Positive electrode and negative electrode vanadium electrolyte based on composite acid medium and preparation method of positive electrode and negative electrode vanadium electrolyte
By using composite acid medium and composite additives in the vanadium electrolyte, the problem of instability of the vanadium electrolyte at high temperatures and the penetration of vanadium ions is solved, thereby improving the performance of the vanadium battery and broadening the temperature range.
Patent Information
- Application Number
- CN202410940645.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
AI Technical Summary
The existing vanadium electrolyte is unstable in high-temperature environments and easily generates precipitation of vanadium compounds, resulting in a decrease in the capacity and efficiency of vanadium batteries. In addition, the amount of vanadium ions permeating across the membrane is large, affecting battery performance.
The positive and negative vanadium electrolytes based on composite acid media are used. By adjusting the molar ratio of sulfuric acid and phosphoric acid and using composite additives, the stability and solubility of vanadium ions are improved, the aggregation and precipitation of vanadium ions are prevented, and the electrochemical performance is improved.
It broadens the applicable temperature range of vanadium electrolyte, improves high temperature stability and long-term operating performance of electrolyte, reduces capacity and efficiency losses, and achieves efficient vanadium electrolyte performance.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of vanadium electrolyte, and specifically relates to a positive electrode and a negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. Background Art
[0002] The all-vanadium liquid redox battery (VRFB) is one of the fastest-growing large-scale, long-term energy storage technologies. Due to the flow of the electrolyte and the heat dissipation of the equipment, the electrolyte temperature will continue to rise. It has been found that if a 1KW vanadium battery is continuously operated, its electrolyte will exceed 50°C within 24 hours, which exceeds the applicable range of traditional electrolytes. In particular, the positive electrode electrolyte is unstable in a high temperature environment and is prone to generate vanadium pentoxide precipitation, which reduces the capacity and efficiency of the vanadium battery. In addition, vanadium ions permeate across the membrane from the negative electrode to the positive electrode. Therefore, the preparation of positive and negative electrode vanadium electrolytes with strong high-temperature stability and low vanadium ion permeation across the membrane is of great significance to improving the performance of vanadium batteries and expanding the application of vanadium batteries.
[0003] "An all-vanadium liquid flow battery electrolyte and its preparation method and application" (CN 113644304A) mixes vanadium oxide with sulfuric acid, activates and reduces with hydrogen, and obtains an all-vanadium electrolyte with a total concentration of 3-4-valent vanadium ions of 1.5-2 mol / L, which improves the preparation process and the influence of impurities. However, the energy efficiency of the prepared electrolyte is 70-83%, and precipitation and capacity loss will occur when the temperature is ≥40°C for a long time, so its high temperature, capacity, efficiency and other performances need to be further improved.
[0004] "An all-vanadium flow battery and its operation mode" (WO 2015 / 007204A1) uses at least one of sulfuric acid, sulfate, phosphoric acid, phosphate, pyrophosphate and polyphosphate as an additive, and reduces discharge energy decay and side reactions such as hydrogen evolution by changing the total vanadium content and voltage range of the positive and negative electrodes. The pentavalent vanadium electrolyte has a stability time of ≤4 days at 50°C, and the trivalent vanadium electrolyte has a stability time of >11 days at -20°C. The vanadium ion concentration is 1.66-1.83 mol / L, and the energy density is 12.7-18.5 Wh / L. The stability time is short, and the vanadium concentration and energy density are low.
[0005] The literature (Sarah Roe, Chris Menictas and Maria Skyllas-Kazacos. A high energy density vanadium redox flow battery with 3M vanadium electrolyte. Journal of The Electrochemical Society, 2016, 163(1): A5023-A5028.) uses potassium phosphate, phosphoric acid and ammonium sulfate as composite additives to increase the applicable temperature range of high-concentration vanadium electrolyte. However, in the presence of the additives, a 3 mol / L pentavalent vanadium solution can only be stable for a few days at 50° C., and the utilization rate of active substances is only 62%. The prepared vanadium electrolyte has problems of instability and low performance.
