A method for recycling waste zinc-manganese batteries to prepare manganese-zinc-iron-based positive electrode materials for sodium ion batteries
By simplifying the recycling process, manganese, zinc and iron in waste zinc-manganese batteries are directly synthesized into sodium ion batteries sodium manganese iron, manganese ferrite positive electrode material, solving the problems of complexity and high cost of traditional recycling technology, and achieving high value-added recycling and industrial applications.
Patent Information
- Application Number
- CN202411217375.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Traditional recycling of zinc-manganese batteries has complex technology, high energy consumption, high cost and low added value of recycling products, making it difficult to promote in industrial production.
Through a method of recycling and preparing manganese-zero-iron-based positive electrode material of sodium ion battery by waste zinc-manganese batteries, the manganese, zinc and iron in waste zinc-manganese batteries are used to directly synthesize high value-added sodium ion battery materials, simplify the recycling process and reduce costs .
The high value-added sodium ion battery material recycling is achieved, reducing recycling costs, avoiding secondary pollution, and improving the recycling rate and industrial application value of the products.
Smart Images

Figure CN118738376B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling and cyclic utilization of electronic waste, and in particular to a method for recycling waste zinc-manganese batteries to prepare manganese-zinc-iron-based positive electrode materials for sodium ion batteries. Background Art
[0002] Zinc-manganese dry batteries have the advantages of low cost and large capacity, and are currently the most widely used consumer primary batteries. The global annual consumption of zinc-manganese batteries is about 14 billion, and it is still growing. Waste zinc-manganese batteries contain a large amount of manganese and zinc and other heavy metal elements. Improper handling of a large number of discarded zinc-manganese batteries will cause soil, water and air pollution. Therefore, it is very important to develop an economically feasible recycling and high-value utilization technology. Recycling waste zinc-manganese batteries to prepare functional materials has gradually become a research hotspot.
[0003] However, waste zinc-manganese dry batteries contain heavy metals such as manganese, zinc, iron, and copper. Traditional recycling methods are too complicated, with high recycling costs and low added value. Most of them only recycle specific metals in waste batteries, and there is also secondary pollution in the recycling process, which is not conducive to promotion and application in actual projects.
[0004] Waste zinc-manganese batteries contain more manganese and zinc. Manganese is usually recovered to prepare MnSO4 or MnCO3; zinc is recovered to prepare zinc chloride. Although the above-mentioned recycled products are in great demand and have a wide range of applications in industrial production, these products are the most basic raw materials in industrial production and have low added value; and the recycling process often involves complex separation and purification processes, and the recycling cost is high. This directly affects the benefits of industrial production, making it difficult for the recycling of zinc-manganese batteries to develop on a large scale in industrial production. Therefore, it is necessary to develop new low-cost recycling processes and high-value-added recycling products, increase the value of product recycling, improve the technical content of production, and synthesize high-value-added products, so as to achieve the purpose of reducing costs and increasing efficiency. Summary of the invention
[0005] In view of the problems of complex separation process, high energy consumption, high cost and low added value of recycled products in existing zinc-manganese battery recycling technology, the present invention provides a method for recycling waste zinc-manganese batteries to prepare manganese-zinc-iron-based positive electrode materials for sodium ion batteries.
[0006] To achieve the above object, the present invention provides a sodium ion battery manganese zinc iron based positive electrode material, the sodium ion battery manganese zinc iron based positive electrode material general formula is Na n Mn 1-x-y Zn x Fe y O2, 0.3< n ≤1.0、0.25≤ x≤0.5, 0.01 <y≤0.5。
[0007] A method for preparing the above-mentioned manganese-zinc-iron-based positive electrode material for a sodium ion battery comprises the following steps:
[0008] S1, recycling and crushing waste zinc-manganese batteries to prepare a first battery powder;
[0009] S2, washing and filtering the first battery powder to obtain a first solution and a second battery powder respectively;
[0010] S3, drying, sorting and removing impurities from the second battery powder to obtain the third battery powder;
[0011] S4, add strong acid solution and co-solvent to the aqueous solution of the third battery powder, and then n Mn 1-x- y Zn x Fe y Add metal zinc powder, iron powder or manganese powder in a stoichiometric ratio in O2 to adjust the manganese-zinc-iron metal ratio in the third battery powder, stir to complete the reaction, and filter to obtain a filter residue and a second solution;
[0012] S5, using the first solution as an alkali solution and a complexing agent and the second solution as a metal solution for a coprecipitation reaction, filtering, washing, and drying to obtain manganese, zinc, and iron hydroxide;
[0013] S6. Mix manganese-zinc-iron hydroxide and sodium salt, and calcine at high temperature to synthesize manganese-zinc-iron based positive electrode material for sodium ion battery.
