Positive electrode material and preparation method thereof, positive electrode plate and battery

By introducing Co4+ into the manganese-based tunnel Na0.44MnO2 material to form a layered-tunnel heterostructure, the problems of low specific capacity and poor cycle stability of the material are solved, and battery performance with high rate and long cycle life is achieved, which is suitable for large-scale Production.

CN118738375APending Publication Date: 2024-10-01JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411179324.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The manganese-based tunnel Na0.44MnO2 material has low specific capacity and poor cycle stability due to the Jahn-Teller distortion of Mn3+ in MnO6 in the structure. It is difficult to meet the needs of modern energy storage. There are existing improvement methods such as doping transition metals and heterojunction core-shell structures. The process is complex and it is difficult to achieve the balance between high capacity and long cycle life.

Method used

By introducing the third element Co4+ to replace part of Mn3+, a layered-tunnel heterostructure sodium-ion battery cathode material NaxMnyCo1-yO2 is formed. It is synthesized using a simple and controllable one-step solid-phase method to form a tunnel and layered composite structure, which reduces Jahn -Teller distortion effect and accelerates the diffusion of sodium ions and electrons.

Benefits of technology

It significantly improves the rate performance and cycle performance of the cathode material, achieves the structural stability and electrochemical activity of the material, is suitable for large-scale production, and overcomes the problems of low capacity and poor stability in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738375A_ABST
    Figure CN118738375A_ABST
Patent Text Reader

Abstract

The invention relates to a positive electrode material and a preparation method thereof, a positive electrode plate and a battery. The positive electrode material comprises a layered-tunnel type heterostructure sodium ion battery positive electrode material, and the chemical general formula of the layered-tunnel type heterostructure sodium ion battery positive electrode material is Na < x > Mn < y > Co < 1-y > O < 2 >, wherein x is more than or equal to 0.4 and less than 0.65, and y is more than or equal to 0.8 and less than 1. According to the positive electrode material, the rate capability and the cycle performance of a battery using the positive electrode material can be remarkably improved, the preparation method is simple and controllable, and large-scale production can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet and a battery. Background Art

[0002] In recent years, with the continuous development of advanced energy storage system (ESS) technology, the application of Na + The further development of deintercalation technology also puts forward higher requirements for the high capacity, energy density and long cycle life of sodium ion batteries. Based on the successful application of LiMeO2 in lithium ion battery systems, its advantages such as large theoretical capacity, low cost and simple synthesis make Na x MeO2 has also received widespread attention, but cathode materials generally face the problem of balancing high capacity, long cycle life and excellent rate performance. 0.44 MnO2 material has MnO6 in its structure. 3+ The low specific capacity and poor cycle stability caused by the Jahn-Teller distortion make it difficult to meet the rapidly developing energy storage needs of modern times.

[0003] Studies have shown that Mn 2+ Ions in Na 0.44 The formation of MnO2 nanoparticles is the main cause of capacity decay, so limiting the 2+ The formation of Na 0.44 An effective method for maintaining the capacity of MnO2. 0.44 The improvement of MnO2 usually uses cation substitution, such as Ni, Cu, Ti and other elements, by replacing part of Mn 3+ To increase the average valence state of Mn and reduce the dissolution of Mn. Although the electronic structure of the material can be improved by doping with transition metals to increase the capacity, the effect of maintaining a single phase on its electrochemical performance is limited. By introducing a third element to adjust the structure, the material is hybridized, and a partial transition occurs from the tunnel type to the P2 phase, thereby forming a tunnel and layered composite structure. Moreover, due to the synergistic effect of its heterogeneous structure, it can not only improve the structural stability of the material, but also accelerate the electron and Na + The diffusion rate of the nanostructured carbon nanotubes can be increased, thereby significantly improving its rate performance and cycle performance.

[0004] In the Chinese patent with application number "CN201510509454.6" and patent name "Method for preparing manganese-based positive electrode materials with layered-tunnel composite structure for sodium ion batteries", by combining the advantages of layered structure and tunnel structure, the functional performance of P2 layered-tunnel composite materials is improved compared with layered structure materials; however, the improvement in cycle stability and rate performance of the materials produced is still not ideal.

