of the silicon negative electrode obtained without pre-lithiation and after pre-lithiation for 20 minutes;
[0023] Figure 4 The figure shows the comparison of the cycle curves of the silicon negative electrode sheet without pre-lithiation and the silicon negative electrode sheet obtained by pre-lithiation for 20 minutes.
[0024] Figure 5 Shown is a comparison of the rate performance of the silicon negative electrode sheet without pre-lithiation and after pre-lithiation for 20 minutes. DETAILED DESCRIPTION
[0025] The present application discloses a method for pre-lithiation of a silicon negative electrode and an assembly method for a lithium-ion battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in this application. The method described in this application has been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the preparation method described in this article without departing from the content, spirit and scope of this application to realize and apply the technology of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0026] It should be noted that, in this article, if relational terms such as "first" and "second", "step 1" and "step 2", and "(1)" and "(2)" appear, they are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements. At the same time, the embodiments in this application and the features in the embodiments may be combined with each other without conflict.
[0027] In view of the problems that the current pre-lithiation process is generally cumbersome, has potential safety hazards, and affects the silicon negative electrode, the present application starts from the perspective of simplicity and efficiency, and realizes the pre-lithiation treatment of the silicon negative electrode by allowing the metal lithium sheet to directly contact the silicon negative electrode sheet under the infiltration of the electrolyte. In the first aspect of the present application, a pre-lithiation method for a silicon negative electrode is provided, comprising:
[0028] Provide silicon negative electrode sheet;
[0029] Placing the silicon negative electrode plate on the first bottom plate, with the side of the silicon negative electrode plate containing the active material facing upward; then adding the electrolyte to the silicon negative electrode plate, and covering the silicon negative electrode plate with a lithium sheet;
[0030] Cover the lithium sheet with a second bottom plate, apply force to the first bottom plate and the second bottom plate to make the lithium sheet fully contact with the silicon negative electrode plate, and control the degree of pre-lithiation by controlling the time for which the lithium sheet and the silicon negative electrode plate are fully in contact. After the pre-lithiation is completed, separate the silicon negative electrode plate.
[0031] In certain embodiments of the present application, providing a silicon negative electrode sheet includes:
[0032] The silicon-based negative electrode material, the conductive agent and the binder are fully mixed, and a solvent is added to the mixture to obtain a silicon negative electrode slurry. The silicon negative electrode slurry is coated on a current collector, and after drying, a silicon negative electrode sheet is obtained.
[0033] Among them, the silicon-based negative electrode material, the conductive agent and the binder are used as active materials of the silicon negative electrode plate, and the weight ratio of the three can be selected as 6:2:2; the silicon-based negative electrode material includes one or more of silicate mineral-derived silicon, nano silicon, micro silicon and spherical silicon. The silicate mineral-derived silicon refers to the elemental silicon prepared by applying magnesium thermal reduction reaction to silicate minerals (such as sepiolite, kaolinite, sand, etc.). The conductive agent includes one or more of carbon black conductive agents, carbon nanotube conductive agents, conductive graphite conductive agents, graphene conductive agents and carbon fiber conductive agents. In some embodiments of the present application, it is conductive carbon black SP. The binder includes one or more of polyvinyl alcohol, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, sodium alginate and fluorinated rubber. In some embodiments of the present application, it is sodium alginate. The current collector can be selected from metal foils, such as aluminum foil, copper foil, etc.
[0034] In certain embodiments of the present application, the top surfaces of the first bottom plate and the second bottom plate are both provided with raised side guard plates, which extend along the circumference of the bottom plate and are connected end to end to prevent the electrolyte from leaking out when force is applied to the first bottom plate and the second bottom plate. In certain embodiments of the present application, the first bottom plate and the second bottom plate are both circular; for example, a standard button battery shell, which can be a CR2016, CR2025 or CR2032 positive and negative button battery shell; in other embodiments of the present application, the inner side of the side guard plate of the first bottom plate is adjacent to the outer side of the side guard plate of the second bottom plate; that is, the side guard plate of the first bottom plate extends along the circumference of the bottom plate of the first bottom plate and is connected end to end to form a slot for the second bottom plate to be embedded. Taking the standard button battery shell as an example, the positive and negative battery shells can be used respectively, and the concave surface is upward for assembly, and the lithium sheet and the silicon negative electrode sheet are sandwiched in the middle, see Figure 1 and Figure 2 .