[0006] "A method for preparing vanadium battery electrolyte by coupled reaction electrolysis" (CN 115418653 A) uses hexamethylenetetramine, or urine urea, methanol, ethanol, hydroxylamine hydrochloride or hydroxylamine sulfate oxidation and other half reactions to replace the acidic oxygen evolution half reaction in the traditional electrolysis method to prepare a 1.6 mol / L vanadium electrolyte, which reduces the voltage required in the whole electrolysis reaction process, saves costs, and broadens the electrolysis ideas. However, the scope or performance of the vanadium battery electrolyte suitable for preparation is not clear, the listed vanadium electrolyte concentration is low, and there is ion transmembrane and active material loss during the electrolysis process.
[0007] In summary, the existing vanadium electrolyte and its preparation method have the problems of high temperature precipitation of vanadium ions, narrow applicable temperature, low performance of vanadium electrolyte and attenuation of capacity and efficiency performance. Summary of the invention
[0008] The present invention aims to overcome the defects of the prior art and aims to provide a positive and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof, which can prevent high-temperature precipitation of vanadium ions, has a wide applicable temperature range, has good vanadium electrolyte performance, and has small capacity and efficiency losses of the vanadium electrolyte.
[0009] To achieve the above purpose, the technical solution steps adopted by the present invention are as follows:
[0010] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0011] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1: (1.6-6.5), the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being (8-48): (10-100): 1, under continuous stirring, the temperature is started to be raised, and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 60-95° C., and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 4.0 or 5.0.
[0012] Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive is 100: (0.5-4), adding the composite additive to the positive electrolyte I under stirring conditions, stirring until the composite additive is completely dissolved, to obtain a positive electrolyte II.
[0013] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is (0.1-1):1; the positive electrode electrolyte II is electrolyzed by electrolysis to a valence state of vanadium ions of 3.5, or 4.0, or an intermediate valence state between 3.5 and 4.0, to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0014] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0015] Step 2.1, according to the mass ratio of vanadium compound to deionized water being 1: (1.6-6.5), the deionized water is added to the vanadium compound, stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being (3.2-48) : (4-100) : 1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 60-95° C., and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 4.0 or 5.0.
[0016] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I: composite additive is 100: (0.5-4), adding the composite additive to the negative electrode electrolyte I under stirring conditions, stirring until the composite additive is completely dissolved, to obtain negative electrode electrolyte II.
[0017] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is (0.1-1):1; the negative electrode electrolyte II is electrolyzed by electrolysis to a valence state of vanadium ions of 3.0, 3.5, or an intermediate valence state between 3.0 and 3.5, to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0018] The sulfuric acid, the phosphoric acid and the vanadium compound described in step 1.1 and step 2.1 are the same.
[0019] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 50 to 500 rpm.
[0020] The vanadium compound is one of vanadium pentoxide and vanadyl sulfate; the purity of the vanadium compound is ≥99%.
[0021] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 0.01 to 3% of the volume of the sulfuric acid or phosphoric acid to be added.
[0022] The mass fraction of the sulfuric acid is 90-98%.
[0023] The mass fraction of the phosphoric acid is 75-85%.
[0024] The composite additive is mixed in a molar ratio of type A additive to type B additive of 1:(0.01-3); wherein the type A additive is one of acetic acid and salicylic acid, and the type B additive is one of methanesulfonic acid, aminosulfonic acid and taurine.
[0025] In the electrolysis method, the voltage is 0.5 to 5.0 V and the current density is 20 to 500 A / m.
[0026] The electrocatalyst is one of amino acids, sugars, hydrazines, polysulfides, alcohols, aldehydes, polycarbons, quinone derivatives, formate and amine compounds; and the concentration of the electrocatalyst is 0.2-5.0 mol / L.
[0027] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6-2.4 mol / L; sulfuric acid is 2.0-5.0 mol / L; phosphoric acid is 0.05-0.20 mol / L.
[0028] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6-2.4 mol / L; sulfuric acid is 2.0-5.0 mol / L; phosphoric acid is 0.05-0.50 mol / L.
