Catalyst slurry and preparation method thereof, preparation method of catalyst coating membrane, and membrane electrode
By rationally formulating the catalyst and solvent in the catalyst slurry, and performing appropriate crushing and degassing treatments, the problems of cracks and poor coverage of the catalyst coating membrane during the coating process are solved, and the electrochemical performance of the membrane electrode is improved. and service life.
Patent Information
- Application Number
- CN202310338783.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
Existing catalyst slurries are prone to cracks and poor coverage during the coating process, resulting in shortened membrane electrode life and deterioration in quality.
By mixing the catalyst, water and n-propanol, performing ball milling and degassing treatment, a catalyst slurry with a solid content of 5 to 20% is prepared, and hot plate or hot air drying is performed on the proton exchange membrane to avoid cracks and coverage. Bad question.
The ductility and stability of the catalyst slurry are improved, the service life of the membrane electrode is extended, and its electrochemical performance is improved.
Smart Images

Figure BDA0004157408930000071 
Figure BDA0004157408930000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of membrane electrodes, and in particular to a catalyst slurry and a preparation method thereof, a preparation method of a catalyst coating membrane, and a membrane electrode. Background Art
[0002] As the core component of proton exchange membrane fuel cells, membrane electrode is usually composed of catalyst-coated membrane (including proton exchange membrane and anode and cathode catalyst layers coated thereon) and anode and cathode gas diffusion layers. Among them, the preparation process of anode and cathode catalyst layers is directly related to the electrochemical catalytic performance of membrane electrode, and the preparation process of catalyst slurry directly determines the performance of anode and cathode catalyst layers.
[0003] In the prior art, researchers have reported that increasing the water content in the catalyst slurry solvent helps to improve the ductility of the adhesive resin in the catalyst slurry, thereby improving the performance of the catalyst slurry. However, an inappropriate water-to-alcohol ratio combined with an inappropriate heating method will cause the catalyst slurry to have cracks in the catalyst layer and poor coverage when the catalyst slurry is coated to obtain a catalyst-coated membrane, and the life of the membrane electrode will be greatly shortened and the quality will deteriorate. Based on this, it is necessary to provide a catalyst slurry to improve the above problems. Summary of the invention
[0004] The main purpose of the present invention is to provide a catalyst slurry and a preparation method thereof, a preparation method of a catalyst coated membrane, and a membrane electrode, so as to solve the problem that when the existing catalyst slurry is coated to obtain a catalyst coated membrane, the catalytic layer has cracks and poor coverage.
[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a catalyst slurry is provided, and the preparation method comprises the following steps: step S1, mixing a catalyst, water, n-propanol and a resin dispersion to obtain a pre-dispersed catalyst slurry; step S2, successively crushing and degassing the pre-dispersed catalyst slurry to obtain a catalyst slurry; wherein the catalyst comprises a carrier and an active component loaded on the carrier, the carrier is graphite carbon, and the active component is selected from one or more of Pt, Pt-Co alloy or Pt-Ni alloy; the weight ratio of water to n-propanol is (0.5-0.9):1.
[0006] Furthermore, the crushing method is selected from one or more of ball milling, ultrasonic crushing or high-pressure crushing, and ball milling is more preferred; preferably, the material of the grinding balls used in ball milling is selected from one or more of zirconium oxide, aluminum oxide, tungsten carbide, and polytetrafluoroethylene; preferably, the equipment used in ball milling is selected from one or more of planetary ball mills, centrifugal ball mills, drum ball mills, stirred ball mills, or vibrating ball mills; preferably, the average diameter of the grinding balls is 1 to 10 mm.
[0007] Furthermore, in the catalyst, the loading of the active component is 20 to 60 wt %; preferably, the resin in the resin dispersion is selected from one or more of perfluorosulfonic acid resin, partially fluorinated sulfonic acid resin or non-fluorinated sulfonic acid resin; preferably, the dispersant in the resin dispersion is water; preferably, the mass concentration of the resin in the resin dispersion is 5 to 30%; preferably, the weight ratio of the catalyst, n-propanol and resin dispersion is (0.03 to 0.14):1:(0.17 to 0.67).
