Method for preparing platinum catalyst by adopting waste lithium battery negative electrode graphite and application of platinum catalyst

CN118738415APending Publication Date: 2024-10-01RESEARCH INSTITUTE OF TSINGHUA UNIVERSITY IN SHENZHEN
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158977.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-01

Smart Images

  • Figure CN118738415A_ABST
    Figure CN118738415A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a platinum catalyst by adopting waste lithium battery negative electrode graphite. The method comprises the following steps: carrying out high-temperature calcination, ultrasonic treatment and suction filtration on a negative electrode plate obtained after the waste lithium ion battery is disassembled, then preliminarily separating out graphite, and then carrying out calcination, acid leaching, centrifugation, washing, drying and ball milling treatment; oxidizing in concentrated acid, and carrying out suction filtration, washing and drying to obtain an activated graphite carbon source; dropwise adding a platinum compound-ethylene glycol solution into the graphite-ethylene glycol solution, adjusting the pH value of the solution to 9-11, stirring in an oil bath, condensing and refluxing, quenching, adjusting the pH value of the solution to 1-2, carrying out suction filtration and washing until the solution is neutral, drying, and grinding to obtain the graphite-supported platinum catalyst. The waste lithium battery graphite is used as a carrier, ethylene glycol is used for reducing a platinum-containing compound to prepare active platinum nano-particles, and the active platinum nano-particles interact with an acidified carbon carrier, so that the nano platinum particles are uniformly distributed on the carbon carrier. The invention also provides application of the platinum catalyst prepared by the method as a cathode oxygen reduction catalyst in a proton exchange membrane fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new energy materials, and specifically relates to a method for preparing a platinum catalyst by using negative electrode graphite of waste lithium batteries and its application. Background Art

[0002] Lithium-ion batteries have become the most widely used rechargeable batteries and are accepted by the market because of their high energy density, light weight, good cycle life, high energy conversion efficiency, good high rate capability, and no memory effect. Graphite negative electrodes are widely used as negative electrode materials for lithium-ion batteries because of their strong cycle stability, high conductivity, and high thermodynamic stability. Although graphite resources are extensive, the graphite required for lithium batteries is of high purity. Graphite mined from mines must undergo necessary purification before it can be used in the battery market. The purification process is not only costly but also causes environmental pollution. Therefore, the recycling and reuse of negative electrode graphite in waste batteries is an effective way to alleviate the surge in graphite demand and avoid environmental pollution.

[0003] The proton exchange membrane fuel cell is a green fuel cell. Its single cell consists of an anode, a cathode and a proton exchange membrane. The anode is the place where hydrogen fuel is oxidized, and the cathode is the place where the oxidant is reduced. Both electrodes contain catalysts that accelerate the electrochemical reaction of the electrodes, and the proton exchange membrane serves as an electrolyte. The proton exchange membrane fuel cell has the advantages of high energy conversion efficiency, zero emissions, simple structure, high reliability, good safety and low noise, making it the best device to replace the internal combustion engine as a power source for automobiles. However, the slow oxygen reduction reaction (ORR) at the cathode of the proton exchange membrane fuel cell seriously hinders the practical application of fuel cells, so catalysts are needed to improve the reaction kinetics. Platinum-based materials are considered to be an ideal oxygen reduction electrocatalyst. At present, the most commonly used platinum-carbon catalyst in industry is platinum loaded on activated carbon. However, commercial platinum-carbon also has disadvantages such as uneven distribution of platinum particles and corrosion of carbon carriers leading to the shedding of platinum particles, which will lead to the problem of reduced catalytic performance and stability. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art. Firstly, a method for preparing a platinum catalyst by using graphite from the negative electrode of waste lithium batteries is provided.

[0005] The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite provided by the present invention comprises the following steps:

[0006] S1: The negative electrode sheets of the disassembled waste lithium-ion batteries are calcined at high temperature in a nitrogen or argon environment, and graphite is initially separated after ultrasonic and filtration;

[0007] S2 The graphite separated initially is calcined again, immersed in an acid solution, subjected to double decomposition reaction to remove metal impurities, and then centrifuged, washed, and dried to obtain purified black-gray powdered graphite;

[0008] S3 ball-milling the black-gray powdered graphite obtained in step S2 to obtain a graphite particle material;

[0009] S4: placing the ball-milled graphite in concentrated acid for oxidation treatment to generate active groups on the graphite surface, and collecting after filtration, washing, drying, and obtaining an activated graphite carbon source;

[0010] S5. Ultrasonic dispersion of the graphite obtained in step S4 in an ethylene glycol / water solution to prepare a graphite alcohol solution, and ultrasonic dispersion of a platinum compound in an ethylene glycol solution to prepare a platinum compound alcohol solution; then slowly dropwise adding the platinum compound alcohol solution into the graphite alcohol solution, adjusting the pH value of the mixed solution to 9-11 after mixing, stirring and condensing the mixed solution in an oil bath for a period of time, rapidly cooling the mixed solution to 30-40° C., adjusting the pH value of the mixed solution to 1-2 again, filtering and washing until the mixed solution is neutral, and drying and grinding to obtain a graphite-supported platinum catalyst;

[0011] The prepared platinum nanoparticles in the graphite-supported platinum catalyst have a particle size of 4 to 5 nm, a Pt loading of less than 20 wt.%, and an electrochemically active surface area (ECSA) of not less than 50 m 2 ·gPt -1 , the half-wave potential (E1 / 2) is not less than 0.83 V (vs. RHE).