[0029] By adopting the above technical solution, the present invention has the following positive effects compared with the prior art:
[0030] 1. The present invention adopts sulfur-phosphorus composite acid medium, which can accelerate the dissolution rate of vanadium compounds and broaden the applicable temperature range of vanadium electrolyte. The composite acid medium has a strong dissolving ability, wherein the phosphate group coordinates with the vanadium ion, reduces the aggregation of free vanadium ions, improves the stability of vanadium ions in a high temperature environment, and can effectively prevent the occurrence of side reactions such as the dehydration condensation of vanadium ions to produce vanadium compound precipitation.
[0031] 2. The composite additive used in the present invention is a combination of a carboxyl compound and an ammonia / ammonium or sulfonic acid compound. The beneficial functional groups in the additive provide active sites for the redox reaction on the electrode surface, improving the electrochemical performance of the vanadium electrolyte. It also has coordination, adsorption, and dispersion effects on vanadium ions, increasing the radius of vanadium ions, reducing the permeation rate through the membrane during electrolysis and operation, and preventing the formation of vanadium phosphate and vanadium pentoxide precipitation, thereby improving the stability of the performance of the electrolyte during long-term operation and effectively reducing the electrolyte capacity and efficiency loss.
[0032] 3. The electrocatalyst used in the present invention accelerates the electrolysis rate, reduces the process energy consumption, cooperates with the positive and negative electrode electrolytes of the composite acid medium containing the composite additive, reduces the transmembrane loss, and ensures the performance of the vanadium electrolyte. The electrocatalyst adopts a low potential reaction compound (<1.1V), compared with the electrolysis of sulfuric acid solution to prepare the vanadium electrolyte, reduces the voltage value and the electrolysis process energy barrier required in the electrolysis full reaction process, preferentially electrolyzes, accelerates the electrolysis reaction rate, reduces the electrolysis time, and the free vanadium ions in the positive and negative electrode electrolytes of the composite acid medium containing the composite additive are reduced, the radius of the vanadium ion complex is larger, and the loss of vanadium ions and water in the electrolyte during electrolysis is also reduced, effectively improving the performance of the vanadium electrolyte.
[0033] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared by the present invention are tested: the static thermal stability time is 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 15 to 30 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density is 20 to 45Wh / L; the coulomb efficiency is ≥90%; and the energy efficiency is ≥70%.
[0034] Therefore, the positive and negative vanadium electrolytes based on the composite acid medium prepared by the present invention prevent high-temperature precipitation of vanadium ions, broaden the applicable temperature range, enhance the performance of the vanadium electrolyte, and reduce the loss of electrolyte capacity and efficiency performance. DETAILED DESCRIPTION
[0035] The present invention is further described below in conjunction with specific embodiments. However, the following embodiments are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0036] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof, the preparation method described in this specific embodiment is:
[0037] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0038] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1: (1.6-6.5), the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being (8-48): (10-100): 1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 60-95° C., and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 4.0 or 5.0.
[0039] Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive is 100: (0.5-4), adding the composite additive to the positive electrolyte I under stirring conditions, stirring until the composite additive is completely dissolved, to obtain a positive electrolyte II.
[0040] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is (0.1-1):1; the positive electrode electrolyte II is electrolyzed by electrolysis to a valence state of vanadium ions of 3.5, or 4.0, or an intermediate valence state between 3.5 and 4.0, to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0041] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0042] Step 2.1, according to the mass ratio of vanadium compound to deionized water being 1: (1.6-6.5), the deionized water is added to the vanadium compound, stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being (3.2-48) : (4-100) : 1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 60-95° C., and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 4.0 or 5.0.
[0043] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I: composite additive is 100: (0.5-4), adding the composite additive to the negative electrode electrolyte I under stirring conditions, stirring until the composite additive is completely dissolved, to obtain negative electrode electrolyte II.
[0044] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is (0.1-1):1; the negative electrode electrolyte II is electrolyzed by electrolysis to a valence state of vanadium ions of 3.0, 3.5, or an intermediate valence state between 3.0 and 3.5, to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0045] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 50 to 500 rpm.
[0046] The vanadium compound is one of vanadium pentoxide and vanadyl sulfate; the purity of the vanadium compound is ≥99%.