[0008] Furthermore, the equipment used for degassing is selected from one or more of a stirring degassing machine, a planetary degassing machine or a centrifugal degassing machine; further preferably, the stirring degassing machine has a stirring speed of 200 to 1000 rpm and a processing time of 5 to 100 min.
[0009] In order to achieve the above object, according to one aspect of the present invention, a catalyst slurry is provided. The catalyst slurry is prepared by the above-mentioned method for preparing the catalyst slurry.
[0010] Furthermore, the solid content of the catalyst slurry is 5 to 20%; preferably, the solid content of the catalyst slurry is D 50 The particle size is 0.05~1μm.
[0011] According to another aspect of the present invention, a method for preparing a catalyst coated membrane is provided, the method for preparing a catalyst coated membrane comprising: coating and drying the aforementioned catalyst slurry on a proton exchange membrane in sequence to obtain a catalyst coated membrane; the drying method is selected from hot plate drying or hot air drying.
[0012] Furthermore, the drying treatment temperature is 30-100° C., and the treatment time is 3-20 min; preferably, when the weight ratio of water to n-propanol in the catalyst slurry is (0.5-0.75):1, the drying method is hot air drying; when the weight ratio of water to n-propanol in the catalyst slurry is (0.75-0.9):1, the drying method is hot plate drying; further preferably, the hot plate substrate used for hot plate drying is selected from one or more of a carbon plate, a metal plate or a ceramic plate.
[0013] Furthermore, the coating method is selected from one or more of blade coating, slit coating or roller coating, and blade coating is further preferred; preferably, the coating is carried out in a blade coater, and the operating speed of the blade coater is 0.5 to 10 m / min.
[0014] According to another aspect of the present invention, a membrane electrode is provided, comprising an anode gas diffusion layer, a catalyst-coated membrane and a cathode gas diffusion layer stacked in sequence, wherein the catalyst-coated membrane is prepared by the above-mentioned catalyst-coated membrane preparation method.
[0015] The present invention combines the above-mentioned carrier with the active component so that the two can work together better, thereby increasing the life of the catalyst while further improving the conductivity and mass transfer capacity of the membrane electrode prepared in the subsequent step of the catalyst slurry, thereby improving the electrochemical performance of the membrane electrode and extending the service life of the membrane electrode. DETAILED DESCRIPTION
[0016] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0017] As described in the background technology part of the present invention, when the existing catalyst slurry is coated to obtain a catalyst-coated membrane, the catalyst layer has cracks and poor coverage, and the life of the membrane electrode is greatly shortened and the quality deteriorates. In order to solve this problem, the present invention provides a method for preparing a catalyst slurry, which comprises the following steps: step S1, taking a catalyst, water, n-propanol and a resin dispersion to mix to obtain a pre-dispersed catalyst slurry; step S2, crushing and degassing the pre-dispersed catalyst slurry in turn to obtain a catalyst slurry. Among them, the catalyst includes a carrier and an active component loaded on the carrier, the carrier is graphite carbon, and the active component is selected from one or more of Pt, Pt-Co alloy or Pt-Ni alloy; the weight ratio of water to n-propanol is (0.5-0.9):1.
[0018] Those skilled in the art can first mix the catalyst, water, n-propanol and resin dispersion to obtain a pre-dispersed catalyst slurry; and then crush and degas the pre-dispersed catalyst slurry in turn to obtain a catalyst slurry. Among them, the catalyst used in the present invention includes a carrier and an active component loaded on the carrier, the carrier is graphite carbon, and the active component is selected from one or more of Pt, Pt-Co alloy or Pt-Ni alloy. The present invention matches the above-mentioned carrier with the active component so that the two can work better together, thereby improving the catalyst life while further improving the conductivity and mass transfer capacity of the catalyst slurry in the subsequent preparation of the membrane electrode, thereby improving the electrochemical performance of the membrane electrode and extending the service life of the membrane electrode.