[0005] In the Chinese patent with application number "202210426239.X" and patent name "Preparation method and positive electrode material of sodium manganese oxygen positive electrode material for heterojunction sodium ion battery", the different diffusion kinetics of Na and Ti elements are used to first form a layered oxide core and then add a titanium source. The shell of the tunnel structure is calcined on the surface of the spherical particles with a layered structure, thereby forming a heterojunction core-shell structure. This process adopts a two-step synthesis method. First, the layered core is made by coprecipitation, and then the shell is formed by a solid phase method. Because it is a two-step synthesis, both the layered core and the tunnel-type shell need to be carefully controlled, and the process is relatively complicated.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a positive electrode material and a preparation method thereof, a positive electrode sheet and a battery. The positive electrode material provided by the present invention can significantly improve the rate performance and cycle performance of a battery using the positive electrode material, and the preparation method is simple and controllable, and can be mass-produced.

[0008] The present invention solves the above technical problems through the following technical solutions: The first aspect of the present invention provides a positive electrode material, the positive electrode material includes a layered-tunnel type heterostructure sodium ion battery positive electrode material, the chemical formula of the layered-tunnel type heterostructure sodium ion battery positive electrode material is: Na x Mn y Co 1-y O2; Among them, 0.4≤x<0.65, 0.8≤y<1.

[0009] Preferably, x satisfies: 0.44≤x<0.6.

[0010] Preferably, y satisfies: 0.9≤y<1.

[0011] Preferably, the mass of the Co element accounts for 1% to 10% of the total mass of the layered-tunnel type heterostructure sodium ion battery positive electrode material.

[0012] The second aspect of the present invention provides a method for preparing the positive electrode material according to the first aspect of the present invention, comprising the following steps: S1: ball milling the Mn source, the Na source and the Co source for the first time to obtain a mixture precursor A; S2: heating the mixture precursor A obtained in step S1 for the first time to obtain a mixture precursor B; S3: ball-milling the mixture precursor B obtained in step S2 for a second time, and then heating it for a second time to obtain the positive electrode material.

[0013] Preferably, the molar ratio of the Na source, Mn source and Co source is (0.4-0.65): (0.8-0.99): (0.01-0.2).

[0014] Preferably, in step S1, the rotation speed of the first ball milling is (600-1000) rpm.

[0015] Preferably, in step S1, the duration of the first ball milling is (0.5-2) hours.

[0016] Preferably, in step S2, the temperature of the first heating is (200-500)°C.

[0017] Preferably, in step S2, the first heating lasts for (1-3) hours.

[0018] Preferably, in step S2, the heating rate of the first heating is 3°C / min to 7°C / min.

[0019] Preferably, in step S3, the rotation speed of the second ball milling is (800-1200) rpm.

[0020] Preferably, in step S3, the duration of the second ball milling is (1-3) hours.

[0021] Preferably, in step S3, the temperature of the second heating is (650-950)°C.

[0022] Preferably, in step S3, the duration of the second heating is (8-12) hours.

[0023] Preferably, in step S3, the heating rate of the second heating is 3°C / min to 7°C / min.

[0024] Preferably, the Mn source includes at least one of manganese dioxide, manganese carbonate, manganese nitrate or manganese acetate.

[0025] Preferably, the Na source includes at least one of sodium carbonate, sodium nitrate or sodium acetate.

[0026] Preferably, the Co source includes at least one of cobalt oxide, cobalt trioxide or cobalt tetroxide.

[0027] The third aspect of the present invention provides a positive electrode plate, which includes a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material is the positive electrode material as described in the first aspect of the present invention or the positive electrode material prepared according to the preparation method described in the second aspect of the present invention.

[0028] A fourth aspect of the present invention provides a battery, comprising the positive electrode sheet as described in the third aspect of the present invention.

[0029] The present invention has the following beneficial effects: The positive electrode material provided by the present invention successfully introduces the third element Co 4+ Replace part of Mn 3+ , a layered-tunnel heterostructured sodium-ion battery cathode material is obtained, which can achieve the stability of the host lattice structure of the cathode material during the charge and discharge process and successfully reduce the Jahn-Teller distortion effect that causes structural degradation and material capacity loss. At the same time, the layered-tunnel heterostructure can accelerate the electron and Na by providing a three-dimensional sodium ion channel. + The diffusion rate is increased, the redox kinetics process is effectively improved, and the electrochemical activity of the material is significantly enhanced, so that the battery prepared from the material has higher rate performance and cycle performance.

[0030] The method for preparing the layered-tunnel type heterostructured sodium ion battery positive electrode material proposed in the present invention can realize large-scale production by synthesizing the material through a simple, process-controllable one-step solid-phase method.