[0035] In certain embodiments of the present application, in order to provide a better electrolyte environment for the lithium sheet and the silicon negative electrode sheet, before placing the silicon negative electrode sheet on the first bottom plate, the electrolyte is added to the first bottom plate, and then the silicon negative electrode sheet is placed in the electrolyte, and the electrolyte is continued to be dripped on the silicon negative electrode sheet.
[0036] In some embodiments of the present application, the electrolyte can be a conventional lithium-ion battery electrolyte, generally an electrolyte for pre-assembled batteries, usually LiPF6 electrolyte. In other embodiments of the present application, the electrolyte includes 1.0M LiPF6, EC / DEC (volume ratio 1:1) and 10% FEC.
[0037] In certain embodiments of the present application, after the pre-lithiation of the silicon negative electrode sheet is completed, the pre-lithiation silicon negative electrode sheet is separated by using acetonitrile solvent to assist. After the pre-lithiation is completed, the silicon negative electrode sheet and the lithium sheet are adhered together, and may be attached to the surface of the first bottom plate (such as a button-type positive battery shell) or the second bottom plate (such as a button-type negative battery shell). The acetonitrile solution is sucked with a dropper and dripped around the silicon negative electrode sheet. After the acetonitrile solution enters the gap between the silicon negative electrode sheet and the lithium sheet, the silicon negative electrode sheet is removed with a tool and placed in a pre-prepared acetonitrile solution. Ultrasonic cleaning is performed, and after the acetonitrile solvent is completely volatilized, the pre-lithiation silicon negative electrode sheet is obtained.
[0038] In certain embodiments of the present application, the lithium sheet is in full contact with the silicon negative electrode for 10-30 minutes. The degree of pre-lithiation is controlled according to the time for which the lithium sheet is in full contact with the silicon negative electrode. Within the pre-lithiation time of 10-30 minutes, the assembled battery has better cycle performance, with 20 minutes of pre-lithiation being the best.
[0039] In some embodiments of the present application, the first bottom plate and the second bottom plate can be applied with a fixing clamp, and the fixing clamp applies force to the bottom surface of the first bottom plate and the top surface of the second bottom plate respectively, so that the two bottom plates clamp the lithium sheet and the silicon negative electrode sheet; in other embodiments of the present application, in order to evenly apply force, two substrates, such as glass plates, can be used to clamp the first bottom plate and the second bottom plate in the middle, and the fixing clamp applies force to the two substrates to avoid uneven force on the two bottom plates. See the schematic diagram Figure 1 and Figure 2 .
[0040] In a second aspect of the present application, a method for assembling a lithium-ion battery is provided, comprising:
[0041] The pre-lithiation silicon negative electrode plate is obtained according to the pre-lithiation method described in the present application, and then assembled into a lithium-ion battery with an electrolyte, a separator and a positive electrode plate according to the lithium-ion battery assembly process.
[0042] In certain embodiments of the present application, the assembly method comprises:
[0043] Drip electrolyte on the negative electrode shell, then put in the pre-lithiation silicon negative electrode sheet with the active material facing up, then drip electrolyte on the surface of the silicon negative electrode sheet, then place the diaphragm, then drip electrolyte on the surface of the diaphragm, then place the lithium sheet, then drip electrolyte on the surface of the lithium sheet, then put in the gasket and spring in turn, and finally cover the positive electrode shell and complete the packaging on the packaging machine.
[0044] In each group of comparative experiments provided in this application, unless otherwise specified, other experimental conditions, materials, etc. are kept consistent except for the differences indicated in each group, so as to provide comparability. The experimental materials and reagents used in the examples can be obtained from commercial channels unless otherwise specified.
[0045] The following is a further description of a pre-lithiation method for a silicon negative electrode and an assembly method for a lithium-ion battery provided in the present application.
[0046] Embodiment 1:
[0047] 1. Preparation of silicon negative electrode
[0048] Silicate mineral-derived silicon, conductive carbon black SP and sodium alginate (SA) were fully mixed in a mortar at a weight ratio of 6:2:2, and then deionized water was used as a solvent and an appropriate amount was added dropwise to obtain a silicon negative electrode slurry;
[0049] The obtained silicon negative electrode slurry was coated on a copper foil with a 100 μm scraper and dried at 60° C. for 24 h to obtain a silicon negative electrode sheet.
[0050] 2. Pre-lithiation method of silicon negative electrode
[0051] The silicon negative electrode piece that needs to be pre-lithiated is dried and weighed (M1, for the subsequent calculation of the weight of lithium ions entering the electrode piece). At the same time, acetonitrile is prepared for cleaning the residue on the electrode piece after pre-lithiation, and a pre-lithiation mold is prepared (a standard button battery case, glass sheet and fixing clip of model CR2016, 2025 or 2032).