[0047] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 0.01 to 3% of the volume of the sulfuric acid or phosphoric acid to be added.
[0048] The mass fraction of the sulfuric acid is 90-98%.
[0049] The mass fraction of the phosphoric acid is 75-85%.
[0050] The composite additive is mixed in a molar ratio of type A additive to type B additive of 1:(0.01-3); wherein the type A additive is one of acetic acid and salicylic acid, and the type B additive is one of methanesulfonic acid, aminosulfonic acid and taurine.
[0051] In the electrolysis method, the voltage is 0.5 to 5.0 V and the current density is 20 to 500 A / m.
[0052] The electrocatalyst is one of amino acids, sugars, hydrazines, polysulfides, alcohols, aldehydes, polycarbons, quinone derivatives, formate and amine compounds; and the concentration of the electrocatalyst is 0.2-5.0 mol / L.
[0053] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6-2.4 mol / L; sulfuric acid is 2.0-5.0 mol / L; phosphoric acid is 0.05-0.20 mol / L.
[0054] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6-2.4 mol / L; sulfuric acid is 2.0-5.0 mol / L; phosphoric acid is 0.05-0.50 mol / L.
[0055] In this specific implementation mode:
[0056] The sulfuric acid, the phosphoric acid and the vanadium compound described in step 1.1 and step 2.1 are the same.
[0057] This will not be described in detail in the embodiments.
[0058] Example 1
[0059] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. The preparation method described in this embodiment is:
[0060] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0061] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1:1.6, the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being 48:100:1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 95°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 4.0.
[0062] Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive being 100:0.5, the composite additive is added to the positive electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain a positive electrolyte II.
[0063] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 1:1; the positive electrode electrolyte II is electrolyzed by electrolysis until the valence state of vanadium ion is 3.5, to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0064] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0065] Step 2.1, according to the mass ratio of vanadium compound to deionized water of 1:1.6, the deionized water is added to the vanadium compound, stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid of 48:100:1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 95°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 4.0.
[0066] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I: composite additive being 100:4, the composite additive is added into the negative electrode electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain negative electrode electrolyte II.
[0067] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 1:1; the negative electrode electrolyte II is electrolyzed by electrolysis until the valence state of vanadium ion is 3.5, to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0068] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 500 rpm.
[0069] The vanadium compound is vanadyl sulfate; the purity of the vanadium compound is 99.5%.
[0070] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 3% of the volume of the sulfuric acid or phosphoric acid to be added.
[0071] The mass fraction of the sulfuric acid is 98%.
[0072] The mass fraction of the phosphoric acid is 85%.
[0073] The composite additive is mixed according to the molar ratio of type A additive to type B additive of 1:0.01; wherein the type A additive is acetic acid and the type B additive is methane sulfonic acid.
[0074] In the electrolysis method, the voltage is 5.0 V and the current density is 20 A / m.
[0075] The electrocatalyst is an amino acid compound; the concentration of the electrocatalyst is 5.0 mol / L.
[0076] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: 2.4 mol / L of vanadium ions; 5.0 mol / L of sulfuric acid; and 0.05 mol / L of phosphoric acid.
[0077] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: 2.4 mol / L of vanadium ions; 5.0 mol / L of sulfuric acid; and 0.05 mol / L of phosphoric acid.
[0078] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this embodiment were tested: the static thermal stability time was 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 15 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density was 25-45Wh / L, the coulomb efficiency was 93%, and the energy efficiency was 80%.
[0079] Example 2
[0080] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. The preparation method described in this embodiment is:
[0081] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0082] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1:1.8, the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being 22:40:1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 80°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 4.0.
[0083] Step 1.2: adding the composite additive to the positive electrode electrolyte I at a molar ratio of vanadium ions to composite additive of 100:1 under stirring, and stirring until the composite additive is completely dissolved to obtain a positive electrode electrolyte II.
[0084] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.8:1; the positive electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.6 by electrolysis to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0085] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0086] Step 2.1, according to the mass ratio of vanadium compound to deionized water of 1:1.8, the deionized water is added to the vanadium compound, stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid of 15:27:1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 80°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 4.0.