[0014] Preferably, in step S2, the water washing conditions are: deionized water, water temperature 20-100° C., and the amount of water used is 0.1-10 times the mass of the first battery powder.
[0015] Preferably, in step S3, the drying temperature is 80°C, and the sorting includes: air sorting and screening, wherein the screening uses vibrating screening with a mesh size of 10-300 meshes.
[0016] Preferably, in step S4, the co-solvent includes one or a combination of sodium sulfite, sodium thiosulfate, hydrogen peroxide solution, hydrazine hydrate, and ascorbic acid.
[0017] Preferably, in step S6, the sodium salt includes one or a combination of sodium hydroxide, sodium carbonate, sodium bicarbonate, sodium nitrate and sodium oxalate.
[0018] Preferably, in step S6, the molar ratio of manganese zinc iron hydroxide to sodium salt is: (Mn+Zn+Fe):Na=1.0:(0.3-1.05).
[0019] Preferably, in step S6, the high temperature calcination conditions are: calcination at a temperature of 200-500° C. for 1-24 hours, or calcination at a temperature of 600-1000° C. for 1-48 hours in air or oxygen.
[0020] The present invention discloses a method for recycling waste zinc-manganese batteries to prepare manganese-zinc-iron-based positive electrode materials for sodium ion batteries, which has the following beneficial effects:
[0021] (1) Use the inherent elements of manganese, zinc and iron in waste zinc-manganese batteries to directly synthesize high-value-added sodium ferrite manganese-zinc positive electrode materials for sodium ion batteries;
[0022] (2) Avoid the complicated separation process of the main elements manganese, zinc and iron during the recycling process, thereby reducing the recycling cost;
[0023] (3) The method of the present invention rationally utilizes manganese dioxide, metallic zinc, iron sheet, potassium hydroxide and ammonium chloride, which are the main components of waste zinc-manganese batteries, with a high recovery rate and less secondary pollutants.
[0024] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a flow chart of a method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery using waste zinc-manganese batteries in Example 1 of the present invention;
[0026] Figure 2 This is an XRD diagram of the manganese-zinc-iron-based positive electrode material for a sodium ion battery in Example 1 of the present invention;
[0027] Figure 3 This is a first charge and discharge curve diagram of the manganese-zinc-iron-based positive electrode material for a sodium ion battery in Example 1 of the present invention;
[0028] Figure 4 This is a rate performance diagram of the manganese-zinc-iron-based positive electrode material for a sodium ion battery in Example 1 of the present invention;
[0029] Figure 5 This is a cycle performance diagram of the manganese-zinc-iron based positive electrode material for a sodium ion battery in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages disclosed in the embodiments of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the embodiments of the present invention and are not intended to limit the embodiments of the present invention. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0031] Embodiment 1
[0032] A method for recycling waste zinc-manganese batteries to prepare manganese-zinc-iron-based positive electrode materials for sodium ion batteries, the process is as follows Figure 1 As shown, the specific steps include:
[0033] (1) 1.0 kg of used zinc-manganese batteries were put into a crusher for crushing to obtain 0.96 kg of first battery powder.
[0034] (2) The first battery powder was washed with 500 mL of deionized water at 55° C. and filtered to obtain 473 mL of a first solution and 1.18 kg of a second battery powder.
[0035] (3) The second battery powder was dried in a forced air drying oven at 80°C for 12 h. The diaphragm was first removed by an air separator. Then, a 100-mesh vibrating screen was used to remove the copper cap and iron cylinder, etc., to obtain 0.672 kg of the third battery powder.
[0036] (4) Pour 100 g of the third battery powder into a 1.0 L reactor, add 100 mL of deionized water base liquid, stir evenly, then add 200 mL of 2.5 mol / L dilute sulfuric acid and 15 mL of 20% hydrogen peroxide solution, stir to dissolve completely, add 4.8 g of metallic zinc powder and 13.5 g of metallic iron powder to adjust the manganese-zinc-iron metal ratio to 0.5:0.25:0.25, stir to react completely, and filter to obtain 18.4 g of filter residue and 304 mL of the second solution.
[0037] (5) Using the first solution as the base liquid, 500 mL of an alkaline solution of 2.0 mol / L potassium hydroxide and 0.2 mol / L ammonia water was prepared. Using the second solution as the base liquid, 250 mL of a 2.0 mol / L manganese-zinc-iron metal liquid was prepared. The alkaline solution and the metal liquid were added into the reactor at a constant liquid addition rate using a constant flow pump. The co-precipitation reaction was carried out for 5 hours under the conditions of controlling the pH value at 9.2, the reaction temperature at 60°C, and the stirring speed at 300 r / min. The manganese-zinc-iron hydroxide was obtained by filtration, washing with water, and drying.