[0052] Use a rubber-tipped dropper to drop a drop of lithium-ion battery electrolyte in the center of the positive electrode shell (the electrolyte is the electrolyte for pre-assembled batteries, 1.0M LiPF6+EC / DEC (volume ratio 1:1)+10% FEC), put in the pole piece with the active material facing up, drop two drops of electrolyte on the pole piece, then select a lithium sheet with a smooth surface to completely cover the pole piece, and finally, assemble the negative electrode shell with the positive electrode shell in reverse so that the lithium sheet and the pole piece are in full contact. At the same time, use two glass sheets to sandwich the assembled pre-lithiation assembly in the middle (to avoid uneven force on the shell), and fix it with a fixing clip, see Figure 1 and Figure 2 , let it stand and wait for the pre-lithiation process to end, and control the degree of pre-lithiation by controlling the pre-lithiation time.
[0053] After the pre-lithiation process is completed, loosen the fixing clamp and separate the negative electrode shell from the positive electrode shell. At this time, the pole piece and the lithium sheet are adhered together, and may be attached to the surface of the positive electrode shell or the negative electrode shell. Use a rubber-tipped dropper to absorb the acetonitrile solution and drip it around the pole piece. After the acetonitrile solution enters the gap between the pole piece and the lithium sheet, use tweezers to remove the pole piece and put it into the pre-prepared acetonitrile solution. After ultrasonic cleaning for 3 minutes, take it out and wait for the acetonitrile solvent to completely evaporate to obtain the pre-lithiation pole piece.
[0054] The pre-lithiation electrode is weighed (M2), and the weight M of the lithium ions entering the electrode can be roughly obtained by calculation, M=M2-M1.
[0055] All the above operations are carried out in a glove box, and the environmental conditions of the glove box are water <0.01ppm, oxygen <0.01ppm. The pre-lithiation lithium sheet can be polished with 3000-grit sandpaper to make the lithium sheet recyclable.
[0056] Embodiment 2:
[0057] 20 μL of electrolyte was dripped on the negative electrode shell, and then the negative electrode sheet (active material side facing up) was placed, and then 20 μL of electrolyte (same as the electrolyte in Example 1) was dripped on the surface of the negative electrode sheet, and then the diaphragm was placed, and then 20 μL of electrolyte was dripped on the surface of the diaphragm, and then the lithium sheet was placed, and then 20 μL of electrolyte was dripped on the surface of the lithium sheet, and then the gasket and shrapnel were placed in sequence, and finally the positive electrode shell was covered, and the packaging was completed on the packaging machine. The battery after packaging needs to be left to stand for 24 hours before testing.
[0058] 1. Referring to the method of Example 1, the pre-lithiation time was controlled at 0, 10, 20, 40, and 60 min, respectively, to obtain silicon negative electrode sheets with different pre-lithiation degrees, which were assembled into button cells and the cycle performance was tested using the same method. The results are shown in Table 1 below;
[0059] Table 1
[0060] Pre-lithiation time Discharge capacity after 100 cycles at 200mA / g 0min 956.9mAh / g 10min 1435.0mAh / g 20min 1728.7mAh / g 40min 1189.0mAh / g 60min 945.8mAh / g
[0061] It can be seen from Table 1 that the cycle performance of silicon negative electrode batteries that have not undergone pre-lithiation is poor; as the pre-lithiation time continues to increase, the cycle performance of the battery shows a trend of first increasing and then decreasing, and the best cycle performance is achieved when the pre-lithiation time is 20 minutes. According to the above experimental results, it can be considered that the battery can obtain good cycle performance within a pre-lithiation time of 10-30 minutes.
[0062] 2. Referring to the method of Example 1, the pre-lithiation time was determined to be 20 min, the silicon-based material was adjusted to commercial nano-silicon, commercial micro-silicon and commercial spherical silicon materials, and pre-lithiation silicon negative electrode sheets were prepared. The button batteries were assembled and the cycle performance was tested using the same method. The results are shown in Table 2 below;
[0063] Table 2
[0064] Types of Silicon Discharge capacity after 100 cycles at 200mA / g Silicon derived from silicate minerals 1728.7mAh / g Nano Silicon 1226.2mAh / g Micron Silicon 1146.1mAh / g Spherical Silicon 1393.4mAh / g
[0065] It can be seen from Table 2 that the pre-lithiation method of the present application is particularly suitable for silicate mineral-derived silicon materials. Compared with batteries assembled using nano-silicon, micron-silicon, and spherical silicon materials, the batteries assembled therefrom show more excellent effects in cycle performance. The discharge specific capacity after 100 cycles at 200mA / g is as high as 1728.7mAh / g, while the batteries of the other three materials do not exceed 1400mAh / g.