[0087] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I: composite additive being 100:3, the composite additive is added into the negative electrode electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain negative electrode electrolyte II.
[0088] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.8:1; the negative electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.4 by electrolysis to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0089] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 400 rpm.
[0090] The vanadium compound is vanadyl sulfate; the purity of the vanadium compound is 99.0%.
[0091] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 2% of the volume of the sulfuric acid or phosphoric acid to be added.
[0092] The mass fraction of the sulfuric acid is 96%.
[0093] The mass fraction of the phosphoric acid is 80%.
[0094] The composite additive is mixed in a molar ratio of 1:1 between the type A additive and the type B additive; wherein the type A additive is acetic acid and the type B additive is aminosulfonic acid.
[0095] In the electrolysis method, the voltage is 1.5 V and the current density is 200 A / m.
[0096] The electrocatalyst is a sugar compound; the concentration of the electrocatalyst is 3.2 mol / L.
[0097] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: 2.2 mol / L of vanadium ions; 4.0 mol / L of sulfuric acid; and 0.10 mol / L of phosphoric acid.
[0098] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: 2.2 mol / L of vanadium ions; 4.0 mol / L of sulfuric acid; and 0.15 mol / L of phosphoric acid.
[0099] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this embodiment were tested: the static thermal stability time was 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 23 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density was 22-35Wh / L, the coulomb efficiency was 90%, and the energy efficiency was 75%.
[0100] Example 3
[0101] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. The preparation method described in this embodiment is:
[0102] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0103] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1:4.5, the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being 13:20:1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 70°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 5.0.
[0104] Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive being 100:2, the composite additive is added to the positive electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain a positive electrolyte II.
[0105] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.3:1; the positive electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.7 by electrolysis to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0106] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0107] Step 2.1, according to the mass ratio of vanadium compound to deionized water of 1:4.5, the deionized water is added to the vanadium compound, stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid of 6.5:10:1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 70°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 5.0.
[0108] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I: composite additive being 100:2, the composite additive is added to the negative electrode electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain negative electrode electrolyte II.
[0109] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.3:1; the negative electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.3 by electrolysis to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0110] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 300 rpm.
[0111] The vanadium compound is vanadium pentoxide; the purity of the vanadium compound is 99.5%.
[0112] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 1% of the volume of the sulfuric acid or phosphoric acid to be added.
[0113] The mass fraction of the sulfuric acid is 95%.
[0114] The mass fraction of the phosphoric acid is 80%.
[0115] The composite additive is mixed in a molar ratio of 1:2 between the type A additive and the type B additive; wherein the type A additive is salicylic acid and the type B additive is taurine.
[0116] In the electrolysis method, the voltage is 3.0 V and the current density is 300 A / m.
[0117] The electrocatalyst is an alcohol compound; the concentration of the electrocatalyst is 0.9 mol / L.
[0118] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: 2.0 mol / L of vanadium ions; 3.0 mol / L of sulfuric acid; and 0.15 mol / L of phosphoric acid.
[0119] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: 2.0 mol / L of vanadium ions; 3.0 mol / L of sulfuric acid; and 0.30 mol / L of phosphoric acid.
[0120] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this embodiment were tested: the static thermal stability time was 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 26 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density was 20-33Wh / L, the coulomb efficiency was 90%, and the energy efficiency was 70%.
[0121] Example 4
[0122] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. The preparation method described in this embodiment is:
[0123] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0124] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1:6.5, the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being 8:10:1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 60°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 5.0.
[0125] Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive being 100:4, the composite additive is added to the positive electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain a positive electrolyte II.
[0126] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.1:1; the positive electrode electrolyte II is electrolyzed by electrolysis until the valence state of vanadium ion is 4.0, to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0127] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0128] Step 2.1, according to the mass ratio of vanadium compound to deionized water of 1:6.5, the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution II; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid and phosphoric acid of 3.2:4:1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 60°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 5.0.