[0031] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings: Figure 1 The positive electrode material obtained in Example 1 and the tunnel-type material Na 0.44 MnO2 (JCPDS No.27-0750) and P2-type material Na 0.7 MnO 2.05 (JCPDS No.27-0751) XRD comparison patterns. DETAILED DESCRIPTION

[0033] In order to make the technical scheme and beneficial effects of the present invention more obvious and easy to understand, the following is a detailed description by listing specific embodiments. Wherein, the drawings are not necessarily drawn to scale, and local features can be enlarged or reduced to more clearly show the details of local features. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually based on conventional experimental conditions. Reagents and raw materials used in the present invention are commercially available unless otherwise specified.

[0034] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and steps are not described in detail.

[0035] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0036] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.

[0037] Unless otherwise defined, technical and scientific terms used in this application have the same meanings as those in the technical field to which this application belongs.

[0038] If no specific techniques or conditions are specified in the following examples, the conventional techniques or conditions described in the literature in the art, or the conditions recommended by the product instructions and the manufacturer are generally used. The numerical ranges in the following examples all include the endpoint values. [Cathode material]

[0039] The first aspect of the present invention provides a positive electrode material, the positive electrode material includes a layered-tunnel type heterostructure sodium ion battery positive electrode material, the chemical formula of the layered-tunnel type heterostructure sodium ion battery positive electrode material is: Na x Mn y Co 1-y O2; Among them, 0.4≤x<0.65, 0.8≤y<1.

[0040] In the present invention, by introducing the third element Co 4+ Replace part of Mn 3+ , realizing the manganese-based tunneling Na 0.44The hybridization of MnO2 material causes the material to partially transform from the tunnel type to the P2 phase, thereby forming a tunnel and layered composite structure. The layered-tunnel heterostructure sodium ion battery positive electrode material can not only improve the structural stability of the material due to the synergistic effect of its heterostructure, but also accelerate the electron and Na by providing a three-dimensional sodium ion channel. + The diffusion rate is increased, and the redox kinetics process is effectively improved, thereby significantly improving the battery prepared from the positive electrode material, which has strong stability, excellent specific capacity and cycle performance.

[0041] In certain embodiments, the x satisfies: 0.44≤x<0.6, for example 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59 or 0.6, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Too much or too little sodium ion content can easily generate impurity phases, thereby affecting the electrochemical performance and stability of the battery prepared using the positive electrode material. The sodium ion content in the positive electrode material of the present application within the above range can avoid the generation of impurity phases.

[0043] In certain embodiments, y satisfies: 0.9≤y<1, for example 0.9, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98 or 0.99, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In some embodiments, the 1-y satisfies 0.01≤1-y≤0.1, for example 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; thus, by controlling the molar amount of the Co element within the above range, the stability and electrochemical performance of the positive electrode material can be significantly improved.

[0045] In some embodiments, the mass of the Co element accounts for 1% to 10% of the total mass of the layered-tunnel heterostructure sodium ion battery positive electrode material, for example, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; thus, by controlling the mass of the Co element within the above range, the stability and electrochemical performance of the positive electrode material can be significantly improved.

[0046] The present invention successfully introduces the third element Co 4+ Replace part of Mn 3+ The host lattice structure of the positive electrode material is stabilized during the charge and discharge process and the Jahn-Teller distortion effect is successfully reduced, which leads to structural degradation and material capacity loss. The stability of the material and the significant improvement of the electrochemical performance are achieved, which overcomes the manganese-based tunnel Na in the prior art. 0.44 MnO2 material has MnO6 in its structure. 3+ The low specific capacity and poor cycle stability caused by the Jahn-Teller distortion make it difficult to meet the needs of modern rapidly developing energy storage.

[0047] In some embodiments, the layered-tunnel heterostructure sodium ion battery positive electrode material is Na 0.5 Mn 0.95 Co 0.05 O2、Na 0.6 Mn 0.99 Co 0.01 O2、Na 0.44 Mn 0.99 Co 0.01 O2、Na 0.5 Mn 0.99 Co 0.01 O2 or Na 0.5 Mn 0.9 Co 0.1 O2. [Method for preparing positive electrode material]

[0048] The second aspect of the present invention provides a method for preparing the positive electrode material according to the first aspect of the present invention, comprising the following steps: S1: ball milling the Mn source, the Na source and the Co source for the first time to obtain a mixture precursor A; S2: heating the mixture precursor A obtained in step S1 for the first time to obtain a mixture precursor B; S3: ball-milling the mixture precursor B obtained in step S2 for a second time, and then heating it for a second time to obtain the positive electrode material.