[0012] The present invention also provides the use of the platinum catalyst prepared by the method described above as a cathode oxygen reduction catalyst in a proton exchange membrane fuel cell.

[0013] The invention provides a preparation method of a platinum catalyst carried on recycled negative electrode graphite of waste lithium ion batteries. The catalyst uses a carbon source of the negative electrode of the waste lithium battery as a carrier. The negative electrode graphite of the waste lithium battery belongs to a graphite material with high electrochemical performance, and is a graphite carbon material recycled after acid leaching and impurity removal and acid etching. The quantum active points in the graphite are increased. Moreover, the negative electrode graphite of the waste lithium battery is artificial graphite that has been subjected to high-temperature roasting treatment, has an orderly crystal structure, a graphitization degree of more than 80%, good electrical and thermal conductivity, far exceeding the grade of graphite ore (about 10%), and has better electrochemical performance than ordinary graphite. Reusing it is beneficial to saving energy consumption and reducing production costs. After further alcoholization of platinum and organic alcohol reduction of platinum, active platinum nanoparticles with small nanoparticle size and good dispersibility can be carried, so that the small-sized platinum nanoparticles can have a strong interaction with the activated carbon carrier, hindering the agglomeration of the platinum particles. The platinum and graphite carbon have a stronger binding force, forming a stable chemical bond bridge and making the nano platinum particles evenly distributed on the carbon carrier. When the platinum loading of the Pt / PC catalyst prepared in this way is less than the commercial 20 wt% Pt / C, its electrochemical oxygen reduction performance reaches the standard of commercial platinum carbon, and its stability is higher than that of commercial platinum carbon, which has a good application prospect.

[0014] The present invention realizes the secondary utilization of recycled negative electrode graphite of waste lithium-ion batteries, which not only solves the problem of partial recycling of waste lithium-ion batteries, but also provides a new idea for a new type of carrier for platinum-based catalysts.

[0015] The present invention uses graphite recovered from waste lithium-ion batteries as a raw material, reduces the cost of the prepared platinum-supported catalyst, can recycle resources, and reduces environmental pollution, thus having both social and economic benefits.

[0016] The platinum catalyst prepared by the method of the present invention is used as a cathode oxygen reduction catalyst in a proton exchange membrane fuel cell, which not only reduces the cost of the fuel cell, but also improves the performance stability of the fuel cell due to its excellent electrochemical performance and stability, thereby promoting the commercial application of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a scanning electron microscope (SEM) image of negative electrode graphite prepared from recycled waste lithium-ion batteries in Example 1 of the present invention;

[0018] Figure 2 The X-ray diffraction (XRD) diagram of the negative electrode graphite and graphite-supported platinum prepared from recycled waste lithium-ion batteries in Example 1 of the present invention;

[0019] Figure 3 Transmission electron microscopy (TEM) of a platinum-supported catalyst prepared using recycled waste lithium-ion battery negative electrode graphite in Example 1 of the present invention;

[0020] Figure 4 The cyclic voltammetry (CV) curve of the platinum-supported catalyst prepared by using recycled waste lithium-ion battery negative electrode graphite in Example 1 of the present invention and the commercial Pt / C catalyst;

[0021] Figure 5 The linear voltammetric scanning curve (LSV) of the platinum-supported catalyst prepared by using recycled waste lithium-ion battery negative electrode graphite in Example 1 of the present invention and the commercial Pt / C catalyst;

[0022] Figure 6 The chrono-current (it) curve of the platinum-supported catalyst prepared by using recycled waste lithium-ion battery negative electrode graphite in Example 1 of the present invention and the commercial Pt / C catalyst. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0024] The present invention provides a method for preparing a platinum catalyst using waste lithium battery negative electrode graphite, comprising the following steps:

[0025] S1 calcines the negative electrode sheets from disassembled waste lithium-ion batteries at high temperature in a nitrogen or argon environment, and preliminarily separates graphite after ultrasonic and filtration.

[0026] In this step, the negative electrode plates after disassembly of the waste lithium-ion battery are calcined at a high temperature of 400-600° C. in a nitrogen or argon environment, with a heating rate of 5° C. / min and a heat treatment time of 4-8 hours.

[0027] The disassembled waste lithium-ion battery negative electrode graphite is calcined at high temperature under a nitrogen or argon protective atmosphere. Within this temperature range, on the one hand, the heating degrades or decomposes the organic adhesive, allowing the graphite powder to separate from the metal current collector and achieve graphite de-powdering. At the same time, the organic impurities such as organic adhesives, carbonates, organic salts attached to the negative electrode graphite powder are cracked, the organic matter is converted into nanographite, and the escaped carbon dioxide gas and organic salts are decomposed, thereby achieving the separation of graphite from the negative electrode current collector and resource conversion, so as to ensure the quality of the recycled negative electrode graphite.

[0028] S2 The graphite that has been initially separated is calcined in air again, so that metal impurities such as copper, iron, and aluminum generate metal oxides at high temperature, and then immersed in an acid solution, and the metal impurity elements are removed by double decomposition reaction. After centrifugation, washing, and drying, purified black-gray powdered graphite is obtained.