[0019] Especially important is that the inventor found in the actual production process that the amount of water and n-propanol will affect the viscosity and ductility of the catalyst slurry, and then affect the performance of the catalyst slurry, especially with different types of organic alcohols is likely to cause the performance of the catalyst slurry to deteriorate further. And the present invention, in the preparation of pre-dispersed catalyst slurry, for the above-mentioned specific catalyst components, the weight ratio of water to n-propanol is limited to (0.5~0.9): 1 range, and the pre-dispersed catalyst slurry is successively broken and deaerated, thereby further improving the ductility of the catalyst slurry, avoiding the problem of cracks in the catalyst coating film and poor coverage of the catalyst slurry, and then making the membrane electrode performance more stable, improving its electrochemical performance and service life. In some optional embodiments, the weight ratio of water to n-propanol can be 0.5: 1, 0.6: 1, 0.7: 1, 0.8: 1 or 0.9: 1.
[0020] In a preferred embodiment, the crushing method is selected from ball milling, ultrasonic crushing or high-pressure crushing, which can make the catalyst slurry more evenly dispersed, thereby improving the performance of the catalyst slurry; the more preferred crushing method is ball milling. In order to further improve the dispersion uniformity of ball milling, so that the catalyst slurry is more stable and has better performance, the grinding ball material used in ball milling is preferably selected from one or more of zirconium oxide, aluminum oxide, tungsten carbide, and polytetrafluoroethylene; the average diameter of the grinding ball is 1 to 10 mm, for example, it can be 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm or 10 mm. In order to further balance the preparation cost and performance of the catalyst slurry and further improve the prospects for industrial application of the catalyst slurry, the equipment used for ball milling is preferably selected from one or more of a planetary ball mill, a centrifugal ball mill, a drum ball mill, a stirring ball mill or a vibrating ball mill.
[0021] It is further explained that the above ball mill crushing means: crushing by collision between medium and particles under the action of centrifugal force and friction. The above ultrasonic crushing means: thorough mixing of solid and liquid through ultrasonic cavitation of liquid. The above high pressure crushing means: when high pressure fluid passes through the fine pore module under pressure, the pressure drops sharply to form ultrasonic flow rate, at which time particle impact, cavitation, turbulence and shear will occur in the fluid, causing the fluid to be destroyed, atomized, emulsified and dispersed.
[0022] In order to further improve the service life of the catalyst, promote the conductivity and mass transfer capacity of the membrane electrode prepared by the catalyst slurry in the subsequent preparation, and then improve the electrochemical performance of the membrane electrode and extend the service life of the membrane electrode, preferably, in the catalyst, the loading of the active component is 20-60wt%, for example, it can be 20wt%, 30wt%, 40wt%, 50wt% or 60wt%. In order to further improve the ductility of the catalyst slurry and reduce the crack phenomenon of the catalyst coating film, the resin in the resin dispersion is preferably selected from perfluorosulfonic acid resin, partially fluorinated sulfonic acid resin or non-fluorinated sulfonic acid resin. The dispersant in the resin dispersion is preferably water, and the mass concentration of the resin dispersion is further preferably 5-30%, for example, it can be 5%, 10%, 15%, 20%, 25% or 30%. In order to further improve the stability of the pre-dispersed catalyst slurry, the weight ratio of the catalyst, n-propanol and resin dispersion is preferably (0.03-0.14): 1: (0.17-0.67).
