Composite comprising active metal particles and sacrificial metal particles, membrane electrode assembly, and fuel cell comprising same

By using a composite of active metal particles and sacrificial metal particles in a fuel cell, which is independently loaded on a carbon carrier and using sacrificial metal particles on the gas diffusion layer, the problem of precious metal catalyst degradation is solved and the catalyst activity and durability are improved.

CN118738416APending Publication Date: 2024-10-01DAEGU GYEONGBUK INSTITUTE OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410347901.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-03-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Precious metal catalysts (such as platinum, palladium, and gold) in existing fuel cells are prone to deterioration during the oxygen reduction reaction, resulting in reduced catalyst activity and durability. In addition, existing coating methods have problems with by-product poisoning and complex manufacturing processes.

Method used

A composite containing active metal particles and sacrificial metal particles is used. The active metal particles are independently loaded on the carbon carrier. The sacrificial metal particles are located on the gas diffusion layer support and are oxidized or reduced to replace the active metal particles to prevent deterioration.

Benefits of technology

Effectively inhibits the deterioration of active metal particles, maintains catalyst activity, and significantly improves the durability and life of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738416A_ABST
    Figure CN118738416A_ABST
Patent Text Reader

Abstract

The present invention relates to a composite comprising active metal particles and sacrificial metal particles, a membrane electrode assembly, and a fuel cell comprising the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite body comprising active metal particles and sacrificial metal particles, a membrane electrode assembly and a fuel cell comprising the same. Background Art

[0002] Fuel cells are electrochemical devices that convert chemical energy generated by oxidation / reduction of fuel into electrical energy, and are attracting attention as an environmentally friendly energy source.

[0003] The electrode reaction in the fuel cell consists of the hydrogen oxidation reaction (HOR: Hydrogen Oxidation Reaction) in the anode (anode) and the oxygen reduction reaction (ORR: Oxygen Reduction Reaction) in the cathode (cathode). In order to improve the efficiency of this electrochemical reaction, a catalyst must be used. In particular, the oxygen reduction reaction in the cathode is slower than the hydrogen oxidation reaction in the anode, and this reaction speed determines the overall performance of the fuel cell. Therefore, in order to promote the oxygen reduction reaction in the cathode, precious metal catalysts such as platinum (Pt), palladium (Pd), and gold (Au) are currently mainly used.

[0004] As an example, Korean Patent Publication No. 10-1484188 discloses a catalyst in which platinum is supported on a carbon carrier. Such a catalyst reduces the amount of precious metal used in the catalyst and improves the catalyst activity by increasing the active surface area, but the degradation of the supported platinum nanoparticles occurs, and with the continuous consumption of the expensive platinum catalyst and the increase in inefficiency, there is a disadvantage of reduced catalyst activity and durability. Specifically, the degradation of such platinum nanoparticles occurs as air intrudes into the anode and side reactions such as oxygen reduction reaction in the anode and platinum oxidation reaction in the cathode occur. In particular, oxidized platinum (Pt) particles cannot perform oxygen reduction reaction normally, and may cause dissolution and Ostwald ripening of platinum. This leads to aggregation or size growth of platinum (Pt) particles and reduces the utilization efficiency of the platinum catalyst. As a result, due to the degradation of such platinum (Pt) particles, the performance of the fuel cell is reduced.

[0005] As a solution for suppressing such degradation phenomena, research is actively being conducted on coating the surface of active metal particles such as platinum (Pt), palladium (Pd), gold (Au), etc. with carbon or metal oxides. However, this coating method has the following disadvantages: the active sites of the active metal are reduced, and the catalyst is poisoned by the generation of unnecessary byproducts such as hydrogen peroxide due to the two-electron reaction, thereby reducing the activity and stability of the fuel cell. In addition, due to characteristics such as the morphology and surface energy of the catalyst, the manufacturing process is complicated.

[0006] Therefore, in order to provide a fuel cell having significantly improved durability while maintaining the activity of a noble metal-based catalyst, it is necessary to fundamentally solve the problem of degradation of active metals.

[0007] [Prior art literature]

[0008] [Patent Literature]

[0009] Korean Patent Publication No. 10-1484188

[0010]

Non-patent literature

[0011] Chem.Mater.2017,29,21,9579–9587(2017.10.17) Summary of the invention

[0012] An object of the present invention is to provide a composite body and a membrane electrode assembly having excellent catalytic activity and significantly improved durability.

[0013] Another object of the present invention is to provide a fuel cell electrode comprising the composite of the present invention.

[0014] Another object of the present invention is to provide a fuel cell comprising the fuel cell electrode and / or membrane electrode assembly.

[0015] Another object of the present invention is to provide a method for manufacturing the composite body and membrane electrode assembly.

[0016] The present invention provides a composite, characterized in that the composite comprises: a carbon carrier; active metal particles; and sacrificial metal particles, which are oxidized or reduced to replace the active metal particles, wherein the active metal particles and the sacrificial metal particles are independently loaded on the carbon carrier.

[0017] In the composite body according to the present invention, the active metal particles and the sacrificial metal particles may not form an alloy with each other.

[0018] In the composite according to the present invention, the active metal particles may include one or more metals selected from the group consisting of palladium (Pd); platinum (Pt); gold (Au); ruthenium (Ru); rhodium (Rh); iridium (Ir); osmium (Os) and alloys thereof.

[0019] In the composite according to the present invention, the standard reduction potential of the metal included in the sacrificial metal particles may be lower than the standard reduction potential of the metal included in the active metal particles.

[0020] In the composite according to the present invention, the sacrificial metal particles may include one or more metals selected from the group consisting of: silver (Ag); palladium (Pd); iridium (Ir); ruthenium (Ru); rhodium (Rh); platinum (Pt); osmium (Os); iron (Fe); aluminum (Al) and alloys thereof.

[0021] In the composite body according to the present invention, the average particle size D of the active metal particles of the composite body after 30,000 cycles of the accelerated durability test is 2 The average particle size D of the active metal particles before the accelerated durability test 1 Ratio D 2 / D 1 It can be 3 or less.

[0022] In the composite body according to the present invention, an atomic ratio of the sacrificial metal included in the sacrificial metal particles to the active metal included in the active metal particles may be 1:0.1 to 1:50.

[0023] In the composite according to the present invention, the active metal included in the active metal particles includes platinum (Pt), and in the X-ray diffraction (XRD) energy spectrum of the composite and pure platinum (Pt), the difference in 2θ value of the maximum peak appearing in the range of 2θ=39.8±1.0° can be less than 0.3°.

[0024] In the composite according to the present invention, the active metal included in the active metal particles includes platinum (Pt). In the X-ray photoelectron spectroscopy (XPS) of the composite, the Pt 4f 7 / 2 In the XPS spectrum, the Pt(0) peak intensity I 0 Pt(II) peak intensity I II Ratio I 0 / I II It can be 1.8 or above.

[0025] The present invention provides a method for manufacturing a composite, which comprises the following steps: preparing a first reaction solution, wherein the first reaction solution is obtained by mixing a dispersion containing a carbon carrier loaded with active metal particles and a solution containing a sacrificial metal precursor; and synthesizing a composite in which the active metal particles and the sacrificial metal particles are independently loaded on the carbon carrier by adding a reducing agent to the first reaction solution.

[0026] The present invention provides another method for manufacturing a composite, which comprises the following steps: preparing a second reaction solution, wherein the second reaction solution is prepared by mixing a dispersion containing a carbon carrier loaded with active metal particles and a dispersion containing a carbon carrier loaded with sacrificial metal particles; and synthesizing a composite in which the sacrificial metal particles are independently loaded on the carbon carrier by adding a reducing agent to the second reaction solution.

[0027] The present invention provides a membrane electrode assembly, characterized in that the membrane electrode assembly comprises: a cathode, comprising a first catalyst layer and a first gas diffusion layer; an anode, comprising a second catalyst layer and a second gas diffusion layer; and a polymer electrolyte membrane, arranged between the cathode and the anode, wherein the first catalyst layer comprises active metal particles, and the first gas diffusion layer comprises: a support body for the first gas diffusion layer; and sacrificial metal particles, which are loaded on the support body for the first gas diffusion layer and are oxidized or reduced to replace the active metal particles.

[0028] In the membrane electrode assembly according to the present invention, a surface of the first gas diffusion support body on which the sacrificial metal particles are located may face a surface of the first catalyst layer.

[0029] In the membrane electrode assembly according to the present invention, the second catalyst layer may include active metal particles, and the second gas diffusion layer may include: a support for the second gas diffusion layer; and sacrificial metal particles, which are loaded on the support for the second gas diffusion layer and are oxidized or reduced to replace the active metal particles.

[0030] In the membrane electrode assembly according to the present invention, the active metal particles may include one or more metals selected from the group consisting of palladium (Pd); platinum (Pt); gold (Au); ruthenium (Ru); rhodium (Rh); iridium (Ir); osmium (Os) and alloys thereof.

[0031] In the membrane electrode assembly according to the present invention, the standard reduction potential of the metal included in the sacrificial metal particles may be lower than the standard reduction potential of the metal included in the active metal particles.

[0032] In the membrane electrode assembly according to the present invention, the sacrificial metal particles may include one or more metals selected from the group consisting of: silver (Ag); palladium (Pd); iridium (Ir); ruthenium (Ru); rhodium (Rh); platinum (Pt); osmium (Os); iron (Fe); aluminum (Al) and alloys thereof.

[0033] In the membrane electrode assembly according to the present invention, the average particle size D of the active metal particles after 30,000 cycles of the accelerated durability test is 2 The average particle size D of the active metal particles before the accelerated durability test 1 Ratio D 2 / D 1 It can be 3 or less.

[0034] In the membrane electrode assembly according to the present invention, an atomic ratio of the sacrificial metal included in the sacrificial metal particles included in the first gas diffusion layer to the active metal included in the active metal particles included in the first catalyst layer may be 0.1:1 to 100:1.

[0035] In the membrane electrode assembly according to the present invention, the active metal included in the active metal particles includes platinum (Pt), and in the Pt 4f XPS spectrum based on X-ray photoelectron spectroscopy (XPS), the Pt (II) peak intensity I of the first catalyst layer after 90,000 cycles of accelerated durability test is 2.347 W / cm2. 2 Compared with the Pt(II) peak intensity before the accelerated durability test 1 Ratio I 2 / I 1 It can be 0.5 or more.

[0036] In the membrane electrode assembly according to the present invention, the content of the sacrificial metal particles per unit area of ​​the first gas diffusion layer support may be 0.1 mg / cm 2 Up to 100mg / cm 2 .

[0037] The present invention provides a method for manufacturing a membrane electrode assembly, which comprises the following steps: a first step of doping a sacrificial metal precursor on a first gas diffusion support; a second step of reducing the sacrificial metal precursor doped on the first gas diffusion layer support to manufacture a first gas diffusion layer loaded with sacrificial metal particles on the first gas diffusion layer support; a third step of forming a first catalyst layer on one surface of a polymer electrolyte membrane; a fourth step of forming a second catalyst layer on the other surface of the polymer electrolyte membrane; a fifth step of forming the first gas diffusion layer on the first catalyst layer; and a sixth step of forming a second gas diffusion layer on the second catalyst layer.

[0038] The present invention provides an electrode for a fuel cell, wherein the electrode for a fuel cell comprises the above-mentioned composite.

[0039] The present invention provides a fuel cell, which comprises the above-mentioned membrane electrode assembly or the above-mentioned fuel cell electrode.

[0040] As active metal particles and sacrificial metal particles independently supported on a carbon support, the composite according to the present invention can suppress the degradation phenomenon of the active metal, thereby having significantly improved durability while maintaining excellent activity of the catalyst.

[0041] With active metal particles located on the carbon support and sacrificial metal particles located on the gas diffusion layer support, the membrane electrode assembly according to the present invention can have excellent catalyst activity and significantly improved durability for the same reasons as the above-mentioned composite.

[0042] The fuel cell according to the present invention can have high charge and discharge durability and life, etc. by including the above-mentioned composite body and / or membrane electrode assembly.

[0043] The method for producing a composite body and the method for producing a membrane electrode assembly according to the present invention can greatly improve the activity and durability of a catalyst in an electrode for a fuel cell through a simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a schematic diagram for explaining the influence of whether or not silver (Ag) particles are included on the ORR catalyst activity.

[0045] Figure 2 and Figure 3 is a schematic diagram of a method for manufacturing a composite body according to an implementation example.

[0046] Figure 4 It is a figure which shows the XRD patterns of Comparative Example 1 and Examples 1 to 3.

[0047] Figure 5 3 is a diagram showing XRD patterns of Comparative Example 1, Comparative Example 2, and Example 2.

[0048] Figure 6 Graphs showing Pt 4f XPS spectra of Comparative Example 1 and Examples 1 to 3.

[0049] Figure 7 3d XPS spectra of Comparative Example 1 and Examples 1 to 3 are shown.

[0050] Figure 8Graphs showing Pt 4f XPS spectra of Comparative Example 1, Comparative Example 2, and Example 2.

[0051] Fig. 9 3d XPS spectra of Comparative Example 2, Comparative Example 3, and Example 2.

[0052] Fig.10 is the HAADF-STEM image of Example 2 and the corresponding EDS mapping image, Fig.11 It is an image of an enlarged HAADF-STEM image of Example 2 and a corresponding EDS mapping image.

[0053] Fig.12 is the HAADF-STEM image of Comparative Example 2 and the corresponding EDS mapping image.

[0054] Fig.13 Graphs showing the evaluation results of the electrochemical performance of Comparative Example 1 and Examples 1 to 3.

[0055] Fig.14 : is a graph which shows the CV curves before and after ADT of each of Comparative Example 1 and Examples 1 to 3.

[0056] Fig.15 The transmission electron microscope (TEM, FEITecnai G2 twin) images of Comparative Example 1 and Example 2 before and after ADT.

[0057] Fig.16 It is a graph showing the evaluation results of the electrochemical performance of Comparative Example 2 which is an alloy form.

[0058] Fig.17 and Fig.18 : is a graph showing the performance before and after ADT performed during 30k cycles of a fuel cell using Comparative Example 1 and each of Examples 1 to 3 as a cathode catalyst.

[0059] Fig.19 It is a graph showing polarization curves and power density curves before and after ADT of a fuel cell using Comparative Example 2 in an alloy form as a cathode catalyst.

[0060] Fig. 20 It is a graph showing the change in particle size of the fuel cells of Comparative Example 1 and Example 2 before and after ADT.