[0029] The temperature of the preliminarily separated graphite when calcined again is 300-700°C, and the heat treatment time is 1-4 h.

[0030] The purpose of heat treating the waste graphite again in the air is mainly to convert the metal impurities contained into metal oxides, so that it is easier to react with inorganic acids and to facilitate the removal of metal elements such as copper, iron, and aluminum. On the other hand, the free amorphous carbon can be generated under the action of heat treatment to generate carbon dioxide to escape, so that the waste negative electrode graphite powder can be deeply purified. The re-calcined graphite is immersed in 0.5-1.5 mol / L sulfuric acid or hydrochloric acid dilution. The metal oxide undergoes double decomposition reaction under the action of acid to generate soluble metal salts. The double decomposition reaction precipitates metal impurity elements, so that the metal impurity components in the graphite can be removed, and then centrifuged, washed and dried to purify the graphite. The solid-liquid ratio during acid leaching is 10g / L-200g / L, the leaching time is 1-24h, and then centrifuged and settled, and then washed with deionized water and dried at 80-100°C for 10-12h to elute and separate the trace metal ions remaining in the graphite, and further purify the impurities.

[0031] S3: ball-milling the black-gray powdered graphite obtained in step S2, so that the graphite is ground to a nanometer size during the ball-milling process to obtain a graphite particle material.

[0032] When the graphite is subjected to ball milling treatment, the parameters of the ball mill are: a rotation speed of 1000-1500 rpm, a time of 5-10 min, and a particle size of the graphite powder after ball milling of ≤200 nm.

[0033] S4 The ball-milled graphite is placed in concentrated acid for oxidation treatment to generate active groups on the graphite surface, which is then filtered, washed, dried, and collected to obtain an activated graphite carbon source.

[0034] The concentrated acid is selected from one or two of concentrated sulfuric acid, concentrated nitric acid or concentrated phosphoric acid. The amount of concentrated acid used relative to graphite is 40-80 mL / g, the treatment temperature is 100-150° C., and the treatment time is 2-6 h.

[0035] In this step, the powdered graphite after ball milling is oxidized, and concentrated acid or a mixture of two concentrated acids is used for treatment, which can further enhance the oxidation activity, oxidize the CO group in the graphite to generate C-OH, that is, generate active groups such as hydroxyl groups on the graphite surface, and make the ionic valence P and S elements remaining in the graphite layer during the oxidation process become new quantum active points, which is beneficial to the chemical adsorption of platinum ions and the chemical deposition of nano-platinum, and improve the platinum loading of graphite and the chemical stability of the platinum-loaded catalyst.

[0036] S5. Ultrasonic dispersion of the graphite obtained in step S4 in an ethylene glycol / water solution to prepare a graphene alcohol solution, wherein the volume ratio of deionized water to ethylene glycol is 1:1-5, and the mass ratio of graphite to ethylene glycol / water solution is 1-4:20. In addition, ultrasonic dispersion of a platinum compound in an ethylene glycol solution to prepare a platinum compound alcohol solution, wherein the mass ratio of the platinum compound to the ethylene glycol solution is 0.5-1:100 (i.e., the mass concentration of the platinum compound in the ethylene glycol solution is 0.5-1%), and then slowly dropwise addition of the platinum compound alcohol solution into the prepared graphene alcohol solution to form a mixed solution, wherein the volume ratio of the graphene alcohol solution to the platinum compound alcohol solution is 1:1-2, and the pH value of the mixed solution is adjusted to 9-11 with an alkaline solution (ammonia water, sodium hydroxide, etc.), and after stirring in an oil bath to condense and reflux for a period of time, the mixed solution is rapidly cooled to 30-40°C, and the pH value of the mixed solution is adjusted to 1-2 with an organic acid (acetic acid) again, and the mixed solution is filtered and washed until the mixed solution is neutral, and then dried and ground to obtain a graphite-supported platinum catalyst.

[0037] The platinum compound is chloroplatinic acid or hexahydrate chloroplatinic acid. The oil bath stirring condensation reflux temperature is 130-180°C, and the time is 1-6 hours. Within this range, ethylene glycol can be decomposed into aldehydes with reducing properties, and the aldehydes reduce the platinum compound.

[0038] In this step, graphite is ultrasonically dispersed in an ethylene glycol / water solution, and a platinum compound is also dispersed in the ethylene glycol solution, so that the graphite surface contains active groups such as hydroxyl groups, which can form a chemical adsorption effect with ethylene glycol and have organic solubility. Ethylene glycol is coated on the outside of the graphite particles to form a steric hindrance, which reduces the adsorption between graphites and reduces the agglomeration of nanographites, which is conducive to the chemical adsorption of platinum ions with more active points on the graphite surface, ensuring that the platinum metal particles obtained by reduction are nanoparticles. The platinum nanoparticles are loaded on the graphitized carbon carrier by a dropwise addition method, which is conducive to the dispersion of the platinum nanoparticles on the graphitized carbon carrier, so that the binding force between platinum and graphite carbon is stronger, and a stable chemical bond bridge is formed.