[0129] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I: composite additive being 100:0.5, the composite additive is added to the negative electrode electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain negative electrode electrolyte II.
[0130] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.1:1; the negative electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.0 by electrolysis to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0131] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 50 rpm.
[0132] The vanadium compound is vanadium pentoxide; the purity of the vanadium compound is 99.0%.
[0133] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 0.01% of the volume of the sulfuric acid or phosphoric acid to be added.
[0134] The mass fraction of the sulfuric acid is 90%.
[0135] The mass fraction of the phosphoric acid is 75%.
[0136] The composite additive is mixed in a molar ratio of 1:3 between the type A additive and the type B additive; wherein the type A additive is salicylic acid and the type B additive is methane sulfonic acid.
[0137] In the electrolysis method, the voltage is 0.5 V and the current density is 500 A / m.
[0138] The electrocatalyst is a hydrazine compound; the concentration of the electrocatalyst is 0.2 mol / L.
[0139] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6 mol / L; sulfuric acid is 2.0 mol / L; phosphoric acid is 0.20 mol / L.
[0140] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6 mol / L; sulfuric acid is 2.0 mol / L; phosphoric acid is 0.50 mol / L.
[0141] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this embodiment were tested: the static thermal stability time was 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 30 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density was 20-31Wh / L, the coulomb efficiency was 92%, and the energy efficiency was 83%.
[0142] Example 5
[0143] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. The preparation method described in this embodiment is:
[0144] Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium
[0145] Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1:2.4, the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being 11:21:1, under the condition of continued stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, the temperature is raised to 90°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 4.0.
[0146] Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive being 100:3, the composite additive is added to the positive electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain a positive electrolyte II.
[0147] Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.5:1; the positive electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.9 by electrolysis to obtain a positive electrode vanadium electrolyte based on a composite acid medium.
[0148] Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium
[0149] Step 2.1, according to the mass ratio of vanadium compound to deionized water of 1:2.4, the deionized water is added to the vanadium compound, stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid and phosphoric acid of 18:35:1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, the temperature is raised to 90°C, and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 4.0.
[0150] Step 2.2, according to the molar ratio of vanadium ions in negative electrode electrolyte I to composite additive being 100:1, the composite additive is added to the negative electrode electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain negative electrode electrolyte II.
[0151] Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is 0.5:1; the negative electrode electrolyte II is electrolyzed to a vanadium ion valence of 3.1 by electrolysis to obtain a negative electrode vanadium electrolyte based on a composite acid medium.
[0152] The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 150 rpm.
[0153] The vanadium compound is vanadyl sulfate; the purity of the vanadium compound is 99.9%.
[0154] The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 0.5% of the volume of the sulfuric acid or phosphoric acid to be added.
[0155] The mass fraction of the sulfuric acid is 98%.
[0156] The mass fraction of the phosphoric acid is 85%.
[0157] The composite additive is mixed in a molar ratio of 1:0.1 between the type A additive and the type B additive; wherein the type A additive is salicylic acid and the type B additive is methane sulfonic acid.
[0158] In the electrolysis method, the voltage is 4.0 V and the current density is 400 A / m.
[0159] The electrocatalyst is a polysulfide compound; the concentration of the electrocatalyst is 1.7 mol / L.
[0160] The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.8 mol / L; sulfuric acid is 3.5 mol / L; phosphoric acid is 0.17 mol / L.
[0161] The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.8 mol / L; sulfuric acid is 3.5 mol / L; phosphoric acid is 0.10 mol / L.
[0162] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this embodiment were tested: the static thermal stability time was 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 30 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density was 22-32Wh / L; the coulomb efficiency was 91%; and the energy efficiency was 78%.
[0163] Example 6
[0164] A positive electrode and negative electrode vanadium electrolyte based on a composite acid medium and a preparation method thereof. The preparation method described in this embodiment is: the following electrocatalysts are used in any one of Examples 1 to 5 respectively.
[0165] The electrocatalyst is one of aldehydes, polycarbons, quinone derivatives, formate and amine compounds.
[0166] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this embodiment are tested: the static thermal stability time is 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 15 to 30 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density is 22 to 43Wh / L; the coulomb efficiency is ≥91%; and the energy efficiency is ≥78%.