[0061] Figure 21 to Figure 23 : is a graph showing the results of online ICP-MS experiments performed on Comparative Example 1 and Example 2.

[0062] Figure 24 to Figure 26: is a graph showing the results of the online ICP-MS experiment performed in the above-mentioned manner for Comparative Examples 1 and 2.

[0063] Fig. 27 The results are shown for Comparative Example 1 (or Comparative Example 3), Comparative Example 2, Example 2, Pt foil (or Ag foil) and PtO 2 (or AgO 2 ) of Pt L 3 -edge (or Ag K-edge) ex situ XAS spectrum.

[0064] Fig.28 The Pt L of Comparative Example 1, Example 2 and Comparative Example 2 is shown. 3 -Figure 1. In situ XAS spectrum of the edge.

[0065] Fig.29 It is shown based on Fig.28 Graph showing the oxidation state of platinum according to the applied potential for Comparative Example 1, Example 2, and Comparative Example 2 calculated based on the results of .

[0066] Fig.30 is a diagram showing a schematic diagram of a membrane electrode assembly according to an implementation example.

[0067] Fig.31 is a diagram showing the operating principle of a fuel cell containing sacrificial metal particles.

[0068] Fig.32 This is a diagram schematically showing a process for manufacturing a first gas diffusion layer in which sacrificial metal particles are supported on a first gas diffusion layer support.

[0069] Fig.33 The diagram shows scanning electron microscope (SEM) images of the gas diffusion layers of Comparative Example 4 and Example 4.

[0070] Fig.34 : is a figure which shows the SEM image of the gas diffusion layer of Comparative Example 4 and the corresponding energy dispersive X-ray spectroscopy (EDS: energy dispersive X-ray spectroscopy) mapping image, Fig.35 : is a figure which shows the SEM image of the gas diffusion layer of Example 4 and the corresponding EDS mapping image.

[0071] Fig.36 (a) is a diagram showing X-ray diffraction (XRD) patterns of the gas diffusion layers of Comparative Example 4 and Example 4, Fig.36(b) is a diagram showing Ag 3d XPS spectra of the gas diffusion layers of Comparative Example 4 and Example 4 by X-ray photoelectron spectroscopy (XPS).

[0072] Fig.37 Graphs showing polarization curves according to accelerated durability test (ADT: Accelerated durability test) cycles using the fuel cells of Example 5 and Comparative Example 5.

[0073] Fig.38 Graphs showing the results of electrochemical impedance spectroscopy (EIS) measurement based on the ADT cycle using the fuel cells of Example 5 and Comparative Example 5.

[0074] Fig.39 Graphs showing cyclic voltammetry (CV) curves according to ADT cycles using the fuel cells of Example 5 and Comparative Example 5.

[0075] Fig.40 : is a graph showing Pt 4f XPS spectra measured for the cathode catalyst layers included in the membrane electrode assemblies manufactured in Comparative Example 5 and Example 5 before and after performing ADT.

[0076] Fig.41 (a) is a diagram showing an XRD pattern according to an ADT cycle of a gas diffusion layer included in a membrane electrode assembly manufactured in Example 5, Fig.41 (b) is a diagram showing the Ag 3d XPS spectrum.

[0077] Fig.42 1 is a diagram showing transmission electron microscope (TEM) images of the catalyst layers included in Comparative Example 5 and Example 5 according to the ADT cycle.

[0078] Fig.43 are graphs showing a high angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of the catalyst layer included in Example 5 after 90,000 (90k) cycles, a corresponding EDS mapping image, and an EDS spectrum.

[0079] Fig.44 is a graph of the Ag 3d XPS spectrum according to the ADT cycle of the catalyst layer included in Example 5.

[0080] Description of Reference Numerals

[0081] 10: First gas diffusion layer

[0082] 20: First catalyst layer

[0083] 30: Polymer electrolyte membrane

[0084] 1: Support for the first gas diffusion layer

[0085] 2: Sacrificial metal particles DETAILED DESCRIPTION

[0086] The implementation forms described in this specification can be transformed into various other forms, and the technology according to an implementation example is not limited to the implementation forms described below. In addition, the implementation form of an implementation example is provided to more completely explain the present disclosure to persons with average knowledge in the technical field. At this time, unless otherwise defined, the technical terms and scientific terms used have the meanings commonly understood by persons with ordinary knowledge in the technical field to which the present invention belongs, and in the following description and drawings, the description of the known functions and structures that may unnecessarily obscure the main purpose of the present invention will be omitted.

[0087] Furthermore, unless the context indicates otherwise, singular forms used in the specification and the appended claims may be intended to include plural forms.

[0088] Furthermore, in this specification and the appended claims, terms such as “including” or “having” refer to the existence of features or constituent elements recorded in the specification, and do not preclude the possibility of adding one or more other features or constituent elements unless otherwise specified.

[0089] Furthermore, the numerical ranges used in this specification include lower and upper limits and all values ​​within the range, increments logically derived from the form and amplitude of the defined range, all values ​​that are doubly defined, and all possible combinations of upper and lower limits of the numerical range defined in different forms from each other.

[0090] Furthermore, in the description of the present invention, unless otherwise defined, values ​​outside the numerical range that may occur due to experimental errors or rounding of values ​​are also included in the defined numerical range.

[0091] Furthermore, the terms "about", "substantially", etc., used in this specification and the appended claims, with respect to degree, are used in the sense of their numerical values ​​or close to their numerical values ​​when the manufacturing and material tolerances inherent in the referenced meanings are proposed. In order to assist in the understanding of this specification and the appended claims, the disclosure of the exact or absolute numerical values ​​will be referred to to prevent improper use by unscrupulous infringers.

[0092] Furthermore, throughout the specification, “comprising” a certain constituent element means that other constituent elements are not excluded but may be included unless otherwise stated.

[0093] Furthermore, in this specification, when a layer, film, region, plate or the like is mentioned as being “above” or “over” another part, this not only includes the situation where it is “immediately above” another part, but also includes the situation where there are other parts between the two.

[0094] Furthermore, the terms "first", "second", etc. used in this specification can be used to describe various components, but the components should not be limited to the terms. The terms are used only to distinguish one component from another component.

[0095] Hereinafter, the composite, the method for producing the composite, the membrane electrode assembly, the method for producing the membrane electrode assembly, the electrode, and the different fuel cells of the present invention will be described in detail.

[0096] The present invention provides a composite, characterized in that the composite comprises: a carbon carrier; active metal particles; and sacrificial metal particles, which are oxidized or reduced to replace the active metal particles, wherein the active metal particles and the sacrificial metal particles are independently loaded on the carbon carrier.

[0097] According to an implementation example, the above-mentioned active metal particles and sacrificial metal particles are independently loaded on the carbon carrier, which may refer to a situation where the active metal particles and the sacrificial metal particles are arranged in a physically separated manner.

[0098] As the composite includes active metal particles and sacrificial metal particles independently supported on a carbon carrier, the composite can effectively inhibit the degradation of the active metal, thereby maintaining the excellent catalytic activity of the precious metal-based catalyst while also having significantly improved durability compared to existing precious metal-based catalysts.

[0099] Specifically, as the composite according to the present invention includes sacrificial metal particles that are oxidized earlier than active metal particles, the oxidation of the active metal can be effectively suppressed, thereby solving the problem of degradation of the active metal particles that causes the reduction of catalyst activity and durability. In addition, since the sacrificial metal particles and the active metal particles exist independently, the sacrificial metal particles do not block the catalyst active sites of the active metal included in the active metal particles, thereby having the advantage of maintaining the excellent catalyst activity of the pure active metal catalyst.

[0100] According to an implementation example, the active metal particles and the sacrificial metal particles may not form an alloy with each other. The active metal particles and the sacrificial metal particles are independently loaded in the sense that even if the active metal particles and the sacrificial metal particles are in physical contact with each other, the active metal included in the active metal particles and the sacrificial metal included in the sacrificial metal particles do not form an alloy and are not chemically combined. In the case where the active metal particles and the sacrificial metal particles form an alloy with each other, the sacrificial metal particles block the catalytic active sites of the active metal particles, which may reduce the catalytic activity. On the contrary, in the case where the active metal particles and the sacrificial metal particles do not form an alloy with each other and exist independently, the sacrificial metal particles do not block the catalytic active sites of the active metal included in the active metal particles, so that the catalytic activity can be excellent.

[0101] According to an implementation example, the standard reduction potential of the metal included in the sacrificial metal particles (i.e., the sacrificial metal) may be lower than the standard reduction potential of the metal included in the active metal particles (i.e., the active metal). The active metal included in the active metal particles can be any metal that has catalytic activity and a standard reduction potential higher than that of the sacrificial metal included in the sacrificial metal particles.

[0102] According to an implementation example, the standard reduction potential of the active metal included in the active metal particles may be greater than 0.7 V, greater than 0.8 V, greater than 0.9 V, or greater than 1.0 V, and the upper limit may be less than 3.0 V, less than 2.5 V, 2.0 V, or less than 1.5 V. Specifically, the standard reduction potential of the active metal included in the active metal particles may be 0.7 V to 3.0 V, 0.8 V to 2.5 V, 0.9 V to 2.0 V, or 1.0 V to 1.5 V.

[0103] According to an implementation example, the standard reduction potential of the sacrificial metal included in the sacrificial metal particles may be above 0.3 V, above 0.4 V, above 0.5 V or above 0.6 V, and the upper limit may be below 1.1 V, below 1.0 V, below 0.9 V or below 0.8 V. Specifically, the standard reduction potential of the sacrificial metal included in the sacrificial metal particles may be 0.3 V to 1.1 V, 0.4 V to 1.0 V, 0.5 V to 0.9 V or 0.6 V to 0.8 V. The sacrificial metal included in the sacrificial metal particles may have a standard reduction potential within the above range, and may have a value less than the standard reduction potential of the active metal included in the active metal particles.

[0104] According to an implementation example, the active metal particles may include one or more metals selected from the group consisting of palladium (Pd); platinum (Pt); gold (Au); ruthenium (Ru); rhodium (Rh); iridium (Ir); osmium (Os) and alloys thereof. The metal included in the active metal particles can be appropriately selected from the above metals to have the above effects, but the active metal included in the active metal particles included in the composite of the present invention is not limited to the above metals, and the active metal included in the active metal particles and the sacrificial metal included in the sacrificial metal particles can be appropriately selected to have the above effects.

[0105] Furthermore, according to an implementation example, the sacrificial metal particles may include one or more metals selected from the group consisting of: silver (Ag); palladium (Pd); iridium (Ir); ruthenium (Ru); rhodium (Rh); platinum (Pt); osmium (Os); iron (Fe); aluminum (Al) and alloys thereof. As a non-limiting example of the alloy included in the sacrificial metal particles, the alloy included in the sacrificial metal particles may include zinc-silver alloy (AgZn), tin-silver alloy (AgSn), antimony-silver alloy (AgSb), indium-silver alloy (AgIn), chromium-iron alloy (FeCr), molybdenum-iron alloy (FeMo), manganese-iron alloy (FeMn), tungsten-iron alloy (FeW), nickel-iron alloy (FeNi) or nickel-chromium-iron alloy (FeCrNi), but the present invention is not limited thereto.

[0106] The metal included in the sacrificial metal particles can be appropriately selected from the above-mentioned metals to have the above-mentioned effects, but the sacrificial metal included in the sacrificial metal particles included in the composite of the present invention is not limited to the above-mentioned metals, and the sacrificial metal included in the sacrificial metal particles and the active metal included in the active metal particles can be appropriately selected respectively to have the above-mentioned effects.

[0107] As a non-limiting and advantageous example, the active metal may include platinum (Pt), and the sacrificial metal may include silver (Ag), so that the silver may inhibit oxidation of the platinum.

[0108] According to an implementation example, the active metal may include platinum (Pt), and the difference between the 2θ value of the maximum peak appearing in the range of 2θ=39.8±1.0° in the X-ray diffraction (XRD) spectrum of the composite and the 2θ value of the maximum peak appearing in the range of 2θ=39.8±1.0° in the X-ray diffraction (XRD) spectrum of pure platinum (Pt) may be 0.3° or less. The difference in the 2θ value may be 0.3° or less or 0.2° or less, more specifically 0.1° or less, and the lower limit may be 0°, 0.01° or 0.05°. Specifically, the difference in the 2θ value may be 0.05° to 0.3°, 0.01° to 0.3° or 0° to 0.1°. Since the platinum (Pt) particles as active metal particles and the sacrificial metal particles do not form an alloy with each other, the composite satisfying the above-mentioned difference in 2θ value may have the advantage of excellent catalyst activity. As a non-limiting and advantageous example, the composite may have a maximum peak within the range of 2θ=39.8±0.2° in an X-ray diffraction (XRD) spectrum.

[0109] According to an implementation example, the active metal may include platinum (Pt), and the composite may be subjected to X-ray photoelectron spectroscopy (XPS) based on Pt 4f 7 / 2 In the XPS spectrum, the Pt(0) peak intensity I 0 Pt(II) peak intensity I II Ratio I 0 / I II It may be 1.8 or more, preferably 2.0 or more, more preferably 2.2 or more, and the upper limit may be 3.5 or 3.0. Since the ratio of the metallic platinum component in the platinum included in the composite is high, the composite satisfying the peak ratio within the above range can more effectively suppress the deterioration of platinum, thereby having more excellent catalyst activity and durability.

[0110] According to one implementation example, the active metal may include platinum (Pt), and the composite may have a peak in the range of 11567.2±0.2 eV in the X-ray absorption near-edge structure (XANES) energy spectrum. Since the ratio of the metallic platinum component in the platinum included in the composite is high, the composite having a peak satisfying the above range can more effectively inhibit the degradation of platinum, thereby having better catalytic activity and durability.

[0111] According to an implementation example, the atomic ratio of the sacrificial metal to the active metal included in the composite can be 1:0.1 to 1:50, specifically 1:0.5 to 1:15, more specifically 1:1 to 1:10, and more specifically 1:2 to 1:8 or 1:3 to 1:8. Since the ratio of the sacrificial metal to the active metal is selected within the above range, the composite can have significantly improved durability while maintaining excellent catalytic activity. In the case where the sacrificial metal included in the composite is excessively included in a ratio above the above range, the activity of the catalyst may be reduced. In addition, in the case where the sacrificial metal included in the composite is included in a ratio below the above range, the effect of the sacrificial metal replacing the active metal to be oxidized or reduced is reduced, thereby possibly reducing the durability of the composite. As an advantageous example, within the above range, since the total number of atoms of the sacrificial metal is greater than the total number of atoms of the active metal, the sacrificial metal replaces the active metal to be oxidized or reduced, thereby improving the durability of the composite.

