Positive electrode composite material for sodium ion battery and preparation method of positive electrode composite material
By boronizing, hydroxylating and nitriding the cathode material of the sodium ion battery to form modified transition metal oxides, cross-linking agents and conductive agents, the problems of irreversible changes in the structure of existing materials and low air stability are solved, achieving It achieves high conductivity and stability, improving the cycle performance and energy density of the battery.
Patent Information
- Application Number
- CN202411107882.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The structure of existing sodium-ion battery cathode materials changes irreversibly during the discharge process, the reversible discharge capacity is reduced, and the air stability is low, resulting in the need to improve cycle performance and air stability.
Modified transition metal oxides, modified cross-linking agents and modified conductive agents are used, and through boronization, hydroxylation and nitridation treatments, a sodium-ion battery cathode composite material with high conductivity, high stability and high capacity is formed.
It improves the capacitance, cycle performance and air stability of sodium-ion battery cathode materials, enhances the efficiency of electrochemical reactions and the energy density and power density of equipment.
Smart Images

Figure CN118738355A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cathode material processing, and in particular to an cathode composite material for a sodium ion battery and a preparation method thereof. Background Art
[0002] Sodium-ion batteries are abundant in resources, inexpensive, and have a similar working principle to lithium-ion batteries, making them a current research hotspot. Since cathode materials play a decisive role in the capacity and power of batteries, the research on cathode materials has become the key to the development of sodium-ion batteries. At present, the cathode materials of sodium-ion batteries include transition metal oxides, polyanion compounds, and Prussian blue compounds. Among them, transition metal oxides have attracted widespread attention due to their rich central elements, high electrochemical activity, and environmental friendliness. However, transition metal oxides have complex phase transitions, surface sensitivity, and slow kinetics, which limit their large-scale development.
[0003] Prior art CN107978743A discloses a sodium ion battery positive electrode material and a preparation method thereof, wherein a sodium source, an iron source, a manganese source, a vanadium source and a phosphorus source are dissolved in deionized water at a specific ratio, and then a mixed solution of tetraethylene glycol and ethylene glycol is added to form a hydrothermal reaction system containing tetraethylene glycol and ethylene glycol, and the volume ratio of tetraethylene glycol and ethylene glycol, the concentration of vanadium ions in the solution system, the temperature and time of the hydrothermal reaction, and the temperature and time of the calcination are controlled to obtain a sodium ion battery positive electrode material, and then the sodium ion battery material is further prepared. The sodium ion battery positive electrode material obtained by this method has a high conductivity during the discharge process due to Na + Excessive insertion leads to Fe 4+ Migration to the sodium layer causes irreversible changes in the structure, resulting in a decrease in the reversible discharge capacity; Mn 3+ The asymmetric electron cloud induces Jahn-Teller strain in the structure. + The continuous strain and distortion during the embedding / ex-embedding process cause the structure to gradually collapse, resulting in a gradual decrease in capacity, and cannot overcome the disadvantage of the low stability of the sodium-ion battery positive electrode material in the air. In summary, the cycle performance and air stability of the sodium-ion battery positive electrode material prepared by the existing technology need to be further improved.
[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0005] The object of the present invention is to provide a positive electrode composite material for a sodium ion battery and a preparation method thereof, so as to solve the technical problem that the capacity and air stability of the positive electrode material of a sodium ion battery in the prior art need to be further improved.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A positive electrode composite material for a sodium ion battery, comprising, by weight, 60-80 parts of a modified transition metal oxide, 5-15 parts of a modified crosslinking agent, 10-20 parts of a modified conductive agent, 85-95 parts of a solvent, and 0.5-1 part of a filler;
[0008] The filler is one or more of single-walled carbon nanotubes, silicon dioxide, graphite and carbon fiber; and the solvent is N-methylpyrrolidone.
[0009] Further, the preparation method of the modified transition metal oxide is as follows: after the boronized transition metal oxide is transferred to a tubular furnace, nitrogen is introduced for protection, the tubular heating furnace is heated to 300±5°C at a rate of 10°C / min, and then heated at a rate of 30-50cm 3 A mixed gas consisting of 5% methanol gas and 95% nitrogen gas is introduced into the tubular heating furnace at a flow rate of 1 / min, the pressure is set to 10-20 Torr, and the temperature is kept for 1-3 hours. After the heating is terminated, the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain a modified transition metal oxide.
[0010] Reaction principle for preparing modified transition metal oxides: At high temperature, methanol gas produces methyl radicals (CH3·) through thermal decomposition. These methyl radicals react with oxygen to form hydroxymethyl radicals (CH2OH·). The hydroxymethyl radicals further react with the oxide groups on the surface of the transition metal oxide to form hydroxyl groups, thereby obtaining modified transition metal oxides.
[0011] Furthermore, the preparation method of the borated transition metal oxide is as follows: 15-20 parts of transition metal oxide and 1-2 parts of lithium borohydride are weighed by weight, mixed evenly and placed in a tubular furnace, nitrogen is introduced for protection, the tubular heating furnace is increased to 800±5°C at a rate of 10°C / min, and the reaction is kept warm for 1-3h to obtain the borated transition metal oxide.