[0038] (6) 11.6 g of manganese zinc iron hydroxide and 7.42 g of sodium carbonate were mixed evenly, and calcined at 450 °C for 6 h under air flow, and then heated to 920 °C for 12 h to synthesize sodium manganese zinc ferrite positive electrode material Na 0.7 Mn 0.5 Zn 0.25 Fe 0.25 O2.
[0039] The obtained P2-type layered sodium manganese zinc ferrite positive electrode material Na 0.7 Mn 0.5 Zn 0.25 Fe 0.25 The XRD spectrum of O2 is as follows Figure 2 As shown in the image, the structure of the obtained sodium manganese zinc ferrite positive electrode material for sodium ion battery is a layered P2 phase Na 0.7 Mn 0.5 Zn 0.25 Fe 0.25 O2 structure.
[0040] The P2 type layered sodium ion battery sodium manganese zinc ferrite positive electrode material Na prepared in this embodiment 0.7 Mn 0.5 Zn 0.25 Fe 0.25 O2 is used as the positive electrode active material of sodium ion battery to prepare the battery. The specific steps are:
[0041] Sodium ion button battery was prepared with sodium ion manganese-based positive electrode material as positive electrode active material, metal sodium sheet as negative electrode, 1 mol / L NaPF6 and EC / DMC (volume ratio 1:1) as electrolyte.
[0042] The battery's first charge and discharge curve, rate performance and cycle performance were tested, and the results were as follows: Figure 3~Figure 5 It is shown that the sodium manganese zinc ferrite positive electrode material for sodium ion batteries has a high first discharge capacity (164mAh / g); has excellent rate performance, and under the condition of 5C (500mA / g) current charge and discharge, the discharge capacity can still reach 85mAh / g; has good cycle performance, and the capacity retention rate reaches 77% after 100 charge and discharge cycles at 0.5C current density.
[0043] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery, characterized in that: The general formula of the manganese-zinc-iron-based positive electrode material for sodium-ion batteries is Na n Mn 1-x-y Zn x Fe y O2, 0.3< n ≤1.0、0.25≤ x ≤0.5, 0.01 <y≤0.5; A method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery comprises the following steps: S1, recovering and crushing waste zinc-manganese batteries to prepare a first battery powder; S2, washing and filtering the first battery powder to obtain a first solution and a second battery powder respectively; S3, drying, sorting and removing impurities from the second battery powder to obtain the third battery powder; S4, add strong acid solution and co-solvent to the aqueous solution of the third battery powder, and then n Mn 1-x-y Zn x Fe y Add metal zinc powder, iron powder or manganese powder in a stoichiometric ratio in O2 to adjust the manganese-zinc-iron metal ratio in the third battery powder, stir to complete the reaction, and filter to obtain a filter residue and a second solution; S5, using the first solution as an alkali solution and a complexing agent and the second solution as a metal solution for a coprecipitation reaction, filtering, washing, and drying to obtain manganese, zinc, and iron hydroxide; S6. Mix manganese-zinc-iron hydroxide and sodium salt, and calcine at high temperature to synthesize manganese-zinc-iron based positive electrode material for sodium ion battery.
2. The method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step S2, the washing conditions are: deionized water, water temperature 20-100°C, and the amount of water used is 0.1-10 times the mass of the first battery powder.
3. The method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step S3, the drying temperature is 80°C, and the sorting includes: air sorting and screening, wherein the screening uses vibrating screening with a mesh size of 10-300 meshes.
4. The method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step S4, the co-solvent is one or a combination of sodium sulfite, sodium thiosulfate, hydrogen peroxide solution, hydrazine hydrate, and ascorbic acid.
5. The method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step S6, the sodium salt is one or a combination of sodium hydroxide, sodium carbonate, sodium bicarbonate, sodium nitrate, and sodium oxalate.
6. The method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step S6, the molar ratio of manganese zinc iron hydroxide to sodium salt is: (Mn+Zn+Fe):Na=1.0:(0.3-1.05).
7. The method for preparing a manganese-zinc-iron-based positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step S6, the high temperature calcination conditions are: calcination at a temperature of 200-500° C. for 1-24 hours, or calcination at a temperature of 600-1000° C. for 1-48 hours under air or oxygen conditions.
Citation Information
Patent Citations
Recycling method of waste zinc-manganese batteries
CN110752384A
Method for regenerating sodium battery positive electrode material by using waste lithium manganate
CN115472948A
Method for preparing sodium-ion battery positive electrode material by recycling waste battery positive electrode (nickel cobalt lithium manganate) and application of sodium-ion battery positive electrode material
CN115611321A
Positive electrode material and preparation method and application thereof
CN117613229A
Process for recharging spent batteries involves converting crushed batteries into manganese-zinc-iron solution, precipitating manganese-zinc-iron hydroxides and manganese-zinc-iron carbonates and reacting with iron oxide to form ferrite
DE102004013531A1