[0112] According to an implementation example, the active metal particles and the sacrificial metal particles may have one or more shapes selected from the group consisting of spherical, angular, linear and amorphous, but the present invention is not particularly limited to the shapes of the active metal particles and the sacrificial metal particles.

[0113] According to one implementation example, the average particle size of the active metal particles and / or the sacrificial metal particles can be 0.1nm to 20nm, specifically 1nm to 10nm, and more specifically 1nm to 5nm, but the composite according to the present invention is not necessarily limited to the average particle size of the above-mentioned active metal particles and / or the above-mentioned sacrificial metal particles.

[0114] According to an implementation example, the average particle size D of the active metal particles of the composite after the cyclic accelerated durability test (ADT) is 2 The average particle size D of the active metal particles before the accelerated durability test 1 Ratio D 2 / D 1 It can be less than 3. Specifically, the D 2 / D 1 The ratio of D may be 0.5 or more, 1 or more, or 1.5 or more, and the upper limit may be 4 or less, 3 or less, or 2.5 or less. 2 / D 1The ratio may be 0.5 to 4, 1 to 3, or 1.5 to 2.5. The composite satisfying the above average particle diameter ratio may have more significantly improved catalyst activity and durability because the degradation phenomenon of the active metal is more suppressed due to the sacrificial metal.

[0115] The execution conditions of the accelerated durability test (ADT) can use the conditions proposed by the U.S. Department of Energy (DOE), specifically, the accelerated durability test can be performed at 80°C and atmospheric pressure, pure hydrogen with a relative humidity of 100% can be supplied to the anode at a flow rate of 100sccm and pure nitrogen with a relative humidity of 100% can be supplied to the cathode at a flow rate of 50sccm, and one cycle of the ADT can consist of a 3-second holding interval at 0.6V, a 0.5-second rising interval, and a 3-second holding interval at 0.95V.

[0116] According to an implementation example, as long as it is a carbon carrier including carbon with excellent chemical stability and conductivity known in the art, the carbon carrier included in the composite can be used without limitation. As a non-limiting example, the carbon carrier can be selected from Vulcan carbon, carbon paper, carbon filter, carbon fiber, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, Timcal, and one or more carbon doped with other heterogeneous elements, but the present invention is not particularly limited thereto.

[0117] According to an implementation example, based on the total weight of the composite, the content of the active metal particles loaded on the carbon carrier may be 1 to 40 weight percent, specifically 4 to 30 weight percent, and more specifically 5 to 24 weight percent.

[0118] According to an implementation example, based on the total weight of the composite, the content of the sacrificial metal particles loaded on the carbon carrier may be 0.5 to 20 weight percent, specifically 2 to 15 weight percent, and more specifically 2.5 to 12 weight percent.

[0119] According to an implementation example, the composite can be a catalyst for oxygen reduction reaction (ORR: Oxygen Reduction Reaction). As described above, the composite includes a carbon carrier, active metal particles and sacrificial metal particles, wherein the composite in which the active metal particles and the sacrificial metal particles are independently loaded on the carbon carrier can be used as a catalyst having excellent activity in oxygen reduction reaction and significantly excellent stability compared with existing pure active metal catalysts.

[0120] Figure 1 As a more specific implementation example, this is a schematic diagram for explaining the effect of whether or not silver (Ag) particles are included as sacrificial metal particles on the activity of an oxygen reduction reaction (ORR) catalyst. Figure 1 In pure platinum catalyst (Pt / C), platinum (Pt) particles are oxidized to produce Pt-O in an anodic potential scan, and Pt-O can be reduced to return to Pt in a cathodic potential scan. 0 However, due to the failure of some Pt-O reduction, platinum is present in ionic form (Pt 2+ ) exists, which may cause the dissolution of platinum and the deterioration of platinum. In contrast, since silver (Ag) particles having a lower standard reduction potential than platinum are oxidized before platinum, the composite according to the present invention (in Figure 1 The composite of the present invention generates significantly less Pt-O than a pure platinum catalyst, thereby greatly reducing the degradation of platinum, and the electron-rich platinum in the cathode potential can polarize oxygen molecules into oxygen atoms, thereby achieving a more stable oxygen reduction reaction (ORR) performance.

[0121] The present invention provides a fuel cell electrode including the above-mentioned composite. Furthermore, the present invention provides a fuel cell including the fuel cell electrode. The fuel cell according to the present invention can be equipped with an anode that generates hydrogen ions and electrons by oxidation of a fuel substance, a cathode that generates oxygen reduction by reaction with hydrogen ions and electrons, and an electrolyte layer (membrane) that can effectively transfer hydrogen ions from the anode to the cathode, wherein the cathode includes the composite according to the present invention, and thus has the advantage of being able to improve not only the efficiency of the fuel cell but also the stability.

[0122] According to an implementation example, the fuel cell can be a proton exchange membrane fuel cell (PEMFC: ProtonExchange Membrane Fuel Cell), a direct methanol fuel cell (DMFC: DirectMethanol Fuel Cell) using alcohol as fuel, a direct ethanol fuel cell (DEFC: Direct Ethanol Fuel Cell), an alkaline fuel cell (AFC: Alkaline Fuel Cell), a phosphoric acid fuel cell (PAFC: Phosphoric Acid Fuel Cell), a molten carbonate fuel cell (MCFC: Molten Carbonate Fuel Cell) and a solid oxide fuel cell (SOFC: Solid Oxide Fuel Cell), etc., but the present invention is not particularly limited to the type of fuel cell.

[0123] According to an implementation example, the fuel cell may be a proton exchange membrane fuel cell (PEMFC) that operates at low temperatures and can be used in transportation vehicles, and the proton exchange membrane fuel cell may include a first gas diffusion layer, an anode, a polymer electrolyte membrane, a cathode, and a second gas diffusion layer. 2 ) can be supplied to the anode through the first gas diffusion layer, the supplied hydrogen is oxidized at the anode to generate hydrogen ions, and the generated hydrogen ions can be transferred to the cathode through the polymer electrolyte membrane. The hydrogen ions can react with the oxygen supplied to the cathode through the second gas diffusion layer as described above on the cathode to generate water. At this time, in the composite according to the present invention included in the cathode, the catalyst activity for oxygen reduction reaction (ORR) is excellent and the durability can be significantly excellent, so the stability of the fuel cell can be improved.

[0124] According to an implementation example, the first gas diffusion layer and the second gas diffusion layer may be smoothly supplied with the supplied fuel material or air and / or oxygen, and may include a conductive material known in the art, but the present invention is not limited thereto.

[0125] According to an implementation example, the energy density reduction rate of the fuel cell after 30,000 cycles of accelerated durability test (ADT) may be 40% or less, 30% or less, 25% or less, or 20% or less, and the lower limit may be 1% or more, 5% or more, 10% or more, or 15% or more. Specifically, the energy density reduction rate of the fuel cell after performing 30,000 cycles of accelerated durability test may be 1% to 40%, 5% to 30%, 10% to 25%, or 15% to 20%. Since the fuel cell includes the above-mentioned composite, a high energy density can be maintained even after more than 30,000 cycles of accelerated durability test.

[0126] According to an implementation example, the execution conditions of the 30,000-cycle accelerated durability test (ADT) can use the conditions proposed by the U.S. Department of Energy (DOE), specifically, the accelerated durability test can be performed at 80°C and ambient pressure, pure hydrogen with a relative humidity of 100% can be supplied to the anode at a flow rate of 100sccm and pure nitrogen with a relative humidity of 100% can be supplied to the cathode at a flow rate of 50sccm, and one cycle of the accelerated durability test can consist of a 3-second holding interval at 0.6V, a 0.5-second rising interval, and a 3-second holding interval at 1.0V.

[0127] The present invention provides a method for manufacturing a composite, which comprises the following steps: preparing a first reaction solution, wherein the first reaction solution is obtained by mixing a dispersion containing a carbon carrier loaded with active metal particles and a solution containing a sacrificial metal precursor; and synthesizing a composite in which the active metal particles and the sacrificial metal particles are independently loaded on the carbon carrier by adding a reducing agent to the first reaction solution.

[0128] The present invention provides another method for manufacturing a composite, which comprises the following steps: preparing a second reaction solution, wherein the second reaction solution is prepared by mixing a dispersion containing a carbon carrier loaded with active metal particles and a dispersion containing a carbon carrier loaded with sacrificial metal particles; and synthesizing a composite in which the sacrificial metal particles are independently loaded on the carbon carrier by adding a reducing agent to the second reaction solution.

[0129] In the respective descriptions of the manufacturing methods of the composites according to the present invention, as the carbon carrier, active metal particles, sacrificial metal particles, etc. are the same or similar to those described in the previous composites, the manufacturing method of the composites according to the present invention includes all the contents described in the previous composites.

[0130] Hereinafter, the method for producing a composite body according to the present invention will be described in detail. The method for producing a composite body and another method for producing a composite body will be collectively referred to as a method for producing a composite body.

[0131] Figure 2 and Figure 3 Schematic diagram of a method for manufacturing a composite body according to an embodiment of the present invention. Figure 2 and Figure 3 , the method for manufacturing the composite according to the present invention is described, but this is only used to help understand the present invention, and the present invention is not limited to the drawings.

[0132] Reference Figure 2 According to a method for manufacturing a composite body of an implementation example, a composite body in which active metal particles and sacrificial metal particles are independently loaded on a carbon carrier can be manufactured in a simple manner. The composite body manufactured by the above-mentioned method for manufacturing a composite body can effectively inhibit the degradation of the active metal, thereby maintaining the excellent catalytic activity of the precious metal-based catalyst while also having significantly improved durability compared to existing precious metal-based catalysts.

[0133] According to an implementation example, in the step of preparing the first reaction solution, 0.5 to 20 parts by weight of a sacrificial metal precursor can be used relative to 100 parts by weight of the carbon carrier loaded with the active metal particles, specifically 2 to 15 parts by weight of a sacrificial metal precursor can be used, and more specifically 2.5 to 12 parts by weight of a sacrificial metal precursor can be used.

[0134] According to an implementation example, the dispersion liquid in the step of preparing the first reaction solution, the solution containing the sacrificial metal precursor, and the dispersion solvent including the same can respectively use one or more solvents selected from the group consisting of: water, isopropanol, toluene, ethanol, n-propanol, n-butylacetate, ethylene glycol, butyl carbitol, and butyl carbitol acetate. However, the present invention is not limited to the solvents, and an appropriate solvent can be selected according to the carbon carrier loaded with the active metal particles and the types of chemicals included in the sacrificial metal precursor.

[0135] According to an implementation example, the sacrificial metal precursor may be a chloride, iodide, sulfide, fluoride, hydroxide, carbonate and / or nitrate of a metal having a standard reduction potential lower than that of the active metal included in the active metal particles. As a non-limiting example, since the sacrificial metal may be silver (Ag), the sacrificial metal precursor may be silver nitrate (AgNO 3 ).

[0136] According to an embodiment, the reducing agent in the step of synthesizing the composite can be one or more reducing agents selected from the group consisting of sodium hydride (NaH), sodium borohydride (NaBH 4 ), lithium aluminum hydride (LiAlH 4 ), hydrazine (N 2 H 4 ), diisobutylaluminum hydride (DIBAH) and potassium triethylborohydride (KEt 3 BH).

[0137] Reference Figure 3 In another method for manufacturing a composite according to an implementation example, in the step of preparing the second reaction solution, all or part of the active metal and / or sacrificial metal included in the carbon carrier loaded with the active metal particles and the carbon carrier loaded with the sacrificial metal particles may be in a state of incomplete reduction reaction.

[0138] In the step of synthesizing the composite according to an implementation example, the reduction reaction using the reducing agent may be performed at 25° C. to 200° C., but the present invention is not particularly limited thereto.

[0139] Matters concerning the dispersion solvent and the reducing agent included in still another method for producing a composite body according to an implementation example are the same as those included in the above-mentioned method for producing a composite body, and thus a detailed description thereof will be omitted.

[0140] According to an implementation example, a third method for manufacturing the composite body may be provided. The third method may include the following steps: manufacturing a mixture by mixing a carbon carrier loaded with active metal particles and a carbon carrier loaded with sacrificial metal particles; and synthesizing a composite body in which active metal particles and sacrificial metal particles are independently loaded on the carbon carrier by heating the mixture.

[0141] According to an implementation example, in the third method for manufacturing the composite body, the temperature at which the mixture is heated may be 100° C. or more, 150° C. or more, or 200° C. or more, and the upper limit may be 600° C. or less, 500° C. or less, or 400° C. or less. Specifically, the temperature at which the mixture is heated may be 100° C. to 600° C., 150° C. to 500° C., or 200° C. to 400° C.

[0142] According to one implementation example, the step of synthesizing a composite body in which active metal particles and sacrificial metal particles are independently loaded on a carbon carrier by heating the mixture can be performed under a mixed gas atmosphere of one or more selected from the group consisting of: inert gases such as nitrogen, helium and argon; hydrogen and ammonia.

[0143] The third method for manufacturing the composite can manufacture a composite in which active metal particles and sacrificial metal particles are independently supported on a carbon carrier in the same simple manner as the method for manufacturing the composite, and the composite manufactured by the above manufacturing method can effectively suppress the deterioration of the active metal, so that the composite can maintain the excellent catalytic activity of the precious metal catalyst while also having significantly improved durability compared to existing precious metal catalysts. The active metal can be selected from one or more of the following groups: palladium (Pd); platinum (Pt); gold (Au); ruthenium (Ru); rhodium (Rh); iridium (Ir); osmium (Os); and alloys thereof, and the sacrificial metal can be selected from metals having a standard reduction potential lower than that of the selected active metal.

[0144] The present invention provides a membrane electrode assembly, characterized in that the membrane electrode assembly comprises: a cathode, comprising a first catalyst layer and a first gas diffusion layer; an anode, comprising a second catalyst layer and a second gas diffusion layer; and a polymer electrolyte membrane, arranged between the cathode and the anode, wherein the first catalyst layer comprises active metal particles, and the first gas diffusion layer comprises: a support body for the first gas diffusion layer; and sacrificial metal particles, which are loaded on the support body for the first gas diffusion layer and are oxidized or reduced to replace the active metal particles.