[0167] Compared with the prior art, this specific implementation has the following positive effects:
[0168] 1. This specific embodiment uses a sulfur-phosphorus composite acid medium, which can accelerate the dissolution rate of vanadium compounds and broaden the applicable temperature range of vanadium electrolyte. The composite acid medium has a strong dissolving ability, in which phosphates coordinate with vanadium ions, reduce the aggregation of free vanadium ions, improve the stability of vanadium ions in a high temperature environment, and effectively prevent the occurrence of side reactions such as the dehydration condensation of vanadium ions to produce vanadium compound precipitation.
[0169] 2. The composite additive used in this specific embodiment is a combination of a carboxyl compound and an ammonia / ammonium group or sulfonic acid group compound. The beneficial functional groups in the additive provide active sites for the redox reaction on the electrode surface, improving the electrochemical performance of the vanadium electrolyte. It also has coordination, adsorption, and dispersion effects on vanadium ions, increasing the radius of vanadium ions, reducing the permeation rate through the membrane during electrolysis and operation, and preventing the formation of vanadium phosphate and vanadium pentoxide precipitation, thereby improving the stability of the performance of the electrolyte during long-term operation and effectively reducing the electrolyte capacity and efficiency losses.
[0170] 3. The electrocatalyst used in this specific embodiment accelerates the electrolysis rate, reduces the process energy consumption, cooperates with the positive and negative electrode electrolytes of the composite acid medium containing the composite additive, reduces the transmembrane loss, and ensures the performance of the vanadium electrolyte. The electrocatalyst uses a low potential reaction compound (<1.1V), compared with the electrolysis of sulfuric acid solution to prepare the vanadium electrolyte, reduces the voltage value and the electrolysis process energy barrier required in the whole electrolysis reaction process, preferentially electrolyzes, accelerates the electrolysis reaction rate, reduces the electrolysis time, and the free vanadium ions in the positive and negative electrode electrolytes of the composite acid medium containing the composite additive are reduced, the radius of the vanadium ion complex is larger, and the loss of vanadium ions and water in the electrolyte during electrolysis is also reduced, effectively improving the performance of the vanadium electrolyte.
[0171] The positive electrode vanadium electrolyte and the negative electrode vanadium electrolyte based on the composite acid medium prepared in this specific embodiment have been tested: the static thermal stability time is 30 days at -20°C for the trivalent negative electrode vanadium electrolyte, and 15 to 30 days at 50°C for the pentavalent positive electrode vanadium electrolyte; within 100 charge and discharge cycles: the energy density is 20 to 45Wh / L; the coulomb efficiency is ≥90%; and the energy efficiency is ≥70%.
[0172] Therefore, the positive and negative vanadium electrolytes based on the composite acid medium prepared in this specific embodiment prevent high-temperature precipitation of vanadium ions, broaden the applicable temperature range, enhance the performance of the vanadium electrolyte, and reduce the loss of electrolyte capacity and efficiency performance.