[0049] In some embodiments, in step S1, the Mn source, Na source and Co source are ball-milled for the first time by a solid phase method, so that the Mn source, Na source and Co source can be fully mixed, so that the battery prepared using the positive electrode material has better specific capacity and better cycle performance.

[0050] The preparation method of the layered-tunnel type heterostructured sodium ion battery positive electrode material proposed in the embodiment of the present invention is a simple, process-controllable one-step solid phase method preparation method, and the synthesized layered-tunnel type heterostructured sodium ion battery positive electrode material Na x Mn y Co 1-y O2 has good rate performance and cycle performance, which can be mass-produced; by successfully introducing the Co element (Co 4+ ) to achieve material hybridization, realize the combination of tunnel-type and layered structures, and then form a layered-tunnel-type heterostructure, which makes the material more stable during charging and discharging. The battery prepared by this positive electrode material has better specific capacity and better cycle performance.

[0051] It should be understood that since the second aspect of the present application provides a method for preparing the positive electrode material described in the first aspect of the present application, the beneficial effects of the positive electrode material described in any of the above embodiments are applicable to the method for preparing the positive electrode material.

[0052] The above-mentioned "Mn source" refers to a compound used to provide Mn. In the embodiments of the present application, there is no particular restriction on the type of Mn source, and it can be selected according to actual needs. As an example, in some embodiments, the Mn source includes any one of manganese dioxide, manganese carbonate, manganese nitrate or manganese acetate, or a mixture of any two or more in any proportion. Further, in some embodiments, the Mn source is selected from manganese carbonate.

[0053] In the above technical solution, the several Mn sources used are simple in structure, easy to synthesize or easy to obtain, widely available, and have good application effects. In addition, in other embodiments of the present application, the above Mn sources are not limited to the above-mentioned ones. In the case of meeting the requirements of excellent performance of the prepared positive electrode material, the Mn source can also adopt other types.

[0054] The above-mentioned "Na source" refers to a compound for providing Na. In the embodiments of the present application, there is no particular restriction on the type of Na source, and it can be selected according to actual needs. As an example, in some embodiments, the Na source includes any one of sodium carbonate, sodium nitrate or sodium acetate, or a mixture of any two or more in any proportion. Further, in some embodiments, the Na source is selected from sodium carbonate.

[0055] In the above technical solution, the several Na sources used are simple in structure, easy to synthesize or easy to obtain, widely available, and have good application effects. In addition, in other embodiments, the above Na sources are not limited to the above-mentioned ones. Under the condition of meeting the requirements of excellent performance of the prepared positive electrode material, the Na source can also adopt other types.

[0056] The above-mentioned "Co source" refers to a compound for providing Co. In the embodiments of the present application, there is no particular limitation on the type of Co source, and it can be selected according to actual needs. As an example, in some embodiments, the Co source includes any one of cobalt oxide, cobalt trioxide or cobalt tetraoxide, or a mixture of any two or more of them in any proportion. Further, in some embodiments, the Co source is selected from cobalt oxide.

[0057] In the above technical solution, the several Co sources used are simple in structure, easy to synthesize or easy to obtain, widely available, and have good application effects. In addition, in other embodiments, the above Co sources are not limited to the above-mentioned ones. Under the condition of meeting the requirements of excellent performance of the prepared positive electrode material, the Co source can also adopt other types.

[0058] In some embodiments, the molar ratio of the Na source, Mn source and Co source is (0.4-0.65): (0.8-0.99): (0.01-0.2). In some embodiments, the molar ratio of the Na source, Mn source and Co source is (0.44-0.6): (0.9-0.99): (0.01-0.1). For example, the molar ratio of the Na source, Mn source and Co source can be 0.44: 0.9: 0.1, 0.5: 0.95: 0.05, 0.5: 0.99: 0.01, 0.5: 0.9: 0.1 or 0.6: 0.99: 0.01, but is not limited to the molar ratios listed, and other ratios not listed within the ratio range are also applicable.

[0059] It should be pointed out that since some Na sources such as sodium carbonate may volatilize during the preheating process, the amount of sodium source such as sodium carbonate can be appropriately increased when added, such as 1% to 5% sodium carbonate.