[0145] In explaining the membrane electrode assembly according to the present invention, as the active metal particles and the sacrificial metal particles and the like are the same or similar to those described in the previous composite, the membrane electrode assembly according to the present invention includes all the contents described in the previous composite.

[0146] Hereinafter, the membrane electrode assembly of the present invention will be described in more detail.

[0147] In a membrane electrode assembly according to an implementation example, since the gas diffusion layer for the cathode (i.e., the first gas diffusion layer) includes the sacrificial metal particles, the degradation of the active metal included in the catalyst layer for the cathode (i.e., the first catalyst layer) can be effectively suppressed, so that the membrane electrode assembly can have significantly improved durability compared with the existing membrane electrode assembly that does not include sacrificial metal particles.

[0148] Fig.30 1 is a diagram showing a schematic diagram of a membrane electrode assembly according to an implementation example of the present invention. Specifically, the membrane electrode assembly according to an implementation example may have a structure in which a first gas diffusion layer 10, a first catalyst layer 20, a polymer electrolyte membrane 30, a second catalyst layer (or a catalyst layer for an anode, not shown), and a second gas diffusion layer (or a gas diffusion layer for an anode, not shown) are stacked in sequence.

[0149] Fig.31 is a diagram showing the working principle of a fuel cell containing sacrificial metal particles. Specifically, Fig.31 (a) is a diagram showing the case where a gas diffusion layer not including sacrificial metal particles 2 is used, and degradation of active metal particles occurs as the fuel cell is driven. Fig.31(b) is a diagram showing the case of using a gas diffusion layer 10 including sacrificial metal particles 2. As the fuel cell is driven, the sacrificial metal particles 2 are oxidized before the active metal particles, thereby effectively suppressing the oxidation of the active metal particles, and thus solving the degradation problem of the active metal particles. Accordingly, the life of the catalyst activity can be significantly extended, so that the performance of the fuel cell using it can be maintained for a long time. In addition, the present invention is different from the prior art that covers the catalytic active sites of the active metal by coating the surface of the active metal particles in order to suppress the degradation phenomenon. The degradation problem of the active metal is solved by including sacrificial metal particles 2 on the first gas diffusion layer support 1. Since the sacrificial metal particles 2 do not block the catalytic active sites of the active metal, it has the advantage of maintaining the excellent catalytic activity of the catalyst. That is, the membrane electrode assembly of the present invention can have excellent catalytic activity while also having significantly improved durability.

[0150] According to an implementation example, a surface of the first gas diffusion support body where the sacrificial metal particles are located may face a surface of the first catalyst layer. Specifically, the sacrificial metal particles included in the first gas diffusion layer support body may be arranged to directly contact a surface of the first catalyst layer. Therefore, the sacrificial metal particles included in the first gas diffusion layer support body may more effectively inhibit the oxidation of the active metal particles included in the first catalyst layer.

[0151] According to an implementation example, the second catalyst layer and the second gas diffusion layer included in the anode may include widely known materials for forming the anode in the art. As an example, the anode may include: a second catalyst layer including the active metal particles; and a second gas diffusion layer including a support for the second gas diffusion layer. That is, the support for the second gas diffusion layer may not include sacrificial metal particles.

[0152] According to an implementation example, the second catalyst layer includes active metal particles, and the second gas diffusion layer may include: a support for the second gas diffusion layer; and sacrificial metal particles, which are loaded on the support for the second gas diffusion layer and oxidized or reduced to replace the active metal particles. Specifically, the second catalyst layer includes active metal particles, and the second gas diffusion layer includes: a support for the second gas diffusion layer; and sacrificial metal particles, which are loaded on the support for the second gas diffusion layer and oxidized or reduced to replace the active metal particles. Furthermore, in the case where the second gas diffusion layer includes the sacrificial metal particles, a surface of the support for the second gas diffusion layer where the sacrificial metal particles are located may face a surface of the second catalyst layer.

[0153] According to an implementation example, the active metal particles included in the second catalyst layer and the active metal particles included in the first catalyst layer may have different compositions from each other. Furthermore, the sacrificial metal particles loaded on the first gas diffusion layer support and the sacrificial metal particles loaded on the second gas diffusion layer support may also have different compositions from each other. As a non-limiting example, in a membrane electrode assembly according to an implementation example of the present invention, the active metal particles included in the first catalyst layer may include palladium (Pd), the active metal particles included in the second catalyst layer may include platinum (Pt), and the sacrificial metal particles included in the first gas diffusion layer may include silver (Ag), and the sacrificial metal particles included in the second gas diffusion layer may include aluminum (Al).

[0154] According to an implementation example, the standard reduction potential of the metal included in the sacrificial metal particles (i.e., the sacrificial metal) may be lower than the standard reduction potential of the metal included in the active metal particles (i.e., the active metal). The active metal included in the active metal particles can be any metal that has catalytic activity and a standard reduction potential higher than that of the sacrificial metal included in the sacrificial metal particles.

[0155] According to an implementation example, the standard reduction potential of the active metal included in the active metal particles may be greater than 0.7 V, greater than 0.8 V, greater than 0.9 V, or greater than 1.0 V, and the upper limit may be less than 3.0 V, less than 2.5 V, less than 2.0 V, or less than 1.5 V. Specifically, the standard reduction potential of the active metal included in the active metal particles may be 0.7 V to 3.0 V, 0.8 V to 2.5 V, 0.9 V to 2.0 V, or 1.0 V to 1.5 V.

[0156] According to an implementation example, the standard reduction potential of the sacrificial metal included in the sacrificial metal particles may be above 0.3 V, above 0.4 V, above 0.5 V or above 0.6 V, and the upper limit may be below 1.1 V, below 1.0 V, below 0.9 V or below 0.8 V. Specifically, the standard reduction potential of the sacrificial metal included in the sacrificial metal particles may be 0.3 V to 1.1 V, 0.4 V to 1.0 V, 0.5 V to 0.9 V or 0.6 V to 0.8 V. The sacrificial metal included in the sacrificial metal particles may have a standard reduction potential within the above range and may also have a value less than the standard reduction potential of the active metal included in the active metal particles.

[0157] According to an implementation example, the active metal particles may include one or more metals selected from the group consisting of palladium (Pd); platinum (Pt); gold (Au); ruthenium (Ru); rhodium (Rh); iridium (Ir); osmium (Os) and alloys thereof. The metal included in the active metal particles can be appropriately selected from the above metals to have the above effects, but the active metal included in the active metal particles included in the membrane electrode assembly of the present invention is not limited to the above metals, and the active metal included in the active metal particles and the sacrificial metal included in the sacrificial metal particles can have the above effects as long as they are appropriately selected respectively.

[0158] Furthermore, according to an implementation example, the sacrificial metal particles may include one or more metals selected from the group consisting of: silver (Ag); palladium (Pd); iridium (Ir); ruthenium (Ru); rhodium (Rh); platinum (Pt); osmium (Os); iron (Fe); aluminum (Al) and alloys thereof. As a non-limiting example of the alloy included in the sacrificial metal particles, the alloy may be zinc-silver alloy (AgZn), tin-silver alloy (AgSn), antimony-silver alloy (AgSb), indium-silver alloy (AgIn), chromium-iron alloy (FeCr), molybdenum-iron alloy (FeMo), manganese-iron alloy (FeMn), tungsten-iron alloy (FeW), nickel-iron alloy (FeNi) or nickel-chromium-iron alloy (FeCrNi), but the present invention is not limited thereto.

[0159] The metal included in the sacrificial metal particles can be appropriately selected from the above-mentioned metals to have the above-mentioned effects, but the sacrificial metal included in the sacrificial metal particles included in the membrane electrode assembly of the present invention is not limited to the above-mentioned metals, and the sacrificial metal included in the sacrificial metal particles and the active metal included in the active metal particles only need to be appropriately selected respectively to have the above-mentioned effects.

[0160] As a non-limiting and advantageous example, the active metal may include platinum (Pt), and the sacrificial metal may include silver (Ag), so that the silver may inhibit oxidation of the platinum.

[0161] According to one implementation example, the active metal particles and / or the sacrificial metal particles may have one or more shapes selected from the group consisting of spherical, angular, linear and amorphous, but the present invention is not particularly limited to the shapes of the active metal particles and / or the sacrificial metal particles.

[0162] According to one implementation example, the average particle size of the active metal particles and / or the sacrificial metal particles can be 0.1nm to 20nm, specifically 1nm to 10nm, and more specifically 1nm to 5nm, but the composite according to the present invention is not necessarily limited to the average particle size of the above-mentioned active metal particles and / or the above-mentioned sacrificial metal particles.

[0163] According to an implementation example, the first catalyst layer has a Pt(II) peak intensity I in a Pt 4fXPS spectrum of X-ray photoelectron spectroscopy (XPS) after 90,000 cycles of an accelerated durability test (ADT). 2 Compared with the Pt(II) peak intensity before the accelerated durability test 1 Ratio I 2 / I 1 It may be 0.5 or more, specifically 0.6 or more, more specifically 0.7 or more, and an example of its upper limit may be 1.0. At this time, the above peak intensity ratio can be obtained by Pt 4f 7 / 2 The XPS spectrum is measured. As the variation of the peak intensity of the electrochemical reaction of the first catalyst layer included in the membrane electrode assembly is reduced, the membrane electrode assembly can more effectively suppress the degradation of platinum, thereby having more excellent catalyst activity and durability.

[0164] At this time, the execution conditions of the 90,000-cycle accelerated durability test (ADT) may use the conditions proposed in the Million Mile Fuel Cell Truck protocol. Specifically, the accelerated durability test may be performed at 80°C and ambient pressure, pure hydrogen with a relative humidity of 100% may be supplied to the anode at a flow rate of 100 sccm and pure nitrogen with a relative humidity of 100% may be supplied to the cathode at a flow rate of 50 sccm, and one cycle of the accelerated durability test may consist of a 3-second hold interval at 0.6V, a 0.5-second rise interval, and a 3-second hold interval at 1.0V.

[0165] In one embodiment, the average particle size D of the active metal particles after 30,000 cycles of the accelerated durability test (ADT) is 2 The average particle size D of the active metal particles before the accelerated durability test 1 Ratio D 2 / D 1It may be 3 or less, specifically 2.5 or less, more specifically 2 or less, more specifically 1.5 or less, and its lower limit may be 1. The membrane electrode assembly satisfying the above average particle size ratio may refer to a membrane electrode assembly having more significantly improved catalyst activity and durability because the degradation phenomenon of the active metal is more suppressed due to the sacrificial metal.

[0166] At this time, the execution conditions of the 30,000-cycle accelerated durability test (ADT) can use the conditions proposed by the U.S. Department of Energy (DOE), specifically, the accelerated durability test can be performed at 80°C and ambient pressure, pure hydrogen with a relative humidity of 100% can be supplied to the anode at a flow rate of 100sccm and pure nitrogen with a relative humidity of 100% can be supplied to the cathode at a flow rate of 50sccm, and one cycle of the accelerated durability test can consist of a 3-second holding interval at 0.6V, a 0.5-second rising interval, and a 3-second holding interval at 1.0V.

[0167] According to an implementation example, the content of the sacrificial metal particles per unit area of ​​the first gas diffusion layer support may be 0.1 mg / cm 2 Up to 100mg / cm 2 , specifically 0.1 mg / cm 2 Up to 50mg / cm 2 , more specifically 0.1 mg / cm 2 Up to 20mg / cm 2 , more specifically, 0.1 mg / cm 2 Up to 10mg / cm 2 , but the content of the sacrificial metal particles included in the membrane electrode assembly according to the present invention is not particularly limited thereto. However, the content of the sacrificial metal particles per unit area of ​​the first gas diffusion layer support satisfies the above range, so that it is possible to have excellent catalyst activity while also having significantly improved durability. In the case where the first gas diffusion layer support contains the sacrificial metal particles to a degree less than the above range, it is difficult to suppress the deterioration of the active metal. In the case where the first gas diffusion layer support contains the sacrificial metal particles to a degree exceeding the above range, the catalyst activity may be reduced, thereby reducing the performance of the fuel cell included in the membrane electrode assembly.

[0168] According to an implementation example, the atomic ratio of the sacrificial metal included in the sacrificial metal particles included in the first gas diffusion layer to the active metal included in the active metal particles included in the first catalyst layer may be 0.1: 1 to 100: 1. In the atomic ratio of the sacrificial metal included in the sacrificial metal particles included in the first gas diffusion layer to the active metal included in the active metal particles included in the first catalyst layer, based on 1 mol of the active metal, the sacrificial metal may be 0.1 mol or more, 0.5 mol or more, 1 mol or more, 2 mol or more, 3 mol or more, 5 mol or more, or 10 mol or more, and the upper limit may be 100 mol or less, 90 mol or less, 80 mol or less, 70 mol or less, 60 mol or less, 50 mol or less, or 30 mol or less. Specifically, in the atomic ratio of the sacrificial metal included in the sacrificial metal particles included in the first gas diffusion layer to the active metal included in the active metal particles included in the first catalyst layer, based on 1 mol of the active metal, the sacrificial metal may be 0.1 mol to 100 mol, 0.5 mol to 90 mol, 1 mol to 80 mol, 3 mol to 70 mol, 5 mol to 60 mol, 10 mol to 50 mol or 10 mol to 30 mol. As an advantageous example, since the total number of atoms of the sacrificial metal is greater than the total number of atoms of the active metal, the sacrificial metal is oxidized or reduced instead of the active metal, thereby improving the durability of the membrane electrode assembly.

[0169] According to an implementation example, the ratio of the sacrificial metal to the active metal included in the membrane electrode assembly can be higher than the ratio of the sacrificial metal to the active metal included in the composite. Specifically, as described above, the membrane electrode assembly and the composite can select the ratio of the active metal to the sacrificial metal from the above range. However, even if the membrane electrode assembly includes a higher ratio of sacrificial metal than the composite under optimal conditions, the catalyst activity will not decrease. Therefore, even if the membrane electrode assembly includes more sacrificial metal than the composite, the catalyst activity is equivalent and can have higher durability. Moreover, even if the membrane electrode assembly includes a similar amount of sacrificial metal as the composite, the durability is equivalent and can have higher catalyst activity.

[0170] According to an implementation example, the first gas diffusion layer support and the second gas diffusion layer support may include a carbon-based material, and the carbon-based material can be smoothly supplied with the supplied fuel material or air and / or oxygen. As long as it is a material widely known in the art with conductivity, it can be used without restriction. Even if a person skilled in the art synthesizes it through common technical knowledge, or purchases a commercially available material for use, there is no restriction. As a non-limiting example, the carbon-based material can be selected from Vulcan carbon, carbon paper, carbon filter, carbon fiber, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, Timcal, and one or more carbon doped with other heterogeneous elements, but the present invention is not particularly limited thereto. The first gas diffusion layer support and the second gas diffusion layer support may be supports composed of the same substance as each other, or supports composed of different substances from each other.