[0012] Reaction principle for preparing borated transition metal oxides: Under high temperature conditions, lithium borohydride begins to decompose and release hydrogen: LiBH4→LiH+B+H2. The released hydrogen and boron react with the oxide on the surface of the transition metal oxide to undergo a reduction reaction. The oxidation state of the transition metal oxide is partially reduced to form a borated transition metal oxide.
[0013] Furthermore, the transition metal oxide is NaNi 0.7 Mn 0.15 Co 0.15 O2、NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15One or more of O2.
[0014] Furthermore, the preparation method of the modified crosslinking agent comprises the following steps:
[0015] A1. Weigh 16-24 parts of 4,4'-oxydiphthalic anhydride, 12-18 parts of 4,4'-diaminodiphenyl sulfone, 100-200 parts of N-methylpyrrolidone and 2-3 parts of triethylamine by weight, dissolve 4,4'-diaminodiphenyl sulfone in N-methylpyrrolidone, add 4,4'-oxydiphthalic anhydride in batches while stirring at room temperature for 2-4h, and add each time in an amount of half of the remaining 4,4'-oxydiphthalic anhydride. After the reaction is completed, an anhydride-terminated polyamic acid glue solution is obtained;
[0016] The reaction equation for synthesizing anhydride-terminated polyamic acid is:
[0017]
[0018] Where:
[0019] The reaction principle of synthesizing anhydride-terminated polyamic acid is as follows: 4,4'-diaminodiphenyl sulfone with an amino group acts as a nucleophilic reagent to attack the carbonyl carbon atom in the 4,4'-oxydiphthalic anhydride molecule, wherein the nitrogen atom of the amino group carries a lone pair of electrons, which can form a new covalent bond with the carbonyl carbon atom, ultimately forming a polyamic acid connected with an amino acyl group, and then by controlling the amount of 4,4'-oxydiphthalic anhydride added, anhydride-terminated polyamic acid glue is finally obtained.
[0020] A2. Weigh 10-20 parts of anhydride-terminated polyamic acid glue, 1-2 parts of 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane, 40-50 parts of N,N-dimethylformamide and 0.5-0.8 parts of triethylamine by weight and add them into a reactor. Raise the temperature of the reactor to 40-60°C, keep the reaction warm for 2-4 hours, and post-treat to obtain a modified cross-linking agent.
[0021] The reaction equation for synthesizing the modified crosslinking agent is:
[0022]
[0023] The reaction principle of synthesizing modified cross-linking agents is as follows: under alkaline conditions, the lone pair of electrons of the oxygen atom in the hydroxyl group attacks the carbonyl carbon atom in the cyclic anhydride. The nucleophilic attack ability of the hydroxyl group enables it to form a new covalent bond with the carbonyl carbon atom of the carboxylic anhydride, and the formed carboxylic acid group will further undergo an esterification reaction with the hydroxyl group to make the cross-linking agent structure more complex, and finally a modified cross-linking agent connected by an ester bond is obtained.
[0024] Furthermore, in step A1, the stirring rate is 120-180 rpm; in step A2, the post-treatment includes: after the reactor is cooled to room temperature, the reaction solution is added to a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain a modified cross-linking agent.
[0025] Furthermore, the preparation method of the modified conductive agent comprises the following steps:
[0026] B1. Weigh 1-3 parts of natural flake graphite and 20-30 parts of N-methylpyrrolidone by weight and add them into a reactor. The temperature of the reactor is raised to 140-160° C., and the reaction is kept warm for 3-5 hours. Then, the reactor is placed in an ultrasonic disperser with a frequency of 20-40 kHz, and ultrasonicated at room temperature for 16-24 hours to obtain a dispersed solution.
[0027] B2. Transfer the dispersed solution to a centrifuge tube, set the speed to 1200-1600 rpm, centrifuge at room temperature for 0.5-1 h, take the upper layer of the solution and filter it, and vacuum dry the obtained filter cake at 60 ° C for 24 h to obtain graphene;
[0028] B3. Place graphene in a pressure chamber of 10 -2 -10 -3 In a 1000-20000 ℃ ammonia nitriding furnace, high-purity ammonia is introduced, the gas pressure is maintained at 0.1-1 Torr, the temperature is raised to 500-800 ℃, the temperature is kept for 2-3 hours, and the sample chamber is gradually cooled to room temperature to obtain nitrided graphene;
[0029] The reaction principle for preparing nitrided graphene is as follows: under the action of ammonia, nitrogen decomposes at high temperature to produce free nitrogen atoms, which can enter the lattice structure of graphene, replace or insert into the position of carbon atoms, and form nitrided graphene.
[0030] B4. After the nitrided graphene is transferred to the tubular furnace, nitrogen is introduced for protection. The tubular heating furnace is heated to 300±5℃ at a rate of 10℃ / min and then heated to 50cm 3 Oxygen was introduced into the tubular heating furnace at a flow rate of 2°C / min, and the temperature was kept at this temperature for 1-2 hours. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min, and then heated at a rate of 25 cm / min. 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 100 Å / min to obtain a modified conductive agent.