[0023] In order to further remove the bubbles remaining in the crushed material, thereby avoiding the influence of bubbles on the performance of the catalyst slurry, and then reducing the phenomenon of cracks in the catalyst coating film and the poor coating rate of the catalyst slurry, the degassing equipment is preferably selected from one or more of a stirring degassing machine, a planetary degassing machine or a centrifugal degassing machine, and a stirring degassing machine is further preferred. In order to further improve the stability of the catalyst slurry and avoid the influence of bubbles on its performance, the stirring speed in the stirring degassing machine is preferably 200 to 1000 rpm, and the processing time is 5 to 100 min, for example, it can be 200 rpm / 5 min, 400 rpm / 25 min, 600 rpm / 50 min, 800 rpm / 75 min or 1000 rpm / 100 min.
[0024] Another aspect of the present invention further provides a catalyst slurry, which is prepared by the above-mentioned catalyst slurry preparation method. The catalyst slurry obtained by the catalyst slurry preparation method of the present invention can effectively avoid the problems of cracks and poor catalyst slurry coverage when preparing a catalyst coating membrane in the subsequent preparation. The membrane electrode performance is more stable, and its electrochemical performance is better and the service life is longer.
[0025] In a preferred embodiment, the solid content of the catalyst slurry is 5-20%, for example, 5%, 10%, 15% or 20%; the solid material D in the catalyst slurry is 50 The particle size is 0.05 to 1 μm. In this way, the stability and uniformity of the catalyst slurry can be further improved, so that the performance of the catalyst slurry is better, so that the catalyst coating membrane prepared by it can avoid cracks and have a higher coverage rate, thereby making the electrochemical performance of the membrane electrode better and the service life longer.
[0026] Another aspect of the present invention also provides a method for preparing a catalyst coated membrane, which comprises: coating and drying the above-mentioned catalyst slurry on a proton exchange membrane in sequence to obtain a catalyst coated membrane; the drying method is selected from hot plate drying or hot air drying.
[0027] Those skilled in the art can take the above-mentioned catalyst slurry and apply and dry it on the proton exchange membrane in sequence to obtain a catalyst-coated membrane. As mentioned above, the catalyst slurry obtained by the preparation method of the present invention has excellent performance, and the catalyst-coated membrane prepared by applying and drying it on the proton exchange membrane in sequence has excellent stability and uniformity, and cracks are not easy to appear on the surface of the catalyst-coated membrane, and the coverage of the catalyst slurry on the above-mentioned catalyst-coated membrane is excellent, so that the membrane electrode prepared subsequently has excellent electrochemical properties and the advantages of a long service life. In particular, the above-mentioned catalyst slurry of the present application is used in combination with a specific hot plate drying or hot air drying method for drying, which can further significantly avoid the phenomenon of cracks in the catalyst-coated membrane, make the coating of the catalyst slurry more uniform and stable, and the coverage of the catalyst slurry on the catalyst-coated membrane is excellent, and the comprehensive performance of the membrane electrode is better.
[0028] In a preferred embodiment, when the weight ratio of water to n-propanol in the catalyst slurry is (0.5-0.75): 1, the drying method is hot air drying; when the weight ratio of water to n-propanol in the catalyst slurry is (0.75-0.9): 1, the drying method is hot plate drying. The specific water-to-alcohol ratio is matched with a specific hot plate drying or hot air drying method for drying, which can further greatly avoid the phenomenon of cracks in the catalyst coating film, make the coating of the catalyst slurry more uniform and stable, and the coverage of the catalyst slurry on the catalyst coating film is better, and the comprehensive performance of the membrane electrode is better. The use of hot plate drying with a high water-to-alcohol ratio is conducive to quickly removing the solvent in the coating and preventing swelling. When hot air drying is used, due to the gas flow on the surface of the coating, the catalyst slurry flows unevenly during the drying process, resulting in poor performance of the catalyst coating film and poor performance of the membrane electrode. It is further preferred that the drying treatment temperature is 30-100°C and the treatment time is 3-20min.