[0171] According to an implementation example, when the membrane electrode assembly is used in a fuel cell as one of the energy conversion devices, the first catalyst layer may include an oxygen reduction reaction (ORR: Oxygen Reduction Reaction) catalyst, and the second catalyst layer may include a hydrogen oxidation reaction (HOR: hydrogen oxidation reaction) catalyst. Specifically, the first catalyst layer and the second catalyst layer may be catalyst layers in which active metal particles are loaded on a first catalyst layer support and a second catalyst layer support, respectively.

[0172] According to an implementation example, when the membrane electrode assembly is used in a water electrolysis reaction device as one of the energy conversion devices, the first catalyst layer includes a catalyst for hydrogen evolution reaction (HER), and the second catalyst layer includes a catalyst for oxygen evolution reaction (OER). Specifically, the first catalyst layer and the second catalyst layer can be catalyst layers with active metal particles loaded on the first catalyst layer support and the second catalyst layer support, respectively.

[0173] According to an implementation example, based on the total weight of the first catalyst layer or the second catalyst layer, the content of the active metal particles loaded on the first catalyst layer carrier or the second catalyst layer carrier can be 1 to 80 weight percent, specifically 4 to 40 weight percent, and more specifically 5 to 24 weight percent, but the membrane electrode assembly according to the present invention is not particularly limited to this.

[0174] According to an implementation example, the first catalyst layer support and the second catalyst layer support may include a carbon-based material, and the carbon-based material can be used without restriction as long as it includes a carbon material with excellent chemical stability and electrical conductivity known in the art, even if the technicians in this field synthesize it through common technical knowledge, or buy commercially available materials for use, there is no restriction. As a non-limiting example, the carbon-based material can be selected from Vulcan carbon, carbon paper, carbon filter, carbon fiber, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, Timcal, and one or more carbon doped with heterogeneous elements other than these, but is not particularly limited thereto. The first catalyst layer support and the second catalyst layer support can be supports composed of the same substance as each other, or supports composed of different substances from each other.

[0175] The present invention provides another fuel cell, the another fuel cell comprising the membrane electrode assembly described above. The another fuel cell may be a fuel cell different from the previous fuel cell comprising the composite according to the present invention, and the effects of the sacrificial metal particles and the active metal particles are the same or similar, and the another fuel cell comprising the membrane electrode assembly includes all the contents described in the fuel cell comprising the composite described above. And, before describing the another fuel cell, the another fuel cell will be collectively referred to as a fuel cell below.

[0176] The present invention provides a fuel cell including a membrane electrode assembly as described above, wherein the fuel cell (i.e., an energy conversion device) improves performance by including the membrane electrode assembly, and in particular, the durability is significantly improved, so that the performance of the energy conversion device can be maintained for a long time. Specifically, even after an accelerated durability test (ADT: Accelerated durability test) under harsh conditions, the retention rate of the electrochemical active surface area (ECSA: electrochemical active surface area), the maximum power density, the current density, and the activity per unit mass is high, and the increase in charge transfer resistance can be significantly reduced.

[0177] According to an implementation example, compared with before the accelerated durability test, the maximum power density retention rate of the fuel cell after 30,000 cycles of accelerated durability test (ADT) can be 80% or more, specifically 85% or more, more specifically 90% or more, and more specifically 95% or more. Moreover, compared with before the accelerated durability test, the maximum power density retention rate of the fuel cell after 90,000 cycles of accelerated durability test under more severe conditions can be 70% or more, specifically 75% or more, and more specifically 80% or more.

[0178] According to an implementation example, compared with before the accelerated durability test, the current density retention rate of the fuel cell at 0.2V after 30,000 cycles of accelerated durability test (ADT) may be 80% or more, specifically 85% or more, more specifically 90% or more, and more specifically 95% or more. Moreover, compared with before the accelerated durability test, the current density retention rate of the fuel cell at 0.2V after 90,000 cycles of accelerated durability test under more severe conditions may be 70% or more, specifically 75% or more, and more specifically 80% or more.

[0179] According to an implementation example, compared with before the accelerated durability test, the activity retention rate per unit mass of the fuel cell at 0.9V after 30,000 cycles of accelerated durability test (ADT) may be 60% or more, specifically 70% or more, more specifically 80% or more, more specifically 90% or more or 95% or more. Moreover, compared with before the accelerated durability test, the activity retention rate per unit mass of the fuel cell at 0.9V after 90,000 cycles of accelerated durability test under more severe conditions may be 50% or more, specifically 60% or more, more specifically 75% or more.

[0180] The fuel cell according to the present invention is one of the energy conversion devices, which may include a fuel cell and a water electrolysis cell, etc. Therefore, the membrane electrode assembly and / or the composite may also be used in the water electrolysis cell, thereby having similar significant effects.

[0181] According to an implementation example, as a non-limiting example of the fuel cell, the fuel cell may be a proton exchange membrane fuel cell (PEMFC) that operates at a low temperature and can be used in transportation vehicles.

[0182] The present invention provides a method for manufacturing a membrane electrode assembly, which comprises the following steps: a first step of doping a sacrificial metal precursor on a first gas diffusion support; a second step of reducing the sacrificial metal precursor doped on the first gas diffusion layer support to manufacture a first gas diffusion layer loaded with sacrificial metal particles on the first gas diffusion layer support; a third step of forming a first catalyst layer on one surface of a polymer electrolyte membrane; a fourth step of forming a second catalyst layer on the other surface of the polymer electrolyte membrane; a fifth step of forming the first gas diffusion layer on the first catalyst layer; and a sixth step of forming a second gas diffusion layer on the second catalyst layer.

[0183] In the manufacturing methods of the membrane electrode assembly according to the present invention, which are respectively described, as the support body for the gas diffusion layer, the active metal particles, the sacrificial metal particles, etc. are the same or similar to those described in the previous membrane electrode assembly, the manufacturing method of the membrane electrode assembly according to the present invention includes all the contents described in the previous membrane electrode assembly.

[0184] Hereinafter, the method for manufacturing the membrane electrode assembly of the present invention will be described in more detail.

[0185] Figure 3 FIG. 1 is a schematic diagram showing a process of supporting the sacrificial metal particles on the first gas diffusion layer support body to form the first gas diffusion layer. Figure 3 , a method for manufacturing a membrane electrode assembly according to the present invention is described, but this is only used to help understand the present invention, and the present invention is not limited to the drawings.

[0186] According to the method for manufacturing a membrane electrode assembly of the present invention, the method for manufacturing a membrane electrode assembly can manufacture a highly durable membrane electrode assembly capable of effectively suppressing degradation of active metals in a simple manner.

[0187] According to an implementation example, the sacrificial metal precursor of the first step may be a chloride, iodide, sulfide, fluoride, hydroxide, carbonate and / or nitrate of a metal having a standard reduction potential lower than that of the active metal included in the active metal particles. As a non-limiting example, the sacrificial metal precursor may be a nitrate of a metal having a standard reduction potential lower than that of the active metal included in the active metal particles, specifically silver nitrate (AgNO 3 ).

[0188] According to an implementation example, the first step may be a step of doping a solution containing a sacrificial metal precursor on the first gas diffusion layer support, and the solvent used at this time may be one or more solvents selected from the group consisting of: water, isopropanol, toluene, ethanol, n-propanol, n-butylacetate, ethylene glycol, butyl carbitol and butyl carbitol acetate, but the present invention is not limited to the solvents, and an appropriate solvent can be selected according to the chemical type of the active metal precursor.

[0189] According to an implementation example, the second step can be performed by immersing the first gas diffusion layer support doped with the sacrificial metal precursor into a solution containing a reducing agent. The solvent used at this time can be the same as the solvent described in the first step.

[0190] According to an implementation example, the reducing agent may be one or more reducing agents selected from the group consisting of sodium hydride (NaH), sodium borohydride (NaBH 4 ), lithium aluminum hydride (LiAlH 4 ), hydrazine (N 2 H 4 ), diisobutylaluminum hydride (DIBAH) and potassium triethylborohydride (KEt 3 BH).

[0191] According to an implementation example, the third step and the fourth step may use a method widely known in the art for stacking layers or thin films. As a non-limiting example, a catalyst layer forming slurry including the active metal particles may be coated on each surface of the polymer electrolyte membrane and then dried to form the first catalyst layer and the second catalyst layer.

[0192] According to an implementation example, the fifth step and the sixth step may use a method widely known in the art for stacking layers or films. As a non-limiting example, each of the first gas diffusion layer and the second gas diffusion layer may be assembled on each of the first catalyst layer and the second catalyst layer without hot-pressing.

[0193] According to an implementation example, the polymer electrolyte membrane can be used without limitation as long as it is a polymer substance known in the art and used in the field of fuel cells. As a non-limiting example, the polymer electrolyte membrane can be a polymer doped with one or more functional groups selected from the group consisting of sulfonated benzimidazoles, sulfonated polyimides, sulfonated polyetherimides, sulfonated polyphenylene sulfides, sulfonated polysulfones, sulfonated polyethers, sulfonated polyether ketones, sulfonated polyether-ether ketones, sulfonated polyether sulfones, sulfonated polyphenylquinoxalines, and sulfonated partial fluorines, but the present invention is not limited thereto.

[0194] Hereinafter, examples and experimental examples are specifically illustrated and described below. However, the examples and experimental examples described below are only examples of a part, and the technology described in this specification is not limited thereto.

[0195] (Example 1) Production of Composite Body 1

[0196] 100 mg of commercially available Pt / C (19.4 wt. % Pt, Tanaka Holdings Co., Ltd) was added to 100 mL of 50% isopropyl alcohol (IPA) solution and ultrasonicated for 30 minutes to prepare a dispersion. 0.1 mL of AgNO was added to the prepared dispersion. 3 solution (10 mg Ag+ / mL) and stirred for 10 minutes to prepare a reaction solution. 1 mL of NaBH 4 Solution (50 mg / mL) was added and the reduction reaction was carried out for 1 hour. The solution after the reaction was washed with deionized water and then dried in an oven overnight to produce a complex 1 (or Ag1+Pt / C) in which platinum (Pt) particles and silver (Ag) particles were loaded on a carbon carrier. The analysis results of inductively coupled plasma-optical emission spectroscopy (ICP-OES) showed that the atomic ratio of silver and platinum included in the complex 1 was 1:12.7.

[0197] (Example 2) Production of Composite Body 2

[0198] In addition to using 0.3 mL of AgNO in Example 1 3 In addition to the solution, a composite 2 (or Ag3+Pt / C) was manufactured in the same manner as in Example 1. The ICP-OES analysis results showed that the atomic ratio of silver and platinum included in the composite 2 was 1:4.41.

[0199] (Example 3) Production of Composite 3

[0200] In addition to using 0.5 mL of AgNO in Example 1 3 In addition to the solution, a composite 3 (or Ag5+Pt / C) was manufactured in the same manner as in Example 1. The ICP-OES analysis results showed that the atomic ratio of silver and platinum included in the composite 3 was 1:2.21.

[0201] (Example 4) Production of a gas diffusion layer loaded with a sacrificial metal

[0202] The area is 5cm 2 A commercial gas diffusion carbon layer (Sigracet39BC) was used as a gas diffusion layer support. The gas diffusion layer support was washed with acetone and dried on a hot plate at 60°C. Isopropyl alcohol (IPA) and deionized water mixed in a volume ratio of 1:1 were used as solvent to prepare 2 mg Ag+ / mL AgNO 3 Solution. 2.5 mL of AgNO 3 The solution was dropped onto the washed and dried gas diffusion layer support, and the gas diffusion layer support loaded with silver (Ag) ions was immersed in 10 mM NaBH 4 The NaBH solution was placed in the precipitate for 10 minutes to reduce the silver (Ag) ions to metallic silver (Ag), and then dried on a hot plate at 60° C. After complete drying, the NaBH was washed with isopropyl alcohol (IPA) and deionized water mixed in a 1:1 volume ratio. 4 The treated support for a gas diffusion layer was dried in an oven at 60° C. overnight, thereby manufacturing a gas diffusion layer in which silver (Ag) particles were supported on the support.

[0203] The analysis results of inductively coupled plasma-optical emission spectroscopy (ICP-OES, iCAP PRO ICP-OES, Thermo Fisher) showed that the loading amount of silver (Ag) on ​​the support was 1 mg / cm 2 .

[0204] (Example 5) Manufacturing of membrane electrode assembly

[0205] The membrane electrode assembly (MEA) was manufactured by spraying the catalyst slurry onto a Nafion N211 membrane (5 cm2 in area). 2) and dried on a hot plate at 60°C for several hours to form an anode catalyst layer and a cathode catalyst layer, respectively, and then the gas diffusion layer manufactured in Example 4 was assembled on each catalyst layer without hot-pressing to manufacture a membrane electrode assembly. The catalyst slurry used was a catalyst slurry composed of commercial Pt / C (19.4 weight percent Pt, Tanaka Holdings Co., Ltd), deionized water, IPA and 5 weight percent Nafion solution. The total catalyst loading of the anode and cathode was 0.05 mg Pt / cm 2 .

[0206] (Comparative Example 1) Commercial Pt / C

[0207] The experimental examples were performed using commercial Pt / C (19.4 weight percent Pt, Tanaka Holdings Co., Ltd).

[0208] (Comparative Example 2) Pt 3 Fabrication of Ag / C

[0209] 80 mg of commercial carbon (ketjen black EC600JD) was ultrasonically treated in 50 mL of deionized water for 1 hour to prepare a dispersion. Then, 0.168 mL of H 2 PtCl 6 solution (100 mg Pt4+ / mL) and 0.32 mL of AgNO 3 solution (10 mg Ag+ / mL) and stirred for 30 minutes to prepare a reaction solution. 2 mL of NaBH 4 Solution (50 mg / mL) was added and stirred for 12 hours. Finally, deionized water was used for filtration to produce Pt 2666, a Pt 2666 carbon support in which platinum and silver were supported in alloy form. 3 Ag / C. The molecular results of ICP-OES showed that the 3 The atomic ratio of silver to platinum in Ag / C is 1:3.67.