[0060] In certain embodiments, in step S1, the rotation speed of the first ball milling is (600-1000) rpm. Further, the rotation speed of the first ball milling is (700-900) rpm, such as 700 rpm, 750 rpm, 800 rpm, 850 rpm or 900 rpm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0061] In certain embodiments, in step S1, the duration of the first ball milling is (0.5-2) hours, such as 0.5 hours, 1 hour, 1.5 hours or 2 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0062] By controlling the ball milling conditions during the preparation of the mixed precursor A, it is helpful to obtain a mixed precursor A with excellent performance, lay the foundation for ultimately obtaining a positive electrode material with excellent performance, and further improve the electrochemical performance of the positive electrode material product.

[0063] In certain embodiments, in step S2, the temperature of the first heating is (200-500)°C, for example, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0064] In certain embodiments, in step S2, the duration of the first heating is (1-3) hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0065] In certain embodiments, in step S2, the heating rate of the first heating is 3°C / min to 7°C / min, for example, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min or 7°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] In certain embodiments, in step S2, the heating is carried out by calcining in an alumina boat.

[0067] By controlling the heating conditions such as the temperature and time during the preparation of the above-mentioned mixture precursor B, it is helpful to obtain a mixture precursor B with excellent performance, lay the foundation for ultimately obtaining a positive electrode material with excellent performance, and further improve the electrochemical performance of the positive electrode material product.

[0068] In certain embodiments, in step S3, the rotation speed of the second ball milling is (800-1200) rpm. Further, the rotation speed of the second ball milling is (900-1100) rpm, such as 900 rpm, 950 rpm, 1000 rpm, 1050 rpm or 1100 rpm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0069] In certain embodiments, in step S3, the duration of the second ball milling is (1-3) hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0070] In certain embodiments, in step S3, the temperature of the second heating is (650-950)°C, for example, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or 950°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0071] In certain embodiments, in step S3, the duration of the second heating is (8-12) hours. Further, the duration of the second heating is (9-11) hours, such as 9 hours, 9.5 hours, 10 hours, 10.5 hours or 11 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0072] In certain embodiments, in step S3, the heating rate of the second heating is 3°C / min to 7°C / min, for example, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min or 7°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0073] In certain embodiments, in step S3, the heating is carried out by calcining in an alumina boat.

[0074] By controlling the ball milling conditions, heating temperature and time and other heating conditions in the above-mentioned preparation process, it is helpful to further improve the electrochemical performance of the prepared positive electrode material product.

[0075] In some embodiments, after the cathode material is prepared, the step of timely storing it in a glove box is also included. Thus, the cathode material can be effectively prevented from contacting with moisture during storage to cause oxidation, and interference from external environmental factors can be avoided to maintain the consistency and stability of the cathode material, and its good electrochemical performance can be maintained, thereby improving the electrochemical performance, cycle life and safety of the prepared battery. [Positive electrode]

[0076] The third aspect of the present invention provides a positive electrode plate, which includes a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material is the positive electrode material as described in the first aspect of the present invention or the positive electrode material prepared according to the preparation method described in the second aspect of the present invention.

[0077] The embodiments of the present application do not particularly limit the types of the conductive agent and the binder in the positive electrode plate, as long as the purpose of the present application can be achieved. For example, the binder may include but is not limited to one or more of polyacrylate, polyimide, polyamide, polyamideimide, polyvinylidene fluoride (PVDF), polystyrene butadiene copolymer (styrene butadiene rubber), polyvinyl alcohol, polytetrafluoroethylene, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose or sodium hydroxymethyl cellulose. The conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, Ketjen black, graphene or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes.

[0078] In certain embodiments, the binder is selected from polyvinylidene fluoride (PVDF).

[0079] In certain embodiments, the conductive agent is selected from conductive carbon black Super P.

[0080] The present application has no particular restriction on the mass ratio of the positive electrode material, the conductive agent, and the binder in the positive electrode sheet. Those skilled in the art can select the ratio according to actual needs as long as the purpose of the present application can be achieved.

[0081] In some embodiments, the mass ratio of the positive electrode active material, the conductive agent and the binder in the positive electrode plate is (8~9.5):(0.2~1.1):(0.2~1.1), for example 8:1:1 or 9:0.5:0.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0082] The present application has no particular limitation on the thickness of the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode sheet is 30 μm to 200 μm.

[0083] The present application has no particular restrictions on the preparation method of the positive electrode sheet, and a preparation method known in the art can be selected as long as the purpose of the present application can be achieved. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: dispersing the positive electrode active material, the conductive agent, and the binder in N-methylpyrrolidone (NMP) solvent and mixing to form a uniform positive electrode slurry, coating the positive electrode slurry on the positive electrode collector, drying, cold pressing, cutting, slitting and re-drying to obtain a positive electrode sheet.