[0029] It is further explained that the above-mentioned hot air drying refers to a method of drying the material to be dried by blowing hot air into the material in an oven or drying chamber. Hot plate drying refers to a method of placing the material to be dried on a hot plate base and drying the material by heating the hot plate base. In some optional embodiments, the hot plate base can be set at the bottom between two reels of roll-to-roll coating; or, the hot plate base can be directly used as a conveyor belt to heat the material while transporting the material; or, the material to be dried passes through one or more heated rollers (i.e., the hot plate base) before winding to be dried.
[0030] In a preferred embodiment, the hot plate substrate used for hot plate drying is selected from one or more of a carbon plate, a metal plate, and a ceramic plate, so that the catalyst slurry can have better ductility on the hot plate substrate, making the subsequent catalyst coating film preparation process more stable and avoiding cracks.
[0031] In order to further improve the performance of the catalyst-coated membrane prepared by the catalyst slurry, the preferred coating method is selected from one or more of blade coating, slit coating or roller coating, and blade coating is further preferred. In order to further avoid cracks in the catalyst slurry-coated membrane and improve the stability of the catalyst-coated membrane, the coating is preferably carried out in a blade coater, and the operating speed of the blade coater is 0.5 to 10 m / min, more preferably 4 to 10 m / min. In order to further increase the coverage of the catalyst slurry on the catalyst-coated membrane and improve the performance of the catalyst-coated membrane, it is necessary to perform a standing treatment after coating and before drying, and it is further preferred that the standing treatment time is 10 to 60 seconds.
[0032] Another aspect of the present invention further provides a membrane electrode, comprising an anode gas diffusion layer, a catalyst-coated membrane and a cathode gas diffusion layer stacked in sequence, wherein the catalyst-coated membrane is prepared by the above-mentioned catalyst-coated membrane preparation method. As mentioned above, the membrane electrode prepared by the present invention has good electrochemical performance and a long service life, and has excellent comprehensive performance.
[0033] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0034] Example 1
[0035] The catalyst, water, n-propanol and resin dispersion are mixed to obtain a pre-dispersed catalyst slurry, wherein the catalyst carrier is graphite carbon, the active component is Pt, the loading amount of the active component is 50wt%, the weight ratio of water to n-propanol is 0.6:1, the resin dispersion is an aqueous solution of perfluorosulfonic acid resin, the mass concentration of the resin in the resin dispersion is 26%, and the weight ratio of the catalyst, n-propanol and resin dispersion is 0.107:1:0.205. Then the pre-dispersed catalyst slurry is placed in a planetary ball mill for ball milling, and the grinding ball material used is selected from ZrO 2 The average diameter of the grinding balls is 1 mm. The crushed material is then degassed in a stirring degasser, first at a stirring speed of 1000 rpm for 10 minutes, and then at a stirring speed of 400 rpm for 5 minutes to obtain a catalyst slurry. The solid content of the catalyst slurry is 10%; the solid D50 particle size in the catalyst slurry is 0.172 μm.
[0036] The catalyst slurry is coated and dried on the proton exchange membrane in sequence by using a blade coating machine with a running speed of 4 m / min. The catalyst slurry is dried by hot air drying at a drying temperature of 60°C and a drying time of 6 min to obtain a catalyst coating membrane.
[0037] Example 2
[0038] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.9:1.
[0039] Example 3
[0040] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.5:1.
[0041] Example 4
[0042] The only difference from Example 1 is that the average diameter of the grinding balls is 3 mm.
[0043] Example 5
[0044] The only difference from Example 1 is that the average diameter of the grinding balls is 10 mm.
[0045] Example 6
[0046] The only difference from Example 1 is that the temperature of the hot plate drying is 30°C.
[0047] Example 7
[0048] The only difference from Example 1 is that the temperature of the hot plate drying is 100°C.
[0049] Example 8
[0050] The only difference from Example 1 is that the drying method is selected from hot plate drying.
[0051] Example 9
[0052] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.7:1.
[0053] Example 10
[0054] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.8:1.
[0055] Embodiment 11
[0056] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.7:1, and the drying method is selected from hot air drying.