[0031] The reaction principle for preparing the modified conductive agent is: thermal oxidation is performed using the oxidant oxygen to generate an oxide layer, and the oxide layer is further exposed to a water vapor environment for hydroxylation.
[0032] A method for preparing a positive electrode composite material for a sodium ion battery comprises the following steps: uniformly mixing 60-80 parts of a modified transition metal oxide, 5-15 parts of a modified crosslinking agent, 10-20 parts of a modified conductive agent, 85-95 parts of a solvent and 0.5-1 part of a filler to obtain a mixed slurry; uniformly coating the mixed slurry on a surface of an aluminum foil having a thickness of 25 microns to form a thin sheet; and placing the sheet in a vacuum drying oven at 120° C. for drying for 12 hours to obtain a composite positive electrode material.
[0033] The present invention has the following beneficial effects:
[0034] 1. In the process of preparing a positive electrode composite material for a sodium ion battery, the present invention firstly borates an existing transition metal oxide for a positive electrode material of a sodium ion battery and performs a surface hydroxylation treatment to obtain a modified transition metal oxide; uses 4,4'-oxydiphthalic anhydride and 4,4'-diaminodiphenyl sulfone to prepare an anhydride-terminated polyamide acid glue solution, and uses 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane to graft it to obtain a modified cross-linking agent; uses natural flake graphite to prepare graphene, and then performs surface nitridation and hydroxylation treatment on it to obtain a modified conductive agent; finally, the modified transition metal oxide, the modified cross-linking agent, the modified conductive agent, the filler and the solvent are mixed to obtain a positive electrode composite material for a sodium ion battery with high conductivity, high stability, high capacity and high cycle performance.
[0035] 2. In the process of preparing a modified transition metal oxide, the present invention first uses lithium borohydride as a boron source to perform surface boronization on the transition metal oxide. The surface boronized transition metal oxide has better conductivity and reduces the chemical reactivity on the surface of the transition metal oxide, further improving the stability of the transition metal oxide, adjusting the energy band structure and electronic state of the transition metal oxide, and helping to improve its capacitance in the electrode material. Further, the surface hydroxylation of the transition metal oxide enhances its binding force with the modified cross-linking agent, making its structure more compact and more resistant to oxidation. By modifying the transition metal oxide, the capacitance of the positive electrode material is increased and it is more resistant to air oxidation.
[0036] 3. In the process of preparing a modified cross-linking agent, the present invention selects 4,4'-diaminodiphenyl sulfone and 4,4'-oxydiphthalic anhydride having an ether bond structure. The presence of the ether bond can make the cross-linking agent better dispersed and dissolved in the solvent, thereby improving the fluidity and processability of the cross-linking agent. The adhesive with the ether bond structure can provide good stability. In addition, the ether bond can also enhance the resistance of the cross-linking agent to the electrolyte solution and improve the cycle performance; further, the polymer is modified by 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane, and the formed carboxylic acid group will further react with it, so that the modified cross-linking agent has a large number of alkoxy structures, so that it is more tightly combined with the inorganic material, and the stability of the slurry obtained by the inorganic material configuration is further improved. , by preparing a modified cross-linking agent, the stability and cycle performance of the positive electrode material are further improved; in the process of preparing a modified conductive agent, the present invention improves the capacitance performance, including charge storage capacity and cycle stability, by preparing graphene and then nitriding its surface. This modification can also effectively improve the charge and discharge rate of the capacitor, thereby improving the energy density and power density of the device; the introduction of nitrogen atoms can adjust the electronic structure and surface active sites of graphene, thereby enhancing its adsorption and electron transfer capabilities for electrochemical reactants, improving reaction efficiency and stability, and increasing the cycle life and energy density of the battery; after further hydroxylation of its surface, it can be more closely combined with the cross-linking component, further improving the capacitance and air stability of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 The present invention is a flow chart of a method for preparing a positive electrode composite material for a sodium ion battery. DETAILED DESCRIPTION
[0039] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] The transition metal oxide Na used in the present invention 0.67 Mn 0.65 Fe 0.2 Ni0.15 O2 refers to patent application CN2020107934258 "A high energy density sodium ion battery Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15 An efficient and stable preparation method for O2 positive electrode materials was prepared.
[0041] Example 1
[0042] This embodiment provides a method for preparing a positive electrode composite material for a sodium ion battery, comprising the following steps:
[0043] S1. Preparation of modified transition metal oxides
[0044] Weigh 105.3gNa 0.67 Mn 0.65 Fe 0.2 Ni 0.15 O2 and 10.3g lithium borohydride were mixed evenly and placed in a tubular furnace, nitrogen was introduced for protection, the tubular heating furnace was heated to 795°C at a rate of 10°C / min, and the temperature was kept for reaction for 1h to obtain 109.6g borated transition metal oxide;
[0045] After 100.0 g of boronized transition metal oxide was transferred to a tube furnace, nitrogen was introduced for protection, and the tube furnace was heated to 295°C at a rate of 10°C / min and then heated at 30 cm 3 A mixed gas consisting of 5% methanol gas and 95% nitrogen gas was introduced into the tubular heating furnace at a flow rate of 10 Torr / min, and the pressure was set to 10 Torr. The mixture was kept warm for 1 hour. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min to obtain 102.5 g of modified transition metal oxide.