[0084] In some embodiments, the preparation process of the positive electrode plate includes the following steps: dispersing the positive electrode active material, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) in an N-methylpyrrolidone (NMP) solvent in a mass ratio of 9:0.5:0.5 and mixing to form a uniform positive electrode slurry, coating the positive electrode slurry into a thin sheet with aluminum foil as the positive electrode current collector, and after drying completely in a vacuum drying oven, slicing to form a positive electrode plate. [Battery]

[0085] A fourth aspect of the present invention provides a battery, comprising the positive electrode sheet as described in the third aspect of the present invention.

[0086] It should be understood that, since the battery provided in the present application includes the positive electrode plate described in the third aspect of the present invention, the beneficial effects of the positive electrode material described in any of the above embodiments are applicable to the battery.

[0087] In some embodiments, the battery further includes a negative electrode sheet, an electrolyte and a separator. Typically, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator, and the separator is disposed between the positive electrode sheet and the negative electrode sheet. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is disposed between the positive electrode sheet and the negative electrode sheet, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0088] In some embodiments, the battery may be a secondary battery or a primary battery, preferably a secondary battery. For example, the battery may be a sodium ion battery, etc., but is not limited thereto. The battery structure of the present application includes but is not limited to a soft-pack sodium ion battery, a square hard-shell battery, or a cylindrical hard-shell battery, etc.

[0089] The battery of the present application also includes a packaging shell for accommodating a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the art in a sodium ion battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging shell, and it can be a packaging shell known in the art, as long as it can achieve the purpose of the present application.

[0090] The present invention has no special limitation on the method for preparing the battery, and the technical scheme for preparing the positive electrode material into a battery such as a secondary battery, which is well known to those skilled in the art, can be adopted.

[0091] The method of the present invention is described below by means of specific examples. It should be understood that these examples are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following examples; the implementation conditions adopted in the examples can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in routine experiments. Example 1

[0092] 1. Preparation of positive electrode materials, including the following steps: Manganese carbonate (MnCO3), sodium carbonate (Na2CO3) and cobalt oxide (CoO) were ball-milled at a molar ratio of 0.95:0.25:0.05 at 800 rpm for 1 hour to obtain a mixture precursor A; the mixture precursor A was placed in an alumina boat and heated and calcined at 300°C for the first time, and heated at this temperature for 1.5 hours to obtain a mixture precursor B. The mixture precursor B was ball-milled for a second time at 1000 rpm for 2 hours, and then placed in an alumina boat and heated and calcined at 800°C for a second time for 10 hours to obtain the positive electrode material NMCO, which is a layered-tunnel heterostructure sodium ion battery positive electrode material (named Na 0.5 Mn 0.95 Co 0.05 O2); Since the positive electrode material is sensitive to moisture, it needs to be stored in a glove box in time after preparation.

[0093] By adding Na 0.5 Mn 0.95 Co 0.05 O2 and typical tunneling material Na 0.44 MnO2 (JCPDS No.27-0750) and P2-type material Na 0.7 MnO 2.05 The crystal structure of (JCPDS No.27-0751) is compared with the XRD peak type, such as Figure 1 As shown, it can be concluded that the material with layered-tunnel type heterostructure was successfully prepared.

[0094] 2. Preparation of positive electrode The prepared positive electrode material NMCO is used as a positive electrode active material, conductive carbon black Super P is used as a conductive agent, and polyvinylidene fluoride (PVDF) is used as a binder.

[0095] The positive electrode material NMCO, conductive carbon black Super P and polyvinylidene fluoride were mixed in a mass ratio of 9:0.5:0.5, and then an appropriate amount of N-methylpyrrolidone (NMP) was added and stirred evenly. The mixed slurry was coated into a thin sheet with aluminum foil as the current collector, dried in a vacuum drying oven at 120°C for 8 hours to completely remove NMP, and then the positive electrode sheet was made by rounding; the loading amount of the positive electrode active material was about 3 mg / cm 2 .

[0096] 3. Preparation of negative electrode sheet The sodium metal sheet is punched into a small disc with a diameter of 16 mm as the negative electrode.

[0097] 4. Preparation of electrolyte In a drying room, non-aqueous solvents ethylene carbonate (EC) and propylene carbonate (PC) are mixed in a volume ratio of 1:1, and then the solute NaClO4 is added to the solvent to dissolve and mix evenly to obtain an electrolyte, wherein the molar concentration of NaClO4 is 1 mol / L.