[0057] Example 12
[0058] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.8:1, and the drying method is selected from hot air drying.
[0059] Embodiment 13
[0060] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.5:1, and the drying method is selected from hot air drying.
[0061] Embodiment 14
[0062] The only difference from Example 1 is that the weight ratio of water to n-propanol is 0.9:1, and the drying method is selected from hot air drying.
[0063] Comparative Example 1
[0064] The only difference from Example 8 is that the weight ratio of water to n-propanol is 0.2:1.
[0065] Comparative Example 2
[0066] The only difference from Example 1 is that no n-propanol was added.
[0067] Comparative Example 3
[0068] The only difference from Example 1 is that the average diameter of the grinding balls used is 20 mm.
[0069] Comparative Example 4
[0070] The only difference from Example 8 is that the weight ratio of water to n-propanol is 0.4:1.
[0071] Comparative Example 5
[0072] The only difference from Example 8 is that the weight ratio of water to n-propanol is 0.9:1.
[0073] Performance Test:
[0074] (1) Coverage test
[0075] The catalyst coating films prepared in the examples and comparative examples were photographed under a microscope (Zeiss A1 metallographic microscope), and the photographs taken under the microscope were processed using image processing software ImageJ. The coverage calculation function of the software was used to integrate and obtain the percentage of the covered area of the catalytic layer to the entire catalytic layer area.
[0076] The specific performance test results are shown in Table 1.
[0077] Table 1
[0078]
[0079]
[0080] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0081] From the test results of Example 8 and Comparative Examples 2, 3, 4, and 5, it can be found that when the catalyst slurry preparation method of the present invention is adopted, wherein the weight ratio of water to n-propanol is within the range of (0.5 to 0.9): 1 (for example, 0.6: 1 in Example 8), the prepared catalyst coating film has a good coverage rate, and there are no cracks on the surface, and the membrane electrode prepared therefrom has a long service life and excellent electrochemical performance. When the weight ratio of water to n-propanol is outside the range of (0.5 to 0.9): 1 (for example, 0.2: 1 in Comparative Example 2, n-propanol is not added in Comparative Example 3, 0.4: 1 in Comparative Example 4, and 0.9: 1 in Comparative Example 5), due to the poor ductility of the ionomer in a solvent with a high water content, the catalyst cannot be uniformly coated, resulting in poor performance of the catalyst slurry, poor coverage of the prepared catalyst coating film, and poor membrane electrode performance.
[0082] From the test results of Examples 1, 4, 5 and Comparative Example 3, it can be found that when the catalyst slurry preparation method of the present invention is used, wherein the average diameter of the grinding balls used is within the range of 1 to 10 mm (e.g., 1 mm in Example 1, 3 mm in Example 4, and 10 mm in Example 5), the prepared catalyst coating membrane has a good coverage rate, and the membrane electrode prepared therefrom has a long service life and excellent electrochemical performance. However, when the average diameter of the grinding balls is outside the range of 1 to 10 mm (e.g., 20 mm in Comparative Example 3), due to the large grinding ball size, the grinding force on the catalyst particles is low, and some catalyst agglomerates are not completely dispersed, resulting in poor catalyst slurry performance, poor catalyst coating membrane and membrane electrode performance.
[0083] From the test results of Examples 1-3 and 8-10, it can be found that when the weight ratio of water to n-propanol in the catalyst slurry is (0.5-0.75):1, the drying method is hot air drying; when the weight ratio of water to n-propanol in the catalyst slurry is (0.75-0.9):1, the drying method is hot plate drying. The specific water-to-alcohol ratio is matched with a specific hot plate drying or hot air drying method for drying, which can further significantly avoid the phenomenon of cracks in the catalyst coating film, make the coating of the catalyst slurry more uniform and stable, and the coverage of the catalyst slurry on the catalyst coating film is better, and the comprehensive performance of the membrane electrode is better.