[0046] S2. Preparation of modified crosslinking agent
[0047] Weigh 18.3g 4,4'-oxydiphthalic anhydride, 13.7g 4,4'-diaminodiphenyl sulfone, 109.7g N-methylpyrrolidone and 1.9g triethylamine, dissolve 4,4'-diaminodiphenyl sulfone in N-methylpyrrolidone, add 4,4'-oxydiphthalic anhydride in batches while stirring for 2h at room temperature, the stirring rate is 120rpm, and the amount added each time is half of the remaining 4,4'-oxydiphthalic anhydride. After the reaction is completed, 30.5g of anhydride-terminated polyamic acid glue is obtained;
[0048] Weigh 20.0g of anhydride-terminated polyamic acid glue, 1.5g of 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane, 43.2g of N,N-dimethylformamide and 0.6g of triethylamine into a reactor, raise the temperature of the reactor to 40°C, and keep the reaction for 2h. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 80°C, and distill under reduced pressure until no liquid is produced to obtain 21.3g of modified cross-linking agent.
[0049] S3. Preparation of modified conductive agent
[0050] 23.5 g of natural flake graphite and 223.5 g of N-methylpyrrolidone were weighed and added into a reactor. The temperature of the reactor was raised to 140° C. After the reaction was kept warm for 3 hours, the reactor was placed in an ultrasonic disperser with a frequency of 20 kHz and ultrasonicated at room temperature for 16 hours to obtain a dispersed solution.
[0051] The dispersed solution was transferred to a centrifuge tube, the speed was set to 1200 rpm, and the upper layer of the solution was filtered after centrifugation at room temperature for 0.5 h. The filter cake was vacuum dried at 60 ° C for 24 h to obtain 22.4 g of graphene;
[0052] 20.0g of graphene is placed in a pressure chamber of 10 -2 Torr ammonia nitriding furnace, introduce high-purity ammonia, maintain the gas pressure at 0.1 Torr, raise the temperature to 500°C, keep the temperature for 2 hours, gradually cool the sample chamber to room temperature, and obtain 20.5g of nitrided graphene;
[0053] After 20.0 g of nitrided graphene was transferred to a tubular furnace, nitrogen was introduced for protection, and the tubular furnace was heated to 295 °C at a rate of 10 °C / min and then heated at 50 cm / min. 3 Oxygen was introduced into the tubular heating furnace at a flow rate of 2°C / min, and the temperature was kept at this temperature for 1 hour. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min, and then heated at 25 cm / min. 3 Water vapor was introduced into the tubular heating furnace at a flow rate of / min to obtain 21.3 g of a modified conductive agent.
[0054] S4. Preparation of positive electrode for sodium ion battery
[0055] Weigh 60.0 g of modified transition metal oxide, 6.8 g of modified crosslinking agent, 12.4 g of modified conductive agent, 93.2 g of N-methylpyrrolidone and 0.7 g of carbon fiber and mix them evenly to obtain a mixed slurry;
[0056] The mixed slurry was evenly coated on the surface of an aluminum foil with a thickness of 25 μm to form a thin sheet, and placed in a vacuum drying oven at 120° C. for 12 hours to obtain a composite positive electrode material.
[0057] S5. Preparation of sodium ion batteries
[0058] The positive electrode sheet is obtained by rolling the composite positive electrode material, and the negative electrode sheet is obtained by vacuum stirring, coating, cold pressing and cutting hard carbon: conductive carbon black: carboxymethyl cellulose: styrene butadiene rubber = 90:3:2:2;
[0059] The positive electrode sheet, the negative electrode sheet, the electrolyte (1 mol / L NaPF6 dissolved in a mixed solvent of ethylene carbonate: diethyl carbonate with a volume ratio of 1:1) and the glass fiber separator are assembled into a button cell (button battery).
[0060] Example 2
[0061] This embodiment provides a method for preparing a positive electrode composite material for a sodium ion battery, comprising the following steps:
[0062] S1. Preparation of modified transition metal oxides
[0063] Weigh 120.5g Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15 O2 and 12.3g lithium borohydride were evenly mixed and placed in a tubular furnace, nitrogen was introduced for protection, the tubular heating furnace was heated to 805°C at a rate of 10°C / min, and the temperature was kept for reaction for 3h to obtain 124.9g borated transition metal oxide;
[0064] After 100.0 g of borided transition metal oxide was transferred to a tubular furnace, nitrogen was introduced for protection, and the tubular furnace was heated to 305 °C at a rate of 10 °C / min and then heated at 50 cm 3 A mixed gas consisting of 5% methanol gas and 95% nitrogen gas was introduced into the tubular heating furnace at a flow rate of 2°C / min, the pressure was set to 20 Torr, and the mixture was kept warm for 3 hours. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min to obtain 103.5 g of modified transition metal oxide.