[0098] 5. Preparation of isolation film A porous polyethylene film with a thickness of 12 μm was used.

[0099] 6. Preparation of sodium ion button half-cell The negative electrode sheet, the separator, and the positive electrode sheet were arranged in the order of electrolyte and then assembled into a button-type CR3032 half-cell in a glove box. Example 2

[0100] The difference from Example 1 is that: In <Step 1 Preparation of positive electrode material>, manganese carbonate (MnCO3), sodium carbonate (Na2CO3) and cobalt oxide (CoO) were mixed in a molar ratio of 0.99:0.3:0.01, and the obtained positive electrode material was named Na 0.6 Mn 0.99 Co 0.01 O2.

[0101] The rest are the same as in Example 1. Example 3

[0102] The difference from Example 1 is that: In <Step 1 Preparation of positive electrode material>, manganese carbonate (MnCO3), sodium carbonate (Na2CO3) and cobalt oxide (CoO) were mixed in a molar ratio of 0.9:0.22:0.1, and the obtained positive electrode material was named Na 0.44 Mn 0.99 Co 0.01 O2.

[0103] The rest are the same as in Example 1. Example 4

[0104] The difference from Example 1 is that: In <Step 1 Preparation of positive electrode material>, manganese carbonate (MnCO3), sodium carbonate (Na2CO3) and cobalt oxide (CoO) were mixed in a molar ratio of 0.99:0.25:0.01, and the obtained positive electrode material was named Na 0.5 Mn 0.99 Co 0.01 O2.

[0105] The rest are the same as in Example 1. Example 5

[0106] The difference from Example 1 is that: In <Step 1 Preparation of positive electrode materials>, manganese carbonate (MnCO3), sodium carbonate (Na2CO3) and cobalt oxide (CoO) were mixed in a molar ratio of 0.9:0.25:0.1, and the resulting material was named Na 0.5 Mn 0.9 Co 0.1 O2.

[0107] The rest are the same as in Example 1. Comparative Example 1

[0108] The difference from Example 1 is that: In <Step 1 Preparation of positive electrode material>, no Co source was added, manganese carbonate (MnCO3) and sodium carbonate (Na2CO3) were mixed at a molar ratio of 1:0.25, and the obtained material was named Na 0.5 MnO2.

[0109] The rest are the same as in Example 1. Comparative Example 2

[0110] The difference from Example 1 is that: In <Step 1 Preparation of positive electrode materials>, cobalt oxide (CoO) was replaced with nickel oxide (NiO), manganese carbonate (MnCO3), sodium carbonate (Na2CO3) and nickel oxide (NiO) were mixed in a molar ratio of 0.95:0.25:0.05, and the resulting material was named Na 0.5 Mn 0.95 Ni 0.05 O2.

[0111] The rest are the same as in Example 1. Performance Testing

[0112] (1) Test method for 1C and 5C specific capacity: Using the Blue Electric system, at 25°C, charge to 4.0V at a constant current of XC (X=1 or 5), and then discharge to 2.0V at a constant current of XC (X=1 or 5). The discharge capacity at this time is recorded as the XC (X=1 or 5) discharge capacity (C0); specific capacity (mAh / g) = C0 (mAh) / mass of positive electrode material (g); (2) Test method for capacity retention rate after 300 cycles at 5C: Using the Blue Power system, at 25°C, charge the battery to 4.0V at 5C constant current, then discharge it to 2.0V at 5C constant current, and record the discharge capacity at this time as the first charge and discharge capacity; repeat the above charge and discharge process, and record the discharge capacity at the 300th cycle. Capacity retention rate = discharge capacity at the 300th cycle / first charge and discharge capacity*100%.

[0113] The test results are shown in Table 1 below.

[0114] Table 1 sample 1C specific capacity (mAh / g) 5C specific capacity (mAh / g) 5C cycle 300 weeks capacity retention rate (%) Example 1 102.5 70.4 88 Example 2 96.5 65.2 82 Example 3 93.4 61.0 80 Example 4 98.6 87.6 84 Example 5 101.2 68.4 86 Comparative Example 1 74.3 63.1 53 Comparative Example 2 81.3 70.5 71 As shown in Table 1, compared with Na 0.5 MnO2 positive electrode material and Na in Comparative Example 2 doped with Ni 0.5 Mn 0.95 Ni 0.05 O2 positive electrode material, layered-tunnel type heterostructure sodium ion battery positive electrode material Na prepared in Examples 1 to 5 of the present application x Mn y Co 1-y O2 has a more excellent rate performance. Taking the material obtained in Example 4 as an example, the 1C and 5C specific capacities of the materials in Comparative Example 1 and Comparative Example 2 are increased by 24.3 mAh / g and 17.3 mAh / g, 24.5 mAh / g and 17.1 mAh / g respectively.