[0084] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst slurry, characterized in that: The preparation method comprises the following steps: Step S1, mixing a catalyst, water, n-propanol and a resin dispersion to obtain a pre-dispersed catalyst slurry; Step S2, crushing and degassing the pre-dispersed catalyst slurry in sequence to obtain the catalyst slurry; The catalyst comprises a carrier and an active component supported on the carrier, the carrier is graphite carbon, and the active component is selected from one or more of Pt, Pt-Co alloy or Pt-Ni alloy; The weight ratio of water to n-propanol is (0.5-0.9):
1.
2. The method for preparing the catalyst slurry according to claim 1, characterized in that: The crushing method is selected from one or more of ball milling, ultrasonic crushing or high-pressure crushing, and the ball milling is more preferred; Preferably, the material of the grinding balls used in the ball milling is selected from one or more of zirconium oxide, aluminum oxide, tungsten carbide and polytetrafluoroethylene; Preferably, the equipment used for the ball milling is selected from one or more of a planetary ball mill, a centrifugal ball mill, a drum ball mill, a stirring ball mill or a vibrating ball mill; Preferably, the average diameter of the grinding balls is 1 to 10 mm.
3. The method for preparing the catalyst slurry according to claim 1 or 2, characterized in that: In the catalyst, the loading amount of the active component is 20 to 60 wt%; Preferably, the resin in the resin dispersion is selected from one or more of a perfluorinated sulfonic acid resin, a partially fluorinated sulfonic acid resin or a non-fluorinated sulfonic acid resin; Preferably, the dispersant in the resin dispersion is water; Preferably, the mass concentration of the resin in the resin dispersion is 5 to 30%; Preferably, the weight ratio of the catalyst, the n-propanol and the resin dispersion is (0.03-0.14): 1: (0.17~0.67)。 4. The method for preparing a catalyst slurry according to any one of claims 1 to 3, characterized in that: The deaerator is selected from one or more of a stirring deaerator, a planetary deaerator or a centrifugal deaerator; preferably a stirring deaerator; More preferably, the stirring speed in the stirring deaerator is 200 to 1000 rpm, and the processing time is 5 to 100 min.
5. A catalyst slurry, characterized in that: The catalyst slurry is prepared by the method for preparing the catalyst slurry according to any one of claims 1 to 4.
6. The catalyst slurry according to claim 5, characterized in that The solid content of the catalyst slurry is 5 to 20%; Preferably, the D of the solid material in the catalyst slurry is 50 The particle size is 0.05~1μm.
7. A method for preparing a catalyst coating membrane, characterized in that: The method for preparing the catalyst coating membrane comprises: The catalyst slurry according to claim 5 or 6 is sequentially coated and dried on a proton exchange membrane to obtain the catalyst coated membrane; The drying method is selected from hot plate drying or hot air drying.
8. The method for preparing a catalyst coating membrane according to claim 7, characterized in that: The drying process temperature is 30-100°C and the process time is 3-20min; Preferably, when the weight ratio of water to n-propanol in the catalyst slurry is (0.5-0.75):1, the drying method is hot air drying; when the weight ratio of water to n-propanol in the catalyst slurry is (0.75-0.9):1, the drying method is hot plate drying; Further preferably, the hot plate substrate used in the hot plate drying is selected from one or more of a carbon plate, a metal plate or a ceramic plate.
9. The method for preparing a catalyst coating membrane according to claim 7 or 8, characterized in that: The coating method is selected from one or more of blade coating, slit coating or roller coating, and is more preferably blade coating; Preferably, the coating is carried out in a blade coater, and the operating speed of the blade coater is 0.5 to 10 m / min.
10. A membrane electrode, comprising an anode gas diffusion layer, a catalyst coating membrane and a cathode gas diffusion layer stacked in sequence, characterized in that: The catalyst-coated membrane is prepared by the method for preparing a catalyst-coated membrane according to any one of claims 7 to 9.
Citation Information
Cited By
Preparation method of ceramic slurry for solid-state battery
CN119419344A