[0065] S2. Preparation of modified crosslinking agent
[0066] Weigh 22.9g 4,4'-oxydiphthalic anhydride, 17.1g 4,4'-diaminodiphenyl sulfone, 171.4g N-methylpyrrolidone and 2.3g triethylamine, dissolve 4,4'-diaminodiphenyl sulfone in N-methylpyrrolidone, add 4,4'-oxydiphthalic anhydride in batches while stirring at room temperature for 4h, the stirring rate is 160rpm, and the amount added each time is half of the remaining 4,4'-oxydiphthalic anhydride. After the reaction is completed, 38.5g of anhydride-terminated polyamic acid glue is obtained;
[0067] Weigh 25.3g of anhydride-terminated polyamic acid glue and 2.65g of 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane, 53.2g of N,N-dimethylformamide and 0.7g of triethylamine into a reactor, raise the temperature of the reactor to 60°C, and keep the reaction for 4h. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 100°C, and distill under reduced pressure until no liquid is produced to obtain 26.8g of modified cross-linking agent.
[0068] S3. Preparation of modified conductive agent
[0069] 24.5 g of natural flake graphite and 236.4 g of N-methylpyrrolidone were weighed and added into a reactor. The temperature of the reactor was raised to 160° C. After the reaction was kept at this temperature for 1 h, the reactor was placed in an ultrasonic disperser with a frequency of 40 kHz, and ultrasonicated at room temperature for 24 h to obtain a dispersed solution.
[0070] The dispersed solution was transferred to a centrifuge tube, the speed was set to 1600 rpm, and the upper layer of the solution was filtered after centrifugation at room temperature for 1 hour. The filter cake was vacuum dried at 60°C for 24 hours to obtain 20.5 g of graphene.
[0071] 20.0g of graphene is placed in a pressure chamber of 10 -3 Torr ammonia nitriding furnace, introduce high-purity ammonia, maintain the gas pressure at 0.1 Torr, raise the temperature to 800°C, keep the temperature for 3 hours, gradually cool the sample chamber to room temperature, and obtain 20.6g of nitrided graphene;
[0072] After 20.0 g of nitrided graphene was transferred to a tubular furnace, nitrogen was introduced for protection, and the tubular furnace was heated to 305 °C at a rate of 10 °C / min and then heated at 50 cm / min. 3 Oxygen was introduced into the tubular heating furnace at a flow rate of 2°C / min, and the temperature was kept at this temperature for 1 hour. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min, and then heated at 25 cm / min. 3 Water vapor was introduced into the tubular heating furnace at a flow rate of / min to obtain 22.1 g of a modified conductive agent.
[0073] S4. Preparation of positive electrode for sodium ion battery
[0074] 70.5 g of modified transition metal oxide, 10.2 g of modified crosslinking agent, 14.2 g of modified conductive agent, 89.8 g of N-methylpyrrolidone and 0.7 g of carbon fiber were uniformly mixed to obtain a mixed slurry;
[0075] The mixed slurry was evenly coated on the surface of an aluminum foil with a thickness of 25 μm to form a thin sheet, and placed in a vacuum drying oven at 120° C. for 12 hours to obtain a composite positive electrode material.
[0076] S5. Preparation of sodium ion batteries
[0077] The composite positive electrode material is weighed and rolled to obtain a positive electrode sheet, and the negative electrode sheet is obtained by vacuum stirring, coating, cold pressing, and cutting hard carbon: conductive carbon black: carboxymethyl cellulose: styrene butadiene rubber = 90:3:2:2;
[0078] The positive electrode sheet, the negative electrode sheet, the electrolyte (1 mol / L NaPF6 dissolved in a mixed solvent of ethylene carbonate: diethyl carbonate with a volume ratio of 1:1) and the glass fiber separator are assembled into a button cell (button battery).
[0079] Example 3
[0080] This embodiment provides a method for preparing a positive electrode composite material for a sodium ion battery, comprising the following steps:
[0081] S1. Preparation of modified transition metal oxides
[0082] Weigh 132.5g Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15 O2 and 13.5g lithium borohydride were mixed evenly and placed in a tubular furnace, nitrogen was introduced for protection, the tubular heating furnace was heated to 800°C at a rate of 10°C / min, and the temperature was kept for reaction for 2h to obtain 141.2g borated transition metal oxide;
[0083] After 100.0 g of borided transition metal oxide was transferred to a tubular furnace, nitrogen was introduced for protection, and the tubular furnace was heated to 300 °C at a rate of 10 °C / min and then heated at 40 cm / min. 3 A mixed gas consisting of 5% methanol gas and 95% nitrogen gas was introduced into the tubular heating furnace at a flow rate of 15 Torr / min, and the pressure was set to 15 Torr. The mixture was kept warm for 2 hours. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min to obtain 103.8 g of modified transition metal oxide.