[0039] In this step, the pH value of the mixed solution is adjusted to 9-11 for the first time, so that the system is in an alkaline environment to provide sufficient hydroxyl groups and promote the adsorption of hydroxyl groups on the active points of graphite C. Chloroplatinic acid is an acidic substance and is easily hydrolyzed. By adding alkaline substances, the alcoholized structure of chloroplatinic acid can be made more complete and stable. In an alkaline environment, it can ensure that the acidic platinum and alcoholized carbon undergo a stable condensation dehydration reaction, effectively ensuring that the platinum is loaded on the organic carbon chain.

[0040] Since chloride ions are highly active, excessive free chloride ions after the platinum-carbon reaction is completed can make the system acidic. Strong acid systems can easily cause graphite to be corroded and promote the separation of platinum from organic graphite carbon. Therefore, adding alkaline substances and adjusting the solution pH to 1-2 with organic acids again can reduce excessive free chloride ions in the reaction solution, form more neutral salts, and prevent chloride ions from acidifying platinum-loaded graphite.

[0041] The use of condensation reflux heating rapid cooling can ensure that the volatile ethylene glycol returns to the reaction system again, maintaining a stable reaction environment. Under alkaline conditions, the chloroplatinic acid alcohol compound and the hydroxyl groups on the graphite form a complex system through chemical adsorption, and then a dehydration exothermic reaction occurs. By rapidly cooling to 40°C, excessive acidification of chloride ions can be prevented, because chloric acid can reduce the platinum loading of loose graphite C due to acidification. In the exothermic reaction, the thermal motion of chloride ions is very fast, and its swimming speed is reduced by low temperature; and by adjusting and adding alkaline substances, neutral salts can be generated by acid-base reaction, so that the acidity of the solution is reduced, and the acidification effect of chloride ions is reduced, which is beneficial to ensure the morphology and distribution of platinum nanoparticles, and try to avoid the agglomeration of metal particles and the generation of volatile impurities that interfere with the activity of the catalyst. Finally, a catalyst with low impurity content, high redox activity and good stability under acidic conditions can be obtained.

[0042] The applicant has found that the microwave heating reduction method used in the existing carbon-supported platinum preparation technology is likely to cause the original microstructure and properties of graphite (such as interlayer spacing, pore size, specific surface area, interface stress / strain, conductivity, order, etc.) to change, causing a certain degree of damage to the ordered graphite crystal structure, and even causing particle cracking and electrical insulation, and even causing defects such as instability and reversibility in the oxidation and reduction of platinum compounds. In addition, during the reduction reaction, the original coordination characteristics of the reaction platinum complex and its ionization constant in the solution will be destroyed, causing platinum ions to more easily form new chemical bonds with the anions of the solution, hindering the reduction of platinum ions; the microwave effect will also make the reduced platinum atoms more easily detach from the physical adsorption of the carbon carrier, detach from the graphite surface and complex or deposit in the solution, affecting the amount of platinum loaded.

[0043] This step is to adsorb the platinum complex onto the surface of the negative electrode graphite and then perform chemical reduction. This can overcome some existing technical defects, so that the layered ordered structure of the negative electrode graphite will not be changed, the degree of crystallinity is relatively high, the electrochemical performance is good, the platinum loading is also high, and there is a synergistic effect, thereby improving the performance of the platinum-loaded catalyst.

[0044] The particle size of the platinum nanoparticles in the graphite-supported platinum catalyst prepared in this step is 4-5 nm, the particle size distribution range is narrow, the Pt loading is less than 20 wt.%, and the electrochemical active area (ECSA) is not less than 50 m 2 ·gPt -1 , the half-wave potential (E1 / 2) is not less than 0.83 V (vs. RHE), the catalytic reaction activity is high and the cycle stability is good.

[0045] The platinum catalyst prepared by the above preparation method is applied to fuel cells. The carbon source is recovered by activation and used as the carbon source of platinum-supported catalyst in hydrogen fuel cells, which reduces the cost of fuel cells. Active platinum nanoparticles with small nanoparticle size and good dispersibility are prepared by reducing platinum-containing compounds with ethylene glycol. The nanoparticles are uniformly loaded on the acidified carbon carrier and show excellent catalytic reaction activity and stability when applied to the oxygen reduction reaction in hydrogen fuel cells. The results of it chronoamperometric tests show that its stability is higher than that of commercial platinum-carbon catalysts.

[0046] The above preparation method and application are further described in detail below in conjunction with specific embodiments. Embodiment 1:

[0047] S1 The negative electrode sheets of the recycled waste lithium-ion batteries were placed in a tube furnace and calcined at high temperature in a nitrogen atmosphere at a heating rate of 5°C / min, a calcination temperature of 500°C, and a heat treatment time of 6 hours. After calcination, the negative electrode sheets were taken out, ultrasonically treated in deionized water, and filtered to preliminarily separate the graphite.

[0048] S2 The graphite separated initially was calcined again in a muffle furnace, with a heating rate of 5°C / min, a temperature of 600°C, and a heat treatment time of 4 hours, and then immersed in a 1.0 mol / L sulfuric acid solution for electrolysis, with a solid-liquid ratio of 20 g / L and a leaching time of 2 hours. Finally, it was centrifuged for 2 hours, washed with deionized water, and vacuum dried at 80°C for 10 hours to collect the black-gray powdered graphite.