[0066] Embodiment 3:
[0067] Referring to the method of Example 1, the pre-lithiation time was determined to be 20 min, a pre-lithiation silicon negative electrode sheet was prepared, and a button cell was assembled to test the first efficiency, cycle performance and rate performance, with a non-pre-lithiation silicon negative electrode sheet as a control;
[0068] 1. Comparison of the first cycle charge and discharge curves is shown in Figure 3 ; At a current density of 200mA / g, the first cycle charge and discharge specific capacities without pre-lithiation were 2171.3723 and 3198.1092mAh / g, respectively, with a first efficiency of 67.9%. After 20 minutes of pre-lithiation, the first cycle charge and discharge specific capacities were 2332.4255 and 2632.8339mAh / g, respectively, with a first efficiency of 88.6%. It can be seen that as a result of pre-lithiation, the first cycle discharge capacity dropped from 3198.1092mAh / g to 2632.8339mAh / g. This is because part of the elemental silicon has formed a lithium-silicon alloy during the pre-lithiation process. The decrease in the first cycle discharge specific capacity is an inevitable result of pre-lithiation and a sign of successful pre-lithiation, which corresponds to an increase in the first efficiency.
[0069] 2. Cycle curve comparison chart Figure 4 ; After 100 cycles at a current density of 200 mA / g, the discharge specific capacities without pre-lithiation and pre-lithiation for 20 minutes are 956.9 and 1728.7 mAh / g, respectively. It can be seen that the pre-lithiation measures of the present application significantly improve the cycle performance of the silicon negative electrode, which can achieve the expected purpose, and the method is faster, safer and more convenient.
[0070] 3. Rate performance comparison chart Figure 5; At current densities of 200, 500, 1000, 2000, 4000, and 8000 mA / g, the discharge specific capacities without pre-lithiation are 2361.7123, 1817.0192, 1622.897, 1378.5887, 915.8719, and 455.7137 mAh / g, respectively; the discharge specific capacities after 20 minutes of pre-lithiation are 2639.5495, 1976.3828, 1793.2156, 1519.8857, 1016.2013, and 500.26 mAh / g, respectively. It can be seen that the rate performance of the silicon negative electrode is improved by the pre-lithiation method of the present application.
[0071] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for pre-lithiation of a silicon negative electrode, characterized in that: include: Provide silicon negative electrode sheet; Placing the silicon negative electrode plate on the first bottom plate, with the side of the silicon negative electrode plate containing the active material facing upwards; Then, the electrolyte is added to the silicon negative electrode plate, and the silicon negative electrode plate is covered with a lithium sheet; Cover the lithium sheet with a second bottom plate, apply force to the first bottom plate and the second bottom plate to make the lithium sheet fully contact with the silicon negative electrode plate, and control the degree of pre-lithiation by controlling the time for which the lithium sheet and the silicon negative electrode plate are fully in contact. After the pre-lithiation is completed, separate the silicon negative electrode plate.
2. The pre-lithiation method according to claim 1, characterized in that: The active material of the silicon negative electrode plate includes one or more of silicate mineral-derived silicon, nano silicon, micro silicon and spherical silicon.
3. The pre-lithiation method according to claim 2, characterized in that: The active material further includes a conductive agent and a binder.
4. The pre-lithiation method according to claim 1, characterized in that: The top surfaces of the first bottom plate and the second bottom plate are both provided with raised side guard plates, and the side guard plates extend along the circumference of the bottom plate and are connected end to end.
5. The pre-lithiation method according to claim 1, characterized in that: The inner side of the side guard plate of the first bottom plate is adjacent to the outer side of the side guard plate of the second bottom plate.
6. The pre-lithiation method according to claim 1, characterized in that: Acetonitrile solvent is used to assist in separating the pre-lithiation silicon negative electrode plate.
7. The pre-lithiation method according to claim 1, characterized in that: The time for the lithium sheet to be in full contact with the silicon negative electrode sheet is 10-30 minutes.
8. A method for assembling a lithium-ion battery, characterized in that: include: The pre-lithiation silicon negative electrode sheet is obtained by the pre-lithiation method according to any one of claims 1 to 7, and then assembled into a lithium-ion battery with an electrolyte, a separator and a positive electrode sheet according to a lithium-ion battery assembly process.