[0115] As shown in Table 1, compared with Na 0.5 MnO2 positive electrode material and Na in Comparative Example 2 doped with Ni 0.5 Mn 0.95 Ni 0.05 O2 positive electrode material, layered-tunnel type heterostructure sodium ion battery positive electrode material Na prepared in Examples 1 to 5 of the present application x Mn y Co 1-y O2 has better cycle performance, and the capacity retention rate of 5C cycle 300 weeks is above 80%, which is significantly improved compared with the capacity retention rate of comparative example 1 material (53%) and comparative example 2 material (71%).

[0116] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.

Claims

1. A positive electrode material, characterized in that: The positive electrode material includes a layered-tunnel type heterostructured sodium ion battery positive electrode material, and the chemical formula of the layered-tunnel type heterostructured sodium ion battery positive electrode material is: Na x Mn y Co 1-y O2; Among them, 0.4≤x<0.65, 0.8≤y<1.

2. The positive electrode material according to claim 1, characterized in that The x satisfies: 0.44≤x<0.6; and / or, The y satisfies: 0.9≤y<1; and / or, The mass of the Co element accounts for 1% to 10% of the total mass of the layered-tunnel type heterostructure sodium ion battery positive electrode material.

3. A method for preparing the positive electrode material according to claim 1 or 2, characterized in that: The following steps are involved: S1: ball milling the Mn source, the Na source and the Co source for the first time to obtain a mixture precursor A; S2: heating the mixture precursor A obtained in step S1 for the first time to obtain a mixture precursor B; S3: ball-milling the mixture precursor B obtained in step S2 for a second time, and then heating it for a second time to obtain the positive electrode material.

4. The method for preparing the positive electrode material according to claim 3, characterized in that: The molar ratio of the Na source, the Mn source and the Co source is (0.4-0.65): (0.8-0.99): (0.01-0.2).

5. The method for preparing the positive electrode material according to claim 3, characterized in that: In step S1, the rotation speed of the first ball milling is (600-1000) rpm; and / or, The duration of the first ball milling is (0.5~2) hours.

6. The method for preparing the positive electrode material according to claim 3, characterized in that: In step S2, the temperature of the first heating is (200-500)°C; and / or, The duration of the first heating is (1-3) hours; and / or, The heating rate of the first heating is 3°C / min to 7°C / min.

7. The method for preparing the positive electrode material according to claim 3, characterized in that: In step S3, the rotation speed of the second ball milling is (800-1200) rpm; and / or, The duration of the second ball milling is (1-3) hours; and / or, The temperature of the second heating is (650-950)°C; and / or, The duration of the second heating is (8-12) hours; and / or, The heating rate of the second heating is 3°C / min to 7°C / min.

8. The method for preparing a positive electrode material according to any one of claims 3 to 7, characterized in that: The Mn source includes at least one of manganese dioxide, manganese carbonate, manganese nitrate or manganese acetate; and / or, The Na source includes at least one of sodium carbonate, sodium nitrate or sodium acetate; and / or, The Co source includes at least one of cobalt oxide, cobalt trioxide or cobalt tetroxide.

9. A positive electrode sheet, characterized in that: The positive electrode plate comprises a positive electrode active material, a conductive agent and a binder, wherein the positive electrode active material is the positive electrode material according to claim 1 or 2 or the positive electrode material prepared by the preparation method according to any one of claims 3-8.

10. A battery, characterized in that: The battery comprises the positive electrode sheet as claimed in claim 9.

Citation Information

Patent Citations

  • Sodium ion battery positive electrode material, preparation method thereof and sodium ion battery comprising same

    CN109607624A

  • Layered and tunnel-shaped mixed structure sodium ion battery positive electrode material and a preparation method thereof and a sodium ion battery

    CN110729475A

  • Method for solid-phase synthesis of low-cost ultrahigh-water-resistance layered tunnel symbiotic oxide positive electrode material and application thereof in sodium-ion battery

    CN117913267A

  • Active material and secondary battery using the same

    JP2014143013A