[0210] (Comparative Example 3) Production of Ag / C

[0211] Ag / C was manufactured in the same manner as in Example 2, except that commercial carbon (ketjen black EC600JD) was used instead of commercial Pt / C.

[0212] (Comparative Example 4) Production of a Gas Diffusion Layer Not Supporting a Sacrificial Metal

[0213] The area is 5cm 2The experimental examples were performed using a commercial gas diffusion carbon layer (Sigracet39BC) as the gas diffusion layer.

[0214] (Comparative Example 5) Production of a membrane electrode assembly without sacrificial metal support

[0215] A membrane electrode assembly was manufactured in the same manner as in Example 5, except that the gas diffusion layer of Comparative Example 4 was used instead of the gas diffusion layer manufactured in Example 4.

[0216] (Experimental Example 1) Chemical Property Analysis

[0217] Chemical property analysis confirmed that no alloy of platinum and silver was formed in the composite body of the embodiment. Specifically, X-ray diffraction (XRD, Rigaku Smartlab, 40 kV, 15 mA, 4 ° min -1 , Cu-Kα radiation, ), X-ray photoelectron spectroscopy (XPS, Kratos, AXIS-NOVA, 2.6×10 -9 torr), high-angle scattering dark-field scanning transmission electron microscopy (HAADF-STEM, FEI Themis Z), and energy dispersive X-ray spectroscopy (EDS, FEI Themis Z).

[0218] Figure 4 It is a figure which shows the XRD patterns of Comparative Example 1 and Examples 1 to 3. Figure 5 : is a diagram showing the XRD patterns of Comparative Example 1, Comparative Example 2 and Example 2. Figure 4 and Figure 5 It can be seen that Comparative Example 1 and Examples 1 to 3 have a main peak at 39.8°, which is (111) equivalent to face-centered cubic (fcc) Pt (JCPDS No. 04-0802). That is, the composite according to the example has a peak at the same position as Pt / C, which indicates that platinum and silver included in the composite are not alloyed. On the contrary, in the case of Comparative Example 2 having an alloy form, it can be seen that there is a peak at 39.2°, which is 0.6° shifted compared with Example 2 and Comparative Example 1.

[0219] In addition, refer to Figure 4 It can be seen that the peak intensity in the (111) plane of the embodiment is increased compared with that of the comparative example. This is because the peak in the (111) plane overlaps with the characteristic peak of Ag (JCPDS No. 04-0783, fcc Ag) added in the embodiment, and this is Figure 6 As shown, this is caused by the increase of metallic Pt components.

[0220] Figure 6 Graphs showing Pt 4f XPS spectra of Comparative Example 1 and Examples 1 to 3. Figure 7 3d XPS spectra of Comparative Example 1 and Examples 1 to 3 are shown. Figure 8 3 is a diagram showing the Pt4f XPS spectra of Comparative Example 1, Comparative Example 2, and Example 2. Fig. 9 3d XPS spectra of Comparative Example 2, Comparative Example 3, and Example 2.

[0221] Reference Figure 6 , Comparative Example 1, Examples 1 to 3 have the same Pt ​​peak position (at Pt 4f 7 / 2 In the case of Pt 0 For Pt 2+ For , it is ~72.9 eV). Figure 7 , Examples 1 to 3 mainly have metallic Ag signals (in Ag 3d 5 / 2 In the case of Ag 0 368.0 eV), and the increase in Ag concentration increases the signal intensity without positional shift. It can be seen that the composite according to the embodiment does not form an alloy. Figure 8 and Fig. 9 , Comparative Example 2 shows a slightly higher binding energy in the Pt 4f XPS spectrum than that of Example 2 and Comparative Example 1, and on the contrary, shows a lower binding energy in the Ag 3d XPS spectrum than that of Example 2 and Comparative Example 3. That is, in Comparative Example 2, the electronic structure changes due to the interaction between Pt and Ag.

[0222] In addition, refer to Figure 6 , Pt 4f based on X-ray photoelectron spectroscopy (XPS) 7 / 2 In the XPS spectrum, the peak intensity I 0 Pt(II) peak intensity I II Ratio I 0 / I II In the case of Comparative Example 1, the value is 1.76; in the case of Example 1, the value is 1.88; in the case of Example 2, the value is 2.38; and in the case of Example 3, the value is 2.85. That is, as the content of Ag included in the composite increases, the metallic Pt 0 The peak intensity of Pt 2+ The peak intensity of Pt 2+ Reduced to Pt 0 , and with Figure 4The XRD spectrum results are consistent with those of

[0223] Fig.10 is the HAADF-STEM image of Example 2 and the corresponding EDS mapping image, Fig.11 It is an image of an enlarged HAADF-STEM image of Example 2 and a corresponding EDS mapping image. Fig.12 is the HAADF-STEM image of Comparative Example 2 and the corresponding EDS mapping image. Figures 10 to 12 In the case of Comparative Example 2, it can be clearly confirmed that an alloy is formed, but in the case of Example 2, the platinum (Pt) particles and the silver (Ag) particles are uniformly distributed on the carbon carrier, and it can be seen that the platinum (Pt) particles and the silver (Ag) particles are distributed independently of each other without any interaction between them.

[0224] (Experimental Example 2) Electrochemical Property Analysis

[0225] The samples were analyzed using a VSP potentiostat (Bio-Logic SAS) with a standard three-electrode cell in 0.1 M HClO 4 The electrochemical performance for oxygen reduction reaction was evaluated in the experiment. KCl-saturated Ag / AgCl electrode, Pt wire and rotating disk electrode (RDE, diameter: 3 mm, area: 0.07065 cm) were used as reference electrode, counter electrode and working electrode, respectively. 2 At this time, 2.5 mg of the powders prepared according to Comparative Example 1, Comparative Example 2, and Examples 1 to 3 were placed in a mixed slurry mixed with 4 mL of deionized water, 1 mL of IPA, and 0.4 mL of a 5 weight percent Nafion solution, and ultrasonically treated for 30 minutes to prepare a uniformly dispersed slurry, and then the uniform slurry was applied to RDE, thereby preparing a Pt loaded 50 μg / cm 2 Degree of the amount of working electrode.

[0226] Before the electrochemical performance evaluation, the 4 The stabilization was performed by 30 cycles of cyclic voltammetry (CV) at a scan rate of 50 mV / s and a scan range of 0.05 V to 1.15 V. In an oxygen or nitrogen saturated 0.1 M HClO 4 In the solution, linear sweep voltammetry (LSV) was performed at a scan rate of 10 mV / s, and the final polarization curve was obtained by subtracting the current density in nitrogen from the current density in oxygen. 4CV was performed in solution at a scan rate of 50 mV / s and a scan range of 0.05 V to 1.15 V.

[0227] The accelerated durability test (ADT) was conducted during 30,000 (30k) cycles by heating the samples in a nitrogen-saturated 0.1 M HClO 4 CV was performed in solution at a scan rate of 100 mV / s and in a scan range of 0.60 V to 0.95 V. After the ADT was completed, LSV was performed under the same initial measurement conditions.

[0228] Fig.13 : is a graph showing the evaluation results of the electrochemical performance of Comparative Example 1 and Examples 1 to 3. Specifically, Fig.13 (a) and Fig.13 (b) is a graph showing an LSV curve and a CV curve, Fig.13 (c) to Fig.13 (f) is a graph showing LSV curves before and after ADT of each of Comparative Example 1 and Examples 1 to 3. Fig.14 : is a graph which shows the CV curves before and after ADT of each of Comparative Example 1 and Examples 1 to 3. Fig.15 : These are transmission electron microscope (TEM, FEI Tecnai G2 twin) images of each of Comparative Example 1 and Example 2 before and after ADT. Fig.16 : is a graph showing the evaluation results of the electrochemical performance of Comparative Example 2 as an alloy form. Specifically, Fig.16 (a) is a diagram showing the LSV curve before and after ADT, Fig.16 (b) is a graph showing CV curves of Comparative Example 1, Comparative Example 2, and Example 2, Fig.16 (c) is a graph showing the CV curves of Comparative Example 2 before and after ADT.

[0229] Reference Fig.13 (a), for Example 1 and Example 2, they show similar onset and half-wave (E 1 / 2 ) potential, while Example 3 exhibited slightly lower performance. This is because, for Example 3, as the silver (Ag) loading amount increased, the aggregated silver nanoparticles blocked the catalyst active sites of platinum.

[0230] Reference Fig.13(b), for Examples 1 to 3, a pair of silver (Ag) reduction and oxidation peaks are shown at ~0.4V and ~0.55V, respectively. As the silver (Ag) loading increases, the maximum value of this redox peak tends to move to the lower potential side. If the silver (Ag) loading increases, the surface area of ​​the exposed silver (Ag) increases, thereby providing more redox reaction sites, and the overvoltage for the redox reaction is relatively reduced. On the contrary, as the silver (Ag) loading increases, the oxidation of platinum (Pt) moves to a higher potential. Specifically, for Comparative Example 1, it is 0.733V, for Example 1, it is 0.745V, for Example 2, it is 0.781V, and for Example 3, it is 0.797V. It can be seen that the composite according to the embodiment can inhibit the oxidation of platinum (Pt) as it includes silver (Ag) particles.

[0231] Reference Fig.13 (c) to Fig.13 (f), for Comparative Example 1, the half-wave potential decreased by 52 mV, whereas for Example 1, it decreased by 38 mV, and for Example 2, it decreased by 12 mV. In particular, for Example 3, it can be seen that the initial half-wave potential of 0.790 V was maintained during the ADT period without substantial change. Fig.14 , the dissolution of platinum (Pt) caused by oxidation of platinum (Pt) and the change of electrochemical active surface area (ECSA) caused by aggregation during ADT can be determined. The retention rate of ECSA increases with the increase of the loading amount of silver (Ag). Specifically, for Comparative Example 1, it is 51.6%, for Example 1, it is 68.4%, for Example 2, it is 84.8%, and for Example 3, it is 100%. And, referring to Fig.15 It can be confirmed that, for Comparative Example 1, the size of the platinum (Pt) particles increased by 2-4 times, whereas, for Example 2, the size distribution of the particles (2-4 nm) was maintained before and after ADT. Fig.16 It can be seen that in the alloy form of Comparative Example 2, after ADT, as the silver (Ag) particles that block the catalyst reaction sites of platinum are dissolved, the half-wave potential and ECSA increase. Even so, they still have significantly lower values ​​than those of Example 2 and Comparative Example 1, thereby having reduced ORR catalyst activity.

[0232] In summary, since the composite according to the example includes the sacrificial metal particles capable of suppressing oxidation of the active metal in a state where the composite does not form an alloy with the active metal, it is known that the ORR catalyst activity is excellent.

[0233] (Experimental Example 3) Property Analysis of Fuel Cell Including Composite Body

[0234] In order to test the performance of proton exchange membrane fuel cells (PEMFC), a 5 cm active area 2 A membrane electrode assembly (MEA) was manufactured using a catalyst-coated membrane (CCM). Commercial Pt / C (19.4 weight percent Pt, Tanaka Holdings Co., Ltd) was used as an anode catalyst. The composite manufactured in the embodiment or comparative example was used as a cathode catalyst. Each catalyst was mixed with deionized water, IPA and 5 weight percent Nafion solution to make a slurry, and then the manufactured slurry was sprayed on a Nafion N211 membrane and dried on a hot plate at 60°C for several hours to manufacture a CCM. All catalyst loadings for the anode and cathode were 0.05 mg Pt / cm 2 .

[0235] The proton exchange membrane fuel cell was operated at 80°C, 0.5 bar back pressure and constant current conditions by supplying pure hydrogen with a relative humidity of 100% to the anode at a flow rate of 300 sccm and pure oxygen with a relative humidity of 100% to the cathode at a flow rate of 1000 sccm. 2 Electrochemical impedance spectroscopy (EIS) was performed at 5 kHz to 100 MHz under the battery current condition.

[0236] In order to evaluate the durability of the catalyst, an accelerated durability test (ADT) was performed based on the CV cycle of 30k proposed by the U.S. Department of Energy (DOE). According to the electrocatalyst cycling protocol, pure hydrogen with a relative humidity of 100% was supplied to the anode at a flow rate of 100 sccm and pure nitrogen with a relative humidity of 100% was supplied to the cathode at a flow rate of 50 sccm at 80°C and ambient pressure, while the positive potential was maintained between 0.6V and 0.95V for 3 seconds. The rise time between positive potentials was 0.5 seconds.

[0237] Fig.17 and Fig.18: is a graph showing the performance before and after ADT performed during 30k cycles of a fuel cell using each of Comparative Example 1 and Examples 1 to 3 as a cathode catalyst. Specifically, Fig.17 (a) is a graph showing a polarization curve and a power density curve of a fuel cell using Comparative Example 1, Fig.17 (b) is a graph showing a polarization curve and a power density curve of a fuel cell using Example 1, Fig.17 (c) is a graph showing a polarization curve and a power density curve of a fuel cell using Example 2, Fig.17 (d) is a graph showing a polarization curve and a power density curve of the fuel cell using Example 3. Fig.18 (a) shows the maximum power density P before and after ADT max The picture, Fig.18 (b) shows the current density j at 0.2 V before and after ADT 0.2V The picture, Fig.18 (c) is a graph showing the activity per unit mass (mass activity) at 0.9 V without iR before and after ADT. Fig.19 It is a graph showing polarization curves and power density curves before and after ADT of a fuel cell using Comparative Example 2 in an alloy form as a cathode catalyst. Fig. 20 : is a graph showing the change in particle size of the fuel cells of Comparative Example 1 and Example 2 before and after ADT. Specifically, Fig. 20 (a) and Fig. 20 (b) are TEM images of the fuel cell of Comparative Example 1 before and after ADT, Fig. 20 (c) and Fig. 20 (d) are TEM images of the fuel cell of Example 2 before and after ADT.

[0238] Reference Fig.17 and Fig.18 It can be seen that all the fuel cells using Examples 1 to 3 have excellent durability compared to Comparative Example 1, and as the amount of silver (Ag) loaded increases, the difference in maximum power density, current density, and activity per unit mass according to ADT at 30k cycles decreases, thereby having a tendency to increase durability. Fig.19 It can be seen that the maximum power density and current density of the fuel cell using Comparative Example 2 after ADT increase, but even so, have significantly lower values ​​than those of Examples 1 to 3, thereby having reduced ORR catalyst activity. Fig. 20 It was confirmed that during the ADT period, the average particle size of the platinum (Pt) particles of Example 2 increased from 2.5 nm to 4 nm, whereas the average particle size of the platinum (Pt) particles of Comparative Example 1 increased from 2.5 nm to 10 nm.