[0084] S2. Preparation of modified crosslinking agent
[0085] Weigh 26.9g 4,4'-oxydiphthalic anhydride, 20.1g 4,4'-diaminodiphenyl sulfone, 201.4g N-methylpyrrolidone and 2.7g triethylamine, dissolve 4,4'-diaminodiphenyl sulfone in N-methylpyrrolidone, add 4,4'-oxydiphthalic anhydride in batches while stirring for 3h at room temperature, the stirring rate is 180rpm, and the amount added each time is half of the remaining 4,4'-oxydiphthalic anhydride. After the reaction is completed, 45.3g of anhydride-terminated polyamic acid glue is obtained;
[0086] Weigh 18.5g of anhydride-terminated polyamic acid glue and 1.9g of 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane, 42.5g of N,N-dimethylformamide and 0.7g of triethylamine into a reactor, raise the temperature of the reactor to 50°C, and keep the reaction for 3h. After the reactor is cooled to room temperature, add the reaction solution into a rotary evaporator with a water bath temperature of 100°C, and distill under reduced pressure until no liquid is produced to obtain 20.1g of modified cross-linking agent.
[0087] S3. Preparation of modified conductive agent
[0088] 25.0 g of natural flake graphite and 265.3 g of N-methylpyrrolidone were weighed and added into a reactor. The temperature of the reactor was raised to 150° C. After the reaction was carried out for 4 hours, the reactor was placed in an ultrasonic disperser with a frequency of 30 kHz, and ultrasonicated at room temperature for 20 hours to obtain a dispersed solution.
[0089] The dispersed solution was transferred to a centrifuge tube, the speed was set to 1500 rpm, and the upper layer of the solution was filtered after centrifugation at room temperature for 0.5 h. The filter cake was vacuum dried at 60 ° C for 24 h to obtain 23.1 g of graphene;
[0090] 20.0g of graphene is placed in a pressure chamber of 10 -2 Torr ammonia nitriding furnace, introduce high-purity ammonia, maintain the gas pressure at 0.1 Torr, raise the temperature to 500°C, keep the temperature for 2 hours, gradually cool the sample chamber to room temperature, and obtain 21.5g of nitrided graphene;
[0091] After 20.0 g of nitrided graphene was transferred to a tubular furnace, nitrogen was introduced for protection, and the tubular furnace was heated to 300 °C at a rate of 10 °C / min and then heated at 50 cm / min. 3 Oxygen was introduced into the tubular heating furnace at a flow rate of 2°C / min, and the temperature was kept at this temperature for 1 hour. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min, and then heated at 25 cm / min. 3 Water vapor was introduced into the tubular heating furnace at a flow rate of / min to obtain 21.3 g of a modified conductive agent.
[0092] S4. Preparation of positive electrode for sodium ion battery
[0093] Weigh 78.5 g of modified transition metal oxide, 12.3 g of modified crosslinking agent, 18.2 g of modified conductive agent, 87.7 g of N-methylpyrrolidone and 0.8 g of carbon fiber and mix them evenly to obtain a mixed slurry;
[0094] The mixed slurry was evenly coated on the surface of an aluminum foil with a thickness of 25 μm to form a thin sheet, and placed in a vacuum drying oven at 120° C. for 12 hours to obtain a composite positive electrode material.
[0095] S5. Preparation of sodium ion batteries
[0096] The positive electrode sheet is obtained by rolling the composite positive electrode material, and the negative electrode sheet is obtained by vacuum stirring, coating, cold pressing and cutting hard carbon: conductive carbon black: carboxymethyl cellulose: styrene butadiene rubber = 90:3:2:2;
[0097] The positive electrode sheet, the negative electrode sheet, the electrolyte (1 mol / L NaPF6 dissolved in a mixed solvent of ethylene carbonate: diethyl carbonate with a volume ratio of 1:1) and the glass fiber separator are assembled into a button cell (button battery).
[0098] Comparative Example 1
[0099] The difference between this comparative example and Example 3 is that step S1 is eliminated and in step S4, Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15 O2 replaces the modified transition metal oxide in equal amounts.
[0100] Comparative Example 2
[0101] The difference between this comparative example and Example 3 is that step S2 is eliminated, and in step S4, an equal amount of polyvinyl alcohol is used to replace the modified cross-linking agent.
[0102] Comparative Example 3
[0103] The difference between this comparative example and Example 3 is that step S3 is eliminated, and in step S2, an equal amount of single-walled carbon nanotubes is used to replace the modified conductive agent.
[0104] Performance testing:
[0105] The conductivity, first charge efficiency, cycle performance test, discharge capacity corresponding to a current density of 0.2C, slurry stability, air stability and rate performance of the button-type batteries prepared using the composite positive electrode materials of Examples 1-3 and Comparative Examples 1-3 were tested, and the test results are shown in Table 1.
[0106] The conductivity of the composite positive electrode material is tested according to the standard SJ / T 11792-2022 "Test method for conductivity of lithium-ion battery electrode materials";
[0107] The test method for the first charge efficiency is: first charge from the open circuit voltage to 4.2V with a current of 0.1C, then charge at a constant voltage of 4.2V with a cut-off current of 0.01C, and finally discharge at 0.2C to 3.0V. The first charge efficiency is obtained by dividing the discharge capacity by the charge capacity.