[0049] S3 The graphite prepared in step S2 is ball milled. The parameters of the ball mill are set as follows: speed 1500 rpm, time 5 min. After one ball milling, open the tank, scrape off the powder attached to the inner wall, mix well and then ball mill again. Repeat the above steps until the particle size of the obtained graphite powder is ≤200nm.

[0050] S4: 1 g of graphite obtained in step S3 is oxidized in concentrated sulfuric acid at 120°C, with the amount of concentrated sulfuric acid used being 50 mL for 4 h, followed by filtration, washing, drying and collection.

[0051] S5 Take 60 mg of the graphite in step S4 and ultrasonically disperse it in ethylene glycol / water solution (the volume ratio of deionized water to ethylene glycol is 1:1) to prepare a graphene alcohol solution, wherein the mass ratio of graphite to ethylene glycol / water solution is 1:20, then ultrasonically disperse 80 mg of chloroplatinic acid hexahydrate in ethylene glycol solution to prepare a chloroplatinic acid hexahydrate alcohol solution, wherein the mass ratio of chloroplatinic acid hexahydrate to ethylene glycol solution is 0.5:100, and then slowly add the chloroplatinic acid hexahydrate alcohol solution to the graphene alcohol solution, wherein the volume ratio of graphene alcohol solution to chloroplatinic acid hexahydrate alcohol solution is 1:1. Use 1 mol / L sodium hydroxide solution to adjust the pH to 10 within 0.5 h, stir and condense in an oil bath at 140°C, and after 5 h, quench the mixed solution to 40°C, add 1 mol / L acetic acid solution to adjust the pH to 2, and stir for 16 h. Finally, the product was filtered and washed until neutral, and then dried overnight and ground to obtain the recovered carbon-supported platinum catalyst (Pt / PC).

[0052] In the platinum-based electrocatalyst prepared in this embodiment, the graphite on the negative electrode sheet of the recycled waste lithium-ion battery is used as a carrier. The platinum nanoparticles are uniform in size and evenly distributed on the surface of the carrier. Statistical results show that the particle size of the platinum nanoparticles is 4 nm.

[0053] The structure and performance of this embodiment 1 are as follows:

[0054] from Figure 1 The SEM results show that the block structure obtained by simple treatment of the recycled negative electrode graphite of waste lithium-ion batteries has a high surface roughness, which is conducive to the subsequent loading of Pt particles. Figure 2 As shown, by analyzing the crystal structure of the catalyst sample, it can be seen that the prepared Pt / PC catalyst has a typical Pt characteristic peak, and its characteristic peak position is consistent with the peak position of Pt (PDF#04-001-1793), proving that Pt is successfully loaded on graphite. Figure 3 The TEM image shows that the platinum particles with a size of about 4 nm in the Pt / PC catalyst are evenly distributed on the surface of the negative electrode graphite carrier after simple treatment, and there is no obvious agglomeration between the particles. The Pt content in the Pt / PC catalyst was tested by inductively coupled plasma optical emission spectrometry (ICP-OES), and the composition was about 12.1 wt%.

[0055] The electrochemical performance of the Pt / PC catalyst and the 20 wt% commercial Pt / C catalyst in this example was tested using a standard three-electrode system, in which the counter electrode was a platinum sheet, the reference electrode was a saturated calomel electrode, and the electrolyte was 0.1 M HClO4 electrolyte. Cyclic voltammetry (CV) tests were performed in a N2-saturated electrolyte at 50 mV∙s -1The electrochemical surface areas (ECSA) of the two catalysts were calculated by performing double-layer correction on the charge integral on the hydrogen adsorption peak (0.05-0.4V). Figure 4 The cyclic voltammetry (CV) curves show that the ECSA of the Pt / FNC catalyst is 50.5 m 2 ∙g Pt -l The oxygen reduction reaction test was carried out in an O2-saturated electrolyte with an electrode rotation speed of 1600 rpm and a scan rate of 10 mV∙s -1 , Linear voltammetric sweep voltammetric curve ( Figure 5 ) The results show that the half-wave potential of the Pt / PC catalyst is 0.85 V (vs.RHE), which is better than 0.84 V of 20 wt% commercial Pt / C catalyst.

[0056] The stability of the catalyst in this example was tested by chronoamperometry (it). Figure 6 As shown in the figure, after 50,000 s, the current retention rate of the Pt / PC catalyst in this example is 93%, which is greater than 68% of the 20 wt% commercial Pt / C catalyst. The above results show that the prepared Pt / PC catalyst has excellent cycle stability. Embodiment 2:

[0057] Steps S1 and S2 are the same as those in Example 1.

[0058] S3 The graphite prepared in step S2 is ball-milled. The parameters of the ball mill are set to: speed 1200 rpm, time 8 min. After one ball milling, open the tank, scrape off the powder attached to the inner wall, mix well and then ball mill again. Repeat the above steps until the particle size of the obtained graphite powder is ≤200nm.

[0059] S4: 1 g of graphite obtained in step S3 is oxidized in concentrated nitric acid at 100°C, with the amount of concentrated nitric acid used being 60 mL for 6 h, followed by suction filtration, washing, drying and collection.