[0239] In summary, since the composite according to the embodiment includes the sacrificial metal particles without forming an alloy with the active metal, the initial ORR catalyst activity can be maintained or reduced at a low reduction rate even after severe ADT, and it can be seen that the durability is excellent.

[0240] (Experimental Example 4) Metal Dissolution Analysis

[0241] For the dissolution analysis of platinum and silver, an in situ inductively coupled plasma mass spectrometer (ICP-MS, iCAP RQ, Thermo-Fisher Science) was used. Specifically, a directly manufactured electrochemical flow cell (EFC) was combined with ICP-MS. The EFC consisted of a U-shaped channel with an opening diameter of 3 mm for connection with a working electrode (A-002012, Bio-Logic), and a graphite tube counter electrode and an Ag / AgCl reference electrode were connected to the inlet and outlet of the EFC, respectively. The catalyst ink was drop-cast onto glassy carbon (0.07065 cm 2 ) with a loading of 10 μg / cm 2 The working electrode was made of metal. The catalyst ink for ICP-MS study was made by dispersing 5 mg of catalyst in an aqueous solution including 1179 μl of deionized water, 50 μl of Nafion and 186 μl of IPA. Argon-saturated 0.1 M HClO 4 The electrolyte contains 5 ppb 187 Re and 0.5 M HNO 3 The internal standard solution is mixed and then put into the ICP-MS. 195 Pt and 107 Ag relative to 187 The Re signal was used to quantitatively estimate the dissolution properties of platinum and silver.

[0242] The electrochemical protocol used for the online ICP-MS experiment consisted of a sequence of chemical dissolution steps, activation steps, and slow scan steps. In the chemical dissolution step, no potential was applied, the activation step consisted of 50 cycles of CV at a fast scan rate (200 mV / s), and the slow scan step consisted of a 0.05 to 1.2 V RHE The CV was composed of 5 cycles of slow scan rate (5 mV / s). Between the activation step and the slow scan step, the potential was kept at 0.05 V. RHE To stabilize the ICP-MS signal.

[0243] Figure 21 to Figure 23is a graph showing the results of online ICP-MS experiments performed on Comparative Example 1 and Example 2. Specifically, Fig.21 It is a graph showing the dissolution curves of platinum and silver according to various treatment conditions. Fig. 22 (a) and Fig. 22 (b) is a graph showing the dissolution rates of platinum and silver relative to the amounts supported on the working electrode. Fig.23 It is a graph showing the dissolution curve according to each cycle performed at a slow scanning speed (5 mV / s). Figure 24 to Figure 26 : is a graph showing the results of the online ICP-MS experiment performed in the above-mentioned manner for Comparative Examples 1 and 2.

[0244] First, in the chemical dissolution step, chemically unstable platinum cannot participate in the reduction reaction after being leached by the acidic electrolyte and is oxidized, thereby dissolving chemically stable platinum. Fig.21 and Fig. 22 For Comparative Example 1, the dissolution rates of platinum in the chemical dissolution step and the activation step were 0.38% and 0.25%, respectively, whereas for Example 2, the dissolution rates of platinum in the chemical dissolution step and the activation step were 0.19% and 0.12%, respectively, so that the composite of Example 2 has further improved stability. In the slow scanning step, for Comparative Example 1, the dissolution rate of platinum per cycle was 0.10%, whereas for Example 2, the dissolution rate of platinum per cycle was 0.043%, which is 23 times smaller than that, so it can be seen that the composite of Example 2 has significantly improved stability because platinum is hardly dissolved.

[0245] If you insert Fig.21 Observing the activation step in detail with reference to the accompanying drawings, the dissolution behavior of platinum in the interval between 300 seconds and 600 seconds for both Comparative Example 1 and Example 2 is similar, and it can be seen that the dissolution of silver in Example 2 is also in the same interval. However, for Example 2, unlike Comparative Example 1, it can be seen that the dissolution of platinum and silver hardly occurs after 600 seconds.

[0246] Reference Fig.23 For Comparative Example 1, the average platinum dissolution rate at 0.77 V was 12 μg / g Pt ·s(3.7×10 16 atom Pt / g Pt ·s), on the contrary, for Example 2, the average dissolution rate of platinum was 0.15μg / g Pt ·s(4.6×10 14 atom Pt / g Pt ·s), the difference is about 80 times. In Example 2, the average dissolution rate of silver is 1.4 μg / g Ag·s(7.8×10 16 atom Ag / g Ag ·s) average dissolution rate.

[0247] Reference Figure 24 to Figure 26 For Comparative Example 2, the dissolution rates of platinum in the chemical dissolution step and the activation step were 0.03% and 0.18%, respectively, and the dissolution rates of silver were 12.26% and 64.43%, respectively. In each cycle of the slow step, the average dissolution rate of platinum was 4.2 μg / g at 0.77 V. Pt ·s, the average dissolution rate of silver is 66.8μg / g at 1.08V Ag s. That is, for Comparative Example 2 in the alloy form, the dissolution of platinum was suppressed compared with Comparative Example 1, but the dissolution of platinum was not effectively suppressed compared with Example 2. Therefore, it is known that the alloy form is unstable under repeated electrochemical oxidation and reduction potentials, and that silver (Ag) included in the composite in the alloy form cannot fully perform the function of a sacrificial metal compared with silver (Ag) included in the composite according to one embodiment in the non-alloy form.

[0248] In summary, it is speculated that the composite according to one embodiment is converted into a structure having high resistance to electrochemical oxidation reaction after dissolving an excessive amount (40% relative to the initial loading amount) of silver in the chemical dissolution and activation steps.

[0249] (Experimental Example 5) Chemical Structure and Electronic Structure Analysis of the Complex

[0250] The chemical structure and electronic structure were analyzed by X-ray absorption spectroscopy (XAS) including XANES (X-ray absorption near edge structure) and EXAFS (extended X-ray absorption fine structure) measurements.

[0251] XAS spectra were measured at the BL8C beamline of Pohang Light Source (PLS-II) at a ring current of 250 mA and 3.0 GeV. They were collected in both transmission and fluorescence modes, and the acquired spectra were processed using the Demeter package.

[0252] To monochromate the X-ray beam, a Si (111) double crystal monochromator was used. The higher order harmonic contamination generated during the XAS experiment was adjusted to reduce the intensity of the transmitted X-ray by 30%.

[0253] In situ XAS was performed using an electrochemical cell of a standard three-electrode system. As the reference electrode, counter electrode, and working electrode, Ag / AgCl electrode, graphite rod, and carbon paper coated with the catalyst of the embodiment or comparative example were used, respectively. A 0.1 M HClO solution saturated with nitrogen was used. 4 was used as the electrolyte. For catalyst stabilization, CV cycles were performed 20 times in the range of 0.05 V to 1.05 V before XAS measurement. Then, after stabilization for 30 minutes, XAS was analyzed using chronoamperometry at various potentials from open circuit voltage (OCV) to 1.5 V. XAS spectra were collected in fluorescence mode by a silicon drift detector (SDD). The acquired spectra were processed using the Demeter package. 3 The Pt oxidation state was evaluated in the white line peak region of the -edge XANES spectrum.

[0254] Fig. 27 The results are shown for Comparative Example 1 (or Comparative Example 3), Comparative Example 2, Example 2, Pt foil (or Ag foil) and PtO 2 (or AgO 2 ) of Pt L 3 -edge (or Ag K-edge). Specifically, Fig. 27 (a) and Fig. 27 (b) is Pt L 3 -Edge XANES spectrum, Fig. 27 (c) is Pt L 3 -Edge FT-EXAFS spectrum, Fig. 27 (d) and Fig. 27 (e) is the Ag K-edge XANES spectrum, Fig. 27 (f) is the Ag K-edge FT-EXAFS spectrum. Fig.28 The Pt L of Comparative Example 1, Example 2 and Comparative Example 2 is shown. 3 -A graph of the in-situ XAS spectrum of the edge. Specifically, Fig.28(a) Fig.28 (d) and Fig.28 (g) are the XANES spectra of Comparative Example 1, Example 2 and Comparative Example 2, respectively. Fig.28 (b) Fig.28 (e) and Fig.28 (h) are the enlarged XANES spectra, Fig.28 (c) Fig.28 (f) and Fig.28 (i) are the FT-EXAFS spectra of Comparative Example 1, Example 2 and Comparative Example 2, respectively. Fig.29 is a graph showing the oxidation state of platinum according to the applied potential of Comparative Example 1, Example 2, and Comparative Example 2. Specifically, it is derived according to Fig.28 data, Fig.29 (a) is a graph showing changes in the oxidation number of platinum, Fig.29 (b) is a graph showing a Pt—O formation curve.

[0255] Reference Fig. 27 (a) and Fig. 27 (b), for Comparative Example 1, in the case of PtO 2 There is a white line peak at 11568.0 eV, which is similar to the peak position of Pt foil, for Example 2, there is a white line peak at 11567.2 eV, and for Comparative Example 2, there is a white line peak at 11566.7 eV, which is almost the same peak position as that of Pt foil. It can be seen that as the composite according to an embodiment includes silver (Ag) particles, the oxidation state of platinum is reduced and the metallic platinum component increases.

[0256] refer to Fig. 27 (c), for Comparative Example 1, respectively and The radial distances of Pt-O and Pt-Pt are similar to those of Pt foil ( ) Similar The Pt-Pt radial distance is longer than that of Comparative Example 2 due to the alloying effect. Pt-Pt radial distance.

[0257] Reference Fig. 27 (d) and Fig. 27 As shown in (e), all samples have white line peaks at similar positions, thus having similar Ag oxidation states. Fig. 27 As can be seen from (f), for Comparative Example 2, similarly, due to the alloying effect, the ) and Comparative Example 3 ( ) compared to mobile Ag-Ag radial distance.

[0258] Reference Fig.29 (a) shows that for Example 2, it has a Pt oxidation number similar to that of Comparative Example 1 in OCV, but has a lower Pt oxidation number in the potential range above OCV, so that the addition of silver (Ag) actually plays a key role in inhibiting the oxidation of platinum (Pt). On the contrary, for Comparative Example 2, a lower platinum (Pt) oxidation state is exhibited in the applied potential range, and alloyed silver (Ag) can also play the role of a sacrificial substance. However, compared with the composite independently loaded with silver (Ag) particles, Comparative Example 2 as an alloy form exhibits low ORR activity because the silver (Ag) present on the surface partially blocks the active sites of platinum (Pt).

[0259] Reference Fig.29 (b), Comparative Example 1 shows a significantly increased Pt-O interaction energy compared to Example 2 or Comparative Example 2. In Example 2 or Comparative Example 2, the tendency to form Pt-O is significantly reduced due to the sacrificial effect of silver that is oxidized earlier than platinum. However, Fig. 9 As shown in the figure, due to the low binding energy of silver, the dissolution of silver in Comparative Example 2 is much faster than that in Example 2, thereby confirming that the silver (Ag) particles supported on the carbon support independently of the platinum (Pt) particles are more suitable and more effective in inhibiting the oxidation and dissolution of platinum. As a result, in the composite according to an embodiment, since the active metal particles and the sacrificial metal particles exist independently, the sacrificial metal particles can better play the role of sacrificial agent, thereby essentially solving the oxidation problem of the active metal.

[0260] (Experimental Example 6) Analysis of properties of gas diffusion layer

[0261] In order to analyze the properties of the gas diffusion layer, scanning electron microscopy (SEM, Magellan400, FEI Company), energy dispersive X-ray spectroscopy (EDS, FEI Themis Z), and X-ray diffraction (XRD, Rigaku Smartlab, 40 kV, 15 mA, 4 ° min -1 , Cu-Kα radiation, X-ray photoelectron spectroscopy (XPS, Kratos, AXIS-NOVA, 2.6×10 -9 torr).

[0262] Fig.33 : is a figure showing the scanning electron microscope (SEM) image of the gas diffusion layer of Comparative Example 4 and Example 4. Specifically, Fig.33 (a) and Fig.33 (b) is an image of a commercial gas diffusion layer of Comparative Example 4, Fig.33 (c) and Fig.33 (d) is an image of the gas diffusion layer manufactured in Example 4. Fig.34 is a diagram showing an SEM image of a gas diffusion layer of Comparative Example 4 and a corresponding EDS mapping image, Fig.35 : is a figure which shows the SEM image of the gas diffusion layer of Example 4 and the corresponding EDS mapping image. Fig.36 (a) is a diagram showing X-ray diffraction (XRD) patterns of the gas diffusion layers of Comparative Example 4 and Example 4, Fig.36 (b) is a diagram showing the Ag 3d XPS spectra of the gas diffusion layers of Comparative Example 4 and Example 4.

[0263] Reference Fig.33 In Comparative Example 4, a porous network structure in which randomly distributed carbon fibers were assembled was observed, and in Example 4, white particles formed on the carbon fibers of the porous network structure were observed. Fig.34 and Fig.35 It can be seen that, for Example 4, the silver (Ag) particles are randomly distributed on the carbon fibers. Fig.36 (a), for Example 4, unlike Comparative Example 4, in the face-centered cubic (fcc) structure, a peak (38°) at the (111) plane and a peak (44°) at the (200) plane corresponding to the (Ag) crystal structure were observed. Fig.36 (b), for Example 4, unlike Comparative Example 4, Ag 3d 3 / 2 and Ag 3d 5 / 2 Ag 0 Peak. It can be seen from this that the white particles observed in the gas diffusion layer of Example 4 are silver (Ag) metal.

[0264] (Experimental Example 7) Property Analysis of Fuel Cell Including Membrane Electrode Assembly

[0265] The performance of a proton exchange membrane fuel cell (PEMFC) was evaluated using the membrane electrode assemblies manufactured in Example 5 and Comparative Example 5. Specifically, the proton exchange membrane fuel cell was operated at 80° C., 0.5 bar back pressure, and constant current by supplying pure hydrogen with a relative humidity of 100% to the anode at a flow rate of 300 sccm and pure oxygen with a relative humidity of 100% to the cathode at a flow rate of 1000 sccm.

[0266] To evaluate the durability of the catalyst, an accelerated durability test (ADT) was performed based on 30,000 (30k) cyclic voltammetry (CV) cycles proposed by the U.S. Department of Energy (DOE), and recently expanded to 90,000 (90k) cycles as proposed in the Million Mile Fuel Cell Truck (M2FCT) protocol. According to the electrocatalyst ADT cycle protocol, pure hydrogen with a relative humidity of 100% was supplied to the anode at a flow rate of 100 sccm and pure nitrogen with a relative humidity of 100% was supplied to the cathode at a flow rate of 50 sccm at 80°C and ambient pressure, while being held between 0.6V and 1.0V for 3 seconds at a positive potential. The rise time between positive potentials was 0.5 seconds.