[0108] The method of cycle performance test is: charge to 4.1V at 0.5C, then charge at 4.1V constant voltage with a cut-off current of 0.02C, discharge to 3.0V at 0.5C, and use this discharge capacity as the cycle discharge capacity for comparison. The highest discharge capacity in the first three cycles of the cycle discharge capacity is taken as 100%;
[0109] The test method for the discharge capacity corresponding to the current density of 0.2C is as follows: first, place the button battery in a 25±2℃ environment for 8h, charge it to 4.0V with a constant current of 0.2C, then let it stand for 5min, and then discharge it to 2.0V with a constant current of 0.2C; then let it stand for 5min, then charge it to 4.0V with a constant current of 0.2C, let it stand for 5min, and then discharge it to 2.0V with a constant current of 0.2C. The obtained capacity is the discharge capacity corresponding to 0.2C. Finally, stop the operation and record the second discharge capacity as the discharge capacity corresponding to 0.2C.
[0110] The test method for slurry stability is as follows: use a test cup to take the prepared slurry and place it in air with a dew point of -20°C for static placement. Select the rotation speed and measurement range, and measure the viscosity change for 24 hours. After the test, record the test results and perform data analysis and processing.
[0111] The test method for air stability is: take the sample and lay it flat in an environment with a humidity of 50%. After leaving it for 10 hours, immediately transfer it to an environment with a humidity below 5% and prepare it for a buckle test. The discharge capacity corresponding to the test current density of 0.2C is tested.
[0112] The test method for rate performance is: record 0.1C constant current and constant voltage charging to 4.0V; 0.1C discharge to 2.0V, the resulting capacity is C1; record 0.1C constant current and constant voltage charging to 4.0V; 5C discharge to 2.0V, the resulting capacity is C2; the rate performance of the battery is measured by the calculated value of C2 / C1×100%.
[0113] Table 1. Test results of samples
[0114]
[0115]
[0116] Data Analysis:
[0117] Analysis of the data in Table 1 shows that the conductivity of the sodium ion battery prepared by using the composite positive electrode material prepared in this experiment reaches 0.12S / cm, the first charge efficiency reaches 89.9%, the cycle performance reaches 94.1%, the discharge capacity corresponding to the current density of 0.2C reaches 156.3mAh / g, the slurry stability reaches 21500mPA·s, and the discharge capacity corresponding to the current density of 0.2C after air humidification treatment reaches 153.6mAh / g, and the rate performance reaches 92.3%.
[0118] By comparing the data of Example 3 and Comparative Example 1, it can be found that by using the surface Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15 The sodium ion battery prepared by surface treatment with modified transition metal oxides is more 0.67 Mn 0.65 Fe 0.2 Ni 0.15 The sodium ion battery prepared by O2 has significantly improved slurry stability and air stability, and the conductivity of the composite positive electrode material has also been significantly improved, indicating that this experiment 0.67 Mn 0.65 Fe 0.2 Ni 0.15 The products obtained by surface modification with O2 provide a basis for improving the conductivity and air stability of composite positive electrode materials.
[0119] By comparing and analyzing the data of Example 3 and Comparative Example 2, it can be found that the sodium ion battery prepared by using the modified cross-linking agent prepared in this experiment has significantly improved cycle performance, discharge capacity, slurry stability and air temperature resistance compared to the sodium ion battery prepared using polyvinyl alcohol as a cross-linking agent, and the conductivity of the composite positive electrode material is significantly improved, indicating that the cross-linking agent prepared in this experiment makes the positive electrode structure more compact, indicating that the modified cross-linking agent prepared in this experiment has a significant effect on improving the performance of the battery composite positive electrode material.
[0120] By comparing and analyzing the data of Example 3 and Comparative Example 3, it can be found that the sodium ion battery prepared by using the modified conductive agent prepared in this experiment has significantly improved rate performance, discharge capacity, slurry stability and air temperature resistance compared to the sodium ion battery prepared using single-walled carbon nanotube alcohol as the conductive agent, and the conductive performance of the composite positive electrode material is significantly improved, indicating that the conductive agent prepared in this experiment has excellent cross-linking effect with the cross-linking agent after surface modification, and its own excellent performance and stability also significantly improve the battery effect.
[0121] In summary, the present invention obtains a modified transition metal oxide by modifying the transition metal oxide, prepares a modified cross-linking agent, modifies the graphene to obtain a modified conductive agent, and mixes the three modified raw materials, a solvent and a filler to obtain a positive electrode composite material for a sodium ion battery with high conductivity, high stability, high capacity and high cycle performance.
[0122] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0123] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0124] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A positive electrode composite material for a sodium ion battery, characterized in that: The invention comprises the following raw material components in parts by weight: 60-80 parts of modified transition metal oxide, 5-15 parts of modified cross-linking agent, 10-20 parts of modified conductive agent, 85-95 parts of solvent and 0.5-1 part of filler; The filler is one or more of single-walled carbon nanotubes, silicon dioxide, graphite and carbon fiber; and the solvent is N-methylpyrrolidone.