[0060] S5 Take 60 mg of the graphite in step S4 and ultrasonically disperse it in ethylene glycol / water solution (the volume ratio of deionized water to ethylene glycol is 1:2) to prepare a graphite alcohol solution, wherein the mass ratio of graphite to ethylene glycol / water solution is 1:10, then ultrasonically disperse 80 mg of chloroplatinic acid hexahydrate in the ethylene glycol solution to prepare a chloroplatinic acid hexahydrate alcohol solution, wherein the mass ratio of chloroplatinic acid hexahydrate to ethylene glycol solution is 1:100, and then slowly add the chloroplatinic acid hexahydrate alcohol solution dropwise to the graphite alcohol solution, wherein the volume ratio of graphite alcohol solution to chloroplatinic acid hexahydrate alcohol solution is 1:2. Use 1 mol / L ammonia water to adjust the pH to 10.5 within 1 hour, stir and condense in an oil bath at 150℃, and after 3 hours, quench the mixed solution to 40℃, add 1 mol / L acetic acid solution to adjust the pH to 1.5, and stir for 16 hours. Finally, the product was filtered and washed until neutral, and then dried overnight and ground to obtain the recovered carbon-supported platinum catalyst (Pt / PC).

[0061] In the platinum-based electrocatalyst prepared in this embodiment, the graphite on the negative electrode sheet of the recycled waste lithium-ion battery is used as a carrier. The platinum nanoparticles are uniform in size and evenly distributed on the surface of the carrier. Statistical results show that the particle size of the platinum nanoparticles is 5 nm.

[0062] The electrochemical performance of the prepared negative electrode graphite supported platinum (Pt / FNC) catalyst was characterized by a standard three-electrode system (RDE), with a platinum sheet as the counter electrode and a saturated calomel electrode as the reference electrode. -1 Cyclic voltammetry (CV) was performed in a 0.1 M HClO4 electrolyte saturated with N2 at a scan rate of 10 mV·s -1 Linear voltammetry (LSV) tests were performed at a scan rate of 1600 rpm. The results showed that the half-wave potential of the Pt / PC catalyst was significantly higher than the 0.84 V of the commercial Pt / C catalyst. Embodiment 3:

[0063] Steps S1 and S2 are the same as those in Example 1.

[0064] S3 The graphite prepared in step S2 is ball milled. The parameters of the ball mill are set to: speed 1300 rpm, time 6 min. After one ball milling, open the tank, scrape off the powder attached to the inner wall, mix well and then ball mill again. Repeat the above steps until the particle size of the obtained graphite powder is ≤200nm.

[0065] S4: 1 g of graphite obtained in step S3 is oxidized in concentrated acid at 120°C. The concentrated acid is a mixture of concentrated phosphoric acid and concentrated nitric acid, with a usage amount of 30 mL of each, for 5 h, followed by filtration, washing, drying and collection.

[0066] S5 Take 60 mg of the graphite in step S4 and ultrasonically disperse it in ethylene glycol / water solution (the volume ratio of deionized water to ethylene glycol is 1:3) to prepare a graphene alcohol solution, wherein the mass ratio of graphite to ethylene glycol / water solution is 1:5, then ultrasonically disperse 80 mg of chloroplatinic acid in ethylene glycol solution to prepare a chloroplatinic acid alcohol solution, wherein the mass ratio of chloroplatinic acid to ethylene glycol solution is 0.6:100, then slowly add the chloroplatinic acid alcohol solution to the graphene alcohol solution, and the volume ratio of graphene alcohol solution to chloroplatinic acid alcohol solution is 1:1.5. Use a 1 mol / L sodium hydroxide solution to adjust the pH to 11 within 2 h, stir and condense in an oil bath at 160°C, and after 2 h, quench the mixed solution to 40°C, add 1 mol / L acetic acid solution to adjust the pH to 1, and stir for 12 h. Finally, filter and wash until neutral, dry the product overnight, and grind it to obtain the recovered carbon-supported platinum catalyst (Pt / PC). In the platinum-based electrocatalyst prepared in this embodiment, the graphite on the negative electrode sheet of the recycled waste lithium-ion battery is used as a carrier. The platinum nanoparticles are uniform in size and evenly distributed on the surface of the carrier. Statistical results show that the particle size of the platinum nanoparticles is 4 nm.

[0067] The electrochemical performance of the prepared negative electrode graphite supported platinum (Pt / FNC) catalyst was characterized by a standard three-electrode system (RDE), with a platinum sheet as the counter electrode and a saturated calomel electrode as the reference electrode. -1 Cyclic voltammetry (CV) was performed in a 0.1 M HClO4 electrolyte saturated with N2 at a scan rate of 10 mV·s -1 Linear voltammetry (LSV) tests were performed at a scan rate of 1600 rpm. The results showed that the half-wave potential of the Pt / PC catalyst was significantly higher than the 0.84 V of the commercial Pt / C catalyst. Embodiment 4:

[0068] Step S1 is the same as that in Example 1.

[0069] S2 The graphite separated initially was calcined again in a muffle furnace, with a heating rate of 5°C / min, a temperature of 600°C, and a heat treatment time of 4 hours, and then immersed in a 1.0 mol / L sulfuric acid solution for electrolysis, with a solid-liquid ratio of 20 g / L and a leaching time of 2 hours. Finally, it was centrifuged for 2 hours, washed with deionized water, and vacuum dried at 80°C for 10 hours to collect the black-gray powdered graphite.