[0267] Fig.37 is a graph showing polarization curves according to ADT cycles using the fuel cells of Example 5 and Comparative Example 5. Specifically, polarization curves were measured at the initial, 30,000 (30k) cycles, 60,000 (60k) cycles, and 90,000 (90k) cycles before performing ADT.

[0268] The maximum power density (P max ), current density at 0.2V (j 0.2V ), activity per unit mass at 0.9 V without iR (MA 0.9V ) values ​​and the retention rates of various properties relative to the initial values ​​are summarized in Table 1.

[0269]

Table 1

[0270]

[0271]

[0272] Referring to Table 1, before ADT was performed, there was no significant difference between Comparative Example 5 and Example 5. In contrast, after ADT was performed, the performance of the fuel cell of Comparative Example 5 was significantly reduced, but the performance of the fuel cell of Example 5 almost maintained the initial performance.

[0273] Fig.38: is a graph showing the measurement results of electrochemical impedance spectroscopy (EIS) according to the ADT cycle using the fuel cells of Example 5 and Comparative Example 5. At this time, the electrochemical impedance spectroscopy was performed at 100 mA / cm 2 The results of Comparative Example 5 are shown in FIG. Fig.38 (a) After 30,000 (30k) cycles, the resistance of the 2 Increased to 1.35Ω·cm 2 , after 90,000 (90k) cycles, it increases to 1.58Ω·cm 2 In contrast, referring to the results of Example 5 Fig.38 (b) After 30,000 (30k) cycles, the resistance of the capacitor decreased from 0.912 Ω·cm 2 Increase to 1.00Ω·cm 2 , after 90,000 (90k) cycles, it increases to 1.24Ω·cm 2 , it can be seen that compared with Comparative Example 5, the charge transfer resistance is greatly reduced.

[0274] Fig.39 is a graph showing CV curves according to the ADT cycle using the fuel cells of Example 5 and Comparative Example 5. Fig.39 For Comparative Example 5, after 30,000 (30k) and 90,000 (90k) cycles, the electrochemically active surface area (ECSA) only maintained 31.7% and 8.6% of the initial value, respectively, while for Example 5, it maintained 100% and 47.1%, respectively.

[0275] It can be seen that the membrane electrode assembly of the present invention and the fuel cell including the membrane electrode assembly contain a gas diffusion layer of sacrificial metal particles, so there is an advantage that the durability of the catalyst is significantly improved. Specifically, even after an accelerated durability test (ADT: Accelerated durability test) under harsh conditions, the retention rate of the electrochemical active surface area (ECSA: electrochemical active surface area), maximum power density, current density and activity per unit mass (mass activity) is high, and the increase in charge transfer resistance can be significantly reduced.

[0276] To illustrate the improvement in performance as described above, the cathode catalyst layer and cathode gas diffusion layer were analyzed after performing ADT.

[0277] Fig.40 4f X-ray photoelectron spectroscopy (XPS) spectra of Pt measured before and after ADT was performed on the cathode catalyst layer in the membrane electrode assemblies manufactured in Comparative Example 5 and Example 5. 0 and Pt 2+ The two corresponding peaks are deconvoluted. For example, in Pt 4f 7 / 2 In the case of Pt 0 For Pt 2+ For , it has ~72.9 eV. Fig.40 For Comparative Example 5, as the ADT cycle increases, Pt 2+ The peak intensity of Pt 0 The peak intensity gradually increases. This is because the surface area of ​​platinum (Pt) decreases and the catalyst activity is greatly lost due to the increase in the size of the platinum (Pt) metal particles. For Example 5, as in Comparative Example 5, the Pt 2+ and Pt 0 The peak intensity of Pt(II) decreases / increases with the increase of ADT cycles, but the rate of change of decrease or increase is significantly small, unlike Comparative Example 5. Specifically, for Comparative Example 5, the peak intensity of Pt(II) after 90,000 cycles of accelerated durability test is 2 Pt(II) peak intensity before and after accelerated durability test 1 Ratio I 2 / I 1 The calculated result is 0.41. For Example 5, the above peak intensity ratio I 2 / I 1 The calculated value is 0.71, thus confirming that P in Example 5 t2+ The change rate of peak intensity reduction is smaller than that of Pt in Comparative Example 5. 2+ The rate of change of peak intensity decrease.

[0278] Fig.41 (a) is a diagram showing an XRD pattern according to an ADT cycle of a gas diffusion layer included in a membrane electrode assembly manufactured in Example 5, Fig.41 (b) is a diagram showing the Ag 3d XPS spectrum.

[0279] Reference Fig.41 , the silver (Ag) particles included in the gas diffusion layer are greatly reduced after 30,000 (30k) cycles, and most of them disappear after 90,000 (90k) cycles. Fig.41 Part (b), Ag 3d after 30,000 (30k) cycles 5 / 2The peak intensity was 15.0% of the initial peak intensity and completely disappeared after 90,000 (90k) cycles. In order to confirm the more accurate reduction of silver (Ag), ICP-OES analysis was further performed. The results showed that after 30,000 (30k) cycles, the amount of silver (Ag) was shown to be as small as the initial loading amount (1 mg / cm 2 ) 13% of 0.13 mg / cm 2 After 90,000 (90k) cycles, no signal was detected. It can be seen that the metallic silver (Ag) included in the gas diffusion layer was oxidized to Ag. + and is etched in the electrolyte, whereas platinum (Pt), the active metal, remains as metallic Pt during the ADT cycle due to the sacrifice of silver (Ag).

[0280] Fig.42 (a) is a diagram showing a transmission electron microscope (TEM, FEI Tecnai G2 twin) image of the catalyst layer included in Comparative Example 5 or Example 5 before performing ADT, Fig.42 (b) and Fig.42 (c) are diagrams showing TEM images of the catalyst layer included in Comparative Example 5 after 30,000 (30k) cycles and 90,000 (90k) cycles, respectively. Fig.42 (d) and Fig.42 (e) are diagrams showing TEM images of the catalyst layer included in Example 5 after 30,000 (30k) cycles and 90,000 (90k) cycles, respectively. Fig.42 (a), before ADT is performed, the size of the platinum (Pt) particles is 2 nm to 3 nm, thus having a uniform size distribution, and the average particle size at this time is 2.5 nm. Fig.42 (b) and Fig.42 (c), the size of the platinum (Pt) particles increased significantly to 5 nm to 50 nm, and the average particle sizes after 30,000 (30k) cycles and 90,000 (90k) cycles were 10 nm and 15 nm, respectively. This increase in the size of the platinum (Pt) particles is caused by the dissolution and aggregation of platinum (Pt), and this is the main reason for the reduction in the performance of the fuel cell. In contrast, referring to Example 5 Fig.42 (d) and Fig.42(e), even after ADT was performed, the changes in the size and size distribution of the platinum (Pt) particles were significantly smaller than those in Comparative Example 5, where the average particle sizes after 30,000 (30k) cycles and 90,000 (90k) cycles were ∼3 nm and ∼4.5 nm, respectively. This result occurs because the inclusion of silver (Ag) particles in the gas diffusion layer can prevent the active metal particles of the catalyst layer from being oxidized and agglomerated.

[0281] Fig.43 are graphs showing a high angle annular dark field scanning transmission electron microscope (HAADF-STEM, FEI Themis Z) image of the catalyst layer included in Example 5 after 90,000 (90k) cycles, a corresponding EDS mapping image, and an EDS spectrum. Fig.44 is a graph of the Ag 3d XPS spectrum according to the ADT cycle of the catalyst layer included in Example 5.

[0282] Reference Fig.43 and Fig.44 It is known that silver (Ag) ions formed by being oxidized during ADT do not deposit on active metal particles included in the catalyst layer or form an alloy, and no silver (Ag) is observed on the catalyst layer after performing ADT.

[0283] As described above, in this specification, the present disclosure is described through specific matters and limited embodiments, but this is only provided to help a more comprehensive understanding of the present disclosure. The present disclosure is not limited to the embodiments, and technicians in the field of the present disclosure can make various modifications and changes from these records.

[0284] Therefore, the concept described in this specification is not limited to the described embodiments, and all contents equivalent to or equivalently modified to the claims belong to the scope of the concept described in this specification.

Claims

1. A composite, characterized in that: include: Carbon support; Active metal particles; as well as sacrificial metal particles, which are oxidized or reduced to replace the active metal particles, Wherein, the active metal particles and the sacrificial metal particles are independently loaded on the carbon carrier.

2. The composite according to claim 1, wherein The active metal particles and the sacrificial metal particles do not form an alloy with each other.

3. The composite according to claim 1, wherein: The active metal particles include one or more metals selected from the group consisting of palladium, platinum, gold, ruthenium, rhodium, iridium, osmium and alloys thereof.

4. The composite according to claim 1, wherein The standard reduction potential of the metal included in the sacrificial metal particles is lower than the standard reduction potential of the metal included in the active metal particles.

5. The composite according to claim 1, wherein: The sacrificial metal particles include one or more metals selected from the group consisting of: silver; palladium; iridium; ruthenium; rhodium; platinum; osmium; iron; aluminum and alloys thereof.

6. The composite according to claim 1, wherein The ratio D2 / D1 of the average particle size D2 of the active metal particles after 30,000 cycles of the accelerated durability test to the average particle size D1 of the active metal particles before the accelerated durability test is 3 or less.

7. The composite according to claim 1, wherein: The atomic ratio of the sacrificial metal included in the sacrificial metal particles to the active metal included in the active metal particles is 0.1 to 1:

50.

8. The composite according to claim 1, wherein: The active metal particles include platinum. In the X-ray diffraction energy spectra of the composite and pure platinum, the difference in 2θ value of the maximum peak appearing in the range of 2θ=39.8±1.0° is 0.3° or less.

9. The composite according to claim 1, wherein: The active metal particles include platinum. In the X-ray photoelectron spectroscopy of the Pt 4f 7 / 2 In the XPS spectrum, the peak intensity of Pt(0) I0 and the peak intensity of Pt(II) I II The ratio I0 / I II It is above 1.

8.

10. A method for manufacturing a composite body, comprising the following steps: preparing a first reaction solution, wherein the first reaction solution is prepared by mixing a dispersion containing a carbon support loaded with active metal particles and a solution containing a sacrificial metal precursor; and A composite body in which the active metal particles and the sacrificial metal particles are independently supported on the carbon support is synthesized by adding a reducing agent to the first reaction solution.

11. A method for manufacturing a composite body, comprising the following steps: preparing a second reaction solution, the second reaction solution being prepared by mixing a dispersion containing a carbon support loaded with active metal particles and a dispersion containing a carbon support loaded with sacrificial metal particles; and The sacrificial metal particles and a composite in which the sacrificial metal particles are independently supported on the carbon support are synthesized by adding a reducing agent to the second reaction solution.

12. A membrane electrode assembly, characterized in that: include: a cathode including a first catalyst layer and a first gas diffusion layer; an anode including a second catalyst layer and a second gas diffusion layer; as well as A polymer electrolyte membrane is arranged between the cathode and the anode, Wherein, the first catalyst layer comprises active metal particles, The first gas diffusion layer includes: a first gas diffusion layer support; and sacrificial metal particles supported on the first gas diffusion layer support and oxidized or reduced to replace the active metal particles.

13. The membrane electrode assembly according to claim 12, wherein: A surface of the first gas diffusion support body on which the sacrificial metal particles are located faces a surface of the first catalyst layer.

14. The membrane electrode assembly according to claim 12, wherein: The second catalyst layer includes active metal particles, The second gas diffusion layer includes: a second gas diffusion layer support; and sacrificial metal particles that are supported on the second gas diffusion layer support and are oxidized or reduced to replace the active metal particles.

15. The membrane electrode assembly according to claim 12, wherein: The active metal particles include one or more metals selected from the group consisting of palladium, platinum, gold, ruthenium, rhodium, iridium, osmium and alloys thereof.

16. The membrane electrode assembly according to claim 12, wherein: The standard reduction potential of the metal included in the sacrificial metal particles is lower than the standard reduction potential of the metal included in the active metal particles.

17. The membrane electrode assembly according to claim 12, wherein: The sacrificial metal particles include one or more metals selected from the group consisting of: silver; palladium; iridium; ruthenium; rhodium; platinum; osmium; iron; aluminum and alloys thereof.

18. The membrane electrode assembly according to claim 12, wherein: A ratio D2 / D1 of an average particle size D2 of the active metal particles after 30,000 cycles of the accelerated durability test to an average particle size D1 of the active metal particles before the accelerated durability test is 3 or less.

19. The membrane electrode assembly according to claim 12, wherein: An atomic ratio of a sacrificial metal included in the sacrificial metal particles included in the first gas diffusion layer to an active metal included in the active metal particles included in the first catalyst layer is 0.1:1 to 100:

1.

20. The membrane electrode assembly according to claim 12, wherein: The active metal particles include platinum. In a Pt 4f XPS spectrum based on X-ray photoelectron spectroscopy, a ratio I2 / I1 of a Pt(II) peak intensity I2 of the first catalyst layer after 90,000 cycles of an accelerated durability test to a Pt(II) peak intensity I1 before the accelerated durability test is 0.5 or more.

21. The membrane electrode assembly according to claim 12, wherein: The content of the sacrificial metal particles per unit area of ​​the first gas diffusion layer support body is 0.1 mg / cm 2 Up to 100mg / cm 2 .

22. A method for manufacturing a membrane electrode assembly, comprising the following steps: The first step is to dope a sacrificial metal precursor on a first gas diffusion layer support; The second step is to manufacture a first gas diffusion layer having sacrificial metal particles supported on the first gas diffusion layer support by reducing the sacrificial metal precursor doped on the first gas diffusion layer support; The third step is to form a first catalyst layer on a surface of the polymer electrolyte membrane; The fourth step is to form a second catalyst layer on the other surface of the polymer electrolyte membrane; The fifth step is to form the first gas diffusion layer on the first catalyst layer; as well as In a sixth step, a second gas diffusion layer is formed on the second catalyst layer.

23. A fuel cell electrode, comprising: The complex according to claim 1.

24. A fuel cell comprising: The membrane electrode assembly according to claim 12; or The fuel cell electrode according to claim 23.