2. The positive electrode composite material for sodium ion battery according to claim 1, characterized in that: The preparation method of the modified transition metal oxide is as follows: after the boronized transition metal oxide is transferred to a tubular furnace, nitrogen is introduced for protection, the tubular heating furnace is heated to 300±5°C at a rate of 10°C / min, and then heated at a rate of 30-50cm 3 A mixed gas consisting of 5% methanol gas and 95% nitrogen gas is introduced into the tubular heating furnace at a flow rate of 1 / min, the pressure is set to 10-20 Torr, and the temperature is kept for 1-3 hours. After the heating is terminated, the tubular heating furnace is cooled to room temperature at a rate of 2°C / min to obtain a modified transition metal oxide.
3. A sodium ion battery cathode composite material according to claim 2, characterized in that: The preparation method of borided transition metal oxide is as follows: 15-20 parts of transition metal oxide and 1-2 parts of lithium borohydride are weighed by weight, mixed evenly and placed in a tubular furnace, nitrogen is introduced for protection, the tubular heating furnace is increased to 800±5°C at a rate of 10°C / min, and the temperature is kept for reaction for 1-3h to obtain borided transition metal oxide.
4. The positive electrode composite material for sodium ion battery according to claim 3, characterized in that: Transition metal oxide is NaNi 0.7 Mn 0.15 Co 0.15 O2、NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Na 0.67 Mn 0.65 Fe 0.2 Ni 0.15 One or more of O2.
5. The positive electrode composite material for sodium ion battery according to claim 1, characterized in that: The preparation method of the modified crosslinking agent comprises the following steps: A1. Weigh 16-24 parts of 4,4'-oxydiphthalic anhydride, 12-18 parts of 4,4'-diaminodiphenyl sulfone, 100-200 parts of N-methylpyrrolidone and 2-3 parts of triethylamine by weight, dissolve 4,4'-diaminodiphenyl sulfone in N-methylpyrrolidone, add 4,4'-oxydiphthalic anhydride in batches while stirring at room temperature for 2-4h, and add each time in an amount of half of the remaining 4,4'-oxydiphthalic anhydride. After the reaction is completed, an anhydride-terminated polyamic acid glue solution is obtained; A2. 10-20 parts of anhydride-terminated polyamic acid glue, 1-2 parts of 3-[bis(2-hydroxyethyl)amino]propanetriethoxysilane, 40-50 parts of N,N-dimethylformamide and 0.5-0.8 parts of triethylamine are weighed by weight and added into a reactor. The temperature of the reactor is increased to 40-60°C, and the reaction is kept warm for 2-4 hours. The modified cross-linking agent is obtained by post-treatment.
6. The positive electrode composite material for sodium ion battery according to claim 1, characterized in that: The preparation method of the modified conductive agent comprises the following steps: B1. Weigh 1-3 parts of natural flake graphite and 20-30 parts of N-methylpyrrolidone by weight and add them into a reactor. The temperature of the reactor is raised to 140-160° C., and the reaction is kept warm for 3-5 hours. Then, the reactor is placed in an ultrasonic disperser with a frequency of 20-40 kHz, and ultrasonicated at room temperature for 16-24 hours to obtain a dispersed solution. B2. Transfer the dispersed solution to a centrifuge tube, set the speed to 1200-1600 rpm, centrifuge at room temperature for 0.5-1 h, take the upper layer of the solution and filter it, and vacuum dry the obtained filter cake at 60 ° C for 24 h to obtain graphene; B3. Place graphene in a pressure chamber of 10 -2 -10 -3 In a 1000-20000 ℃ ammonia nitriding furnace, high-purity ammonia is introduced, the gas pressure is maintained at 0.1-1 Torr, the temperature is raised to 500-800 ℃, the temperature is kept for 2-3 hours, and the sample chamber is gradually cooled to room temperature to obtain nitrided graphene; B4. After the nitrided graphene is transferred to the tubular furnace, nitrogen is introduced for protection. The tubular heating furnace is heated to 300±5℃ at a rate of 10℃ / min and then heated to 50cm 3 Oxygen was introduced into the tubular heating furnace at a flow rate of 2°C / min, and the temperature was kept at this temperature for 1-2 hours. After the heating was terminated, the tubular heating furnace was cooled to room temperature at a rate of 2°C / min, and then heated at a rate of 25 cm / min. 3 Water vapor is introduced into the tubular heating furnace at a flow rate of 100 Å / min to obtain a modified conductive agent.
7. A method for preparing a positive electrode composite material for a sodium ion battery according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, uniformly mixing a modified transition metal oxide, a modified cross-linking agent, a modified conductive agent, a solvent and a filler to obtain a mixed slurry; S2. The mixed slurry is evenly coated on the surface of an aluminum foil with a thickness of 25 μm to form a thin sheet, and the sheet is placed in a vacuum drying oven at 120° C. and dried for 12 hours to obtain a composite positive electrode material.
Citation Information
Cited By
Lithium battery pack with excellent cycle performance and preparation method thereof
CN120015949A