[0070] S3 The graphite prepared in step S2 is ball milled. The parameters of the ball mill are set to: speed 1000 rpm, time 10 min. After one ball milling, open the tank, scrape off the powder attached to the inner wall, mix well and then ball mill again. Repeat the above steps until the particle size of the obtained graphite powder is ≤200nm.

[0071] S4: 1 g of graphite obtained in step S3 is acidified in concentrated acid at 150°C, wherein the concentrated acid is 35 mL of concentrated sulfuric acid and concentrated phosphoric acid, and the time is 3 hours, followed by suction filtration, washing, drying and collection.

[0072] S5 Take 60 mg of the graphite in step S4 and ultrasonically disperse it in ethylene glycol / water solution (the volume ratio of deionized water to ethylene glycol is 1:5) to prepare a graphene alcohol solution, wherein the mass ratio of graphite to ethylene glycol / water solution is 3:20, then ultrasonically disperse 80 mg of chloroplatinic acid in ethylene glycol solution to prepare a chloroplatinic acid alcohol solution, wherein the mass ratio of chloroplatinic acid to ethylene glycol solution is 0.8:100, then slowly add the chloroplatinic acid alcohol solution to the graphene alcohol solution, and the volume ratio of graphene alcohol solution to chloroplatinic acid alcohol solution is 1:2. Use a 1 mol / L sodium hydroxide solution to adjust the pH to 9 within 2 hours, stir and condense in an oil bath at 180°C, and after 1 hour, quench the mixed solution to 40°C, add 1 mol / L acetic acid solution to adjust the pH to 2, and stir for 16 hours. Finally, filter and wash until neutral, dry the product overnight, and grind it to obtain the recovered carbon-supported platinum catalyst (Pt / PC).

[0073] In the platinum-based electrocatalyst prepared in this embodiment, the graphite on the negative electrode sheet of the recycled waste lithium-ion battery is used as a carrier. The platinum nanoparticles are uniform in size and evenly distributed on the surface of the carrier. Statistical results show that the particle size of the platinum nanoparticles is 5 nm.

[0074] The electrochemical performance of the prepared negative electrode graphite supported platinum (Pt / FNC) catalyst was characterized by a standard three-electrode system (RDE), with a platinum sheet as the counter electrode and a saturated calomel electrode as the reference electrode. -1 Cyclic voltammetry (CV) was performed in a 0.1 M HClO4 electrolyte saturated with N2 at a scan rate of 10 mV·s -1 Linear voltammetry (LSV) tests were performed at a scan rate of 1600 rpm. The results showed that the half-wave potential of the Pt / PC catalyst was significantly higher than the 0.84 V of the commercial Pt / C catalyst. Embodiment 5:

[0075] S1 is the same as the step in Example 1.

[0076] S2 The graphite separated initially was calcined again in a muffle furnace, with a heating rate of 5°C / min, a temperature of 600°C, and a heat treatment time of 4 hours, and then immersed in a 1.5mol / L sulfuric acid solution for electrolysis, with a solid-liquid ratio of 200g / L and a leaching time of 24h. Finally, it was centrifuged for 2h, washed with deionized water, and vacuum dried at 100°C for 10h to collect the black-gray powdered graphite.

[0077] S3 The graphite prepared in step S2 is ball milled. The parameters of the ball mill are set to: speed 1000 rpm, time 10 min. After one ball milling, open the tank, scrape off the powder attached to the inner wall, mix well and then ball mill again. Repeat the above steps until the particle size of the obtained graphite powder is ≤200nm.

[0078] S4: 1 g of graphite obtained in step S3 is acidified in concentrated acid at 150°C, wherein the concentrated acid is concentrated sulfuric acid, the amount used is 35 mL, and the time is 4 hours, followed by suction filtration, washing, drying and collection.

[0079] S5 Take 60 mg of the graphite in step S4 and ultrasonically disperse it in ethylene glycol / water solution (the volume ratio of deionized water to ethylene glycol is 1:5) to prepare a graphene alcohol solution, wherein the mass ratio of graphite to ethylene glycol / water solution is 3:20, then ultrasonically disperse 80 mg of chloroplatinic acid in ethylene glycol solution to prepare a chloroplatinic acid alcohol solution, wherein the mass ratio of chloroplatinic acid to ethylene glycol solution is 0.8:100, then slowly add the chloroplatinic acid alcohol solution to the graphene alcohol solution, and the volume ratio of graphene alcohol solution to chloroplatinic acid alcohol solution is 1:2. Use a 1 mol / L sodium hydroxide solution to adjust the pH to 9 within 2 hours, stir and condense in an oil bath at 180°C, and after 1 hour, quench the mixed solution to 40°C, add 1 mol / L acetic acid solution to adjust the pH to 2, and stir for 16 hours. Finally, filter and wash until neutral, dry the product overnight, and grind it to obtain the recovered carbon-supported platinum catalyst (Pt / PC).

[0080] In the platinum-based electrocatalyst prepared in this embodiment, the graphite on the negative electrode sheet of the recycled waste lithium-ion battery is used as a carrier. The platinum nanoparticles are uniform in size and evenly distributed on the surface of the carrier. Statistical results show that the particle size of the platinum nanoparticles is 5 nm.

[0081] The electrochemical performance of the prepared negative electrode graphite supported platinum (Pt / FNC) catalyst was characterized by a standard three-electrode system (RDE), with a platinum sheet as the counter electrode and a saturated calomel electrode as the reference electrode. -1 Cyclic voltammetry (CV) was performed in a 0.1 M HClO4 electrolyte saturated with N2 at a scan rate of 10 mV·s -1Linear voltammetry (LSV) tests were performed at a scan rate of 1600 rpm. The results showed that the half-wave potential of the Pt / PC catalyst was significantly higher than the 0.84 V of the commercial Pt / C catalyst.

[0082] The above-mentioned embodiments of the present invention are only part of the preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made by those skilled in the art without departing from the essence of the present invention are within the protection scope of the present invention.

Claims

1. A method for preparing a platinum catalyst using waste lithium battery negative electrode graphite, comprising the following steps: S1: The negative electrode sheets of the disassembled waste lithium-ion batteries are calcined at high temperature in a nitrogen or argon environment, and graphite is initially separated after ultrasonic and filtration; S2 The graphite separated initially is calcined again and immersed in an acid solution to remove metal impurities by double decomposition reaction. After centrifugation, washing and drying, purified black-grey powdered graphite is obtained; S3 ball-milling the black-gray powdered graphite obtained in step S2 to obtain a graphite particle material; S4: placing the ball-milled graphite in concentrated acid for oxidation treatment to generate active groups on the graphite surface, and collecting after filtration, washing, drying, and obtaining an activated graphite carbon source; S5. Ultrasonic dispersion of the graphite obtained in step S4 in an ethylene glycol / water solution to prepare a graphite alcohol solution, and ultrasonic dispersion of a platinum compound in an ethylene glycol solution to prepare a platinum compound alcohol solution; then slowly dropwise adding the platinum compound alcohol solution into the graphite alcohol solution, adjusting the pH value of the mixed solution to 9-11 after mixing, stirring and condensing the mixed solution in an oil bath for a period of time, rapidly cooling the mixed solution to 30-40° C., adjusting the pH value of the mixed solution to 1-2 again, filtering and washing until the mixed solution is neutral, and drying and grinding to obtain a graphite-supported platinum catalyst; The prepared platinum nanoparticles in the graphite-supported platinum catalyst have a particle size of 4 to 5 nm, a Pt loading of less than 20 wt.%, and an electrochemically active surface area (ECSA) of not less than 50 m 2 ·gPt -1 , the half-wave potential (E1 / 2) is not less than 0.83 V (vs. RHE).

2. The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite as claimed in claim 1, characterized in that: In the step S1, the negative electrode sheets after disassembly of the waste lithium-ion battery are calcined at a high temperature of 400 to 600° C. in a nitrogen or argon environment, with a heating rate of 5° C. / min and a heat treatment time of 4 to 8 hours.

3. The method for preparing a platinum catalyst using graphite from the negative electrode of waste lithium batteries as claimed in claim 2, characterized in that: In the step S2, the graphite initially separated is calcined again at a temperature of 300 to 700°C, and the heat treatment time is 1 to 4 hours.

4. The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite as claimed in claim 1 or 3, characterized in that: In the step S2, the re-calcined graphite is immersed in a 0.5-1.5 mol / L sulfuric acid or hydrochloric acid solution to remove metal impurities, the solid-liquid ratio is 10 g / L-200 g / L, the leaching time is 1-24 hours, and then centrifuged, washed with deionized water and dried at 80-100°C for 10-12 hours.

5. The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite as claimed in claim 1, characterized in that: In the step S3, when the graphite is subjected to ball milling treatment, the parameters of the ball mill are: a rotation speed of 1000 to 1500 rpm and a time of 5 to 10 min.

6. The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite as claimed in claim 1, characterized in that: In the step S4, the concentrated acid is selected from one or two of concentrated sulfuric acid, concentrated nitric acid or concentrated phosphoric acid. During the oxidation treatment, the amount of the concentrated acid used relative to the graphite is 40-80 mL / g, the treatment temperature is 100-150° C., and the treatment time is 2-6 hours.

7. The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite as claimed in claim 1, characterized in that: In the step S5, the volume ratio of deionized water to ethylene glycol is 1:1-5; the mass ratio of graphite to ethylene glycol / water solution is 1-4:20, the mass ratio of platinum compound to ethylene glycol solution is 0.5-1:100, and the volume ratio of graphite alcohol solution to platinum compound alcohol solution is 1:1-2.

8. The method for preparing a platinum catalyst using waste lithium battery negative electrode graphite as claimed in claim 1 or 7, characterized in that: In the step S5, the oil bath stirring condensation reflux temperature is 130-180° C. and the time is 1-6 h.

9. Use of the platinum catalyst prepared by the method according to any one of claims 1 to 8 as a cathode oxygen reduction catalyst in a proton exchange membrane fuel cell.

Citation Information

Cited By

  • Method for preparing platinum catalyst by using waste lithium battery negative electrode graphite and application of platinum catalyst

    CN119702046A