Claims
1. A method for preparing positive and negative electrode vanadium electrolytes based on composite acid media, characterized in that The specific steps of the preparation method are: Step 1: Preparation of positive electrode vanadium electrolyte based on composite acid medium Step 1.1, according to the mass ratio of vanadium compound to deionized water being 1: (1.6-6.5), the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution I; then, according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being (8-48): (10-100): 1, under the condition of continued stirring, the temperature is started to be raised, and the sulfuric acid and the phosphoric acid are added to the mixed solution I in sequence at a uniform rate, and the temperature is raised to 60-95° C., and the temperature is kept until the vanadium compound is completely dissolved to obtain a positive electrode electrolyte I; the valence state of the positive electrode electrolyte I is 4.0 or 5.0; Step 1.2, according to the molar ratio of vanadium ions in the positive electrolyte I: composite additive is 100: (0.5-4), adding the composite additive to the positive electrolyte I under stirring conditions, stirring until the composite additive is completely dissolved, to obtain a positive electrolyte II; Step 1.3, the positive electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is (0.1-1):1; the positive electrode electrolyte II is electrolyzed by electrolysis to a valence state of vanadium ions of 3.5, or 4.0, or an intermediate valence state between 3.5 and 4.0, to obtain a positive electrode vanadium electrolyte based on a composite acid medium; Step 2: Preparation of negative electrode vanadium electrolyte based on composite acid medium Step 2.1, according to the mass ratio of vanadium compound to deionized water being 1: (1.6-6.5), the deionized water is added to the vanadium compound, and stirred to obtain a mixed solution II, and then according to the molar ratio of vanadium in the vanadium compound to sulfuric acid to phosphoric acid being (3.2-48): (4-100): 1, under the condition of continuous stirring, the temperature is started to be raised and the sulfuric acid and the phosphoric acid are added to the mixed solution II in sequence at a uniform rate, and the temperature is raised to 60-95° C., and the temperature is kept until the vanadium compound is completely dissolved to obtain a negative electrode electrolyte I; the valence state of the negative electrode electrolyte I is 4.0 or 5.0; Step 2.2, according to the molar ratio of vanadium ions in the negative electrode electrolyte I to the composite additive being 100: (0.5-4), the composite additive is added to the negative electrode electrolyte I under stirring, and stirred until the composite additive is completely dissolved to obtain a negative electrode electrolyte II; Step 2.3, the negative electrode electrolyte II is the cathode, and the mixed solution of sulfuric acid solution and electrocatalyst is the anode, wherein the molar ratio of electrocatalyst: sulfuric acid solution is (0.1-1):1; using electrolysis method, the negative electrode electrolyte II is electrolyzed to a valence state of vanadium ions of 3.0, 3.5, or an intermediate valence state between 3.0 and 3.5, to obtain a negative electrode vanadium electrolyte based on a composite acid medium; The sulfuric acid, the phosphoric acid and the vanadium compound in step 1.1 and step 2.1 are the same; The stirring speed in step 1.1, step 1.2, step 2.1 and step 2.2 is 50 to 500 rpm.
2. The method for preparing positive and negative vanadium electrolytes based on composite acid media according to claim 1, characterized in that The vanadium compound is one of vanadium pentoxide and vanadyl sulfate; the purity of the vanadium compound is ≥99%.
3. The method for preparing positive and negative vanadium electrolytes based on composite acid media according to claim 1, characterized in that The sequential and uniform addition of sulfuric acid and phosphoric acid means that the volume of sulfuric acid or phosphoric acid added per minute is 0.01 to 3% of the volume of the sulfuric acid or phosphoric acid to be added.
4. The method for preparing positive and negative vanadium electrolytes based on composite acid medium according to claim 1, characterized in that The mass fraction of the sulfuric acid is 90-98%.
5. The method for preparing positive and negative vanadium electrolytes based on composite acid medium according to claim 1, characterized in that The mass fraction of the phosphoric acid is 75-85%.
6. The method for preparing positive and negative vanadium electrolytes based on composite acid media according to claim 1, characterized in that The composite additive is mixed in a molar ratio of type A additive to type B additive of 1:(0.01-3); wherein the type A additive is one of acetic acid and salicylic acid, and the type B additive is one of methanesulfonic acid, aminosulfonic acid and taurine.
7. The method for preparing positive and negative vanadium electrolytes based on composite acid medium according to claim 1, characterized in that In the electrolysis method, the voltage is 0.5 to 5.0 V and the current density is 20 to 500 A / m.
8. The method for preparing positive and negative vanadium electrolytes based on composite acid medium according to claim 1, characterized in that The electrocatalyst is one of amino acids, sugars, hydrazines, polysulfides, alcohols, aldehydes, polycarbons, quinone derivatives, formate and amine compounds; and the concentration of the electrocatalyst is 0.2-5.0 mol / L.
9. A positive and negative vanadium electrolyte based on a composite acid medium, characterized in that The positive and negative vanadium electrolytes based on composite acid media are positive and negative vanadium electrolytes based on composite acid media prepared by the method for preparing positive and negative vanadium electrolytes based on composite acid media according to any one of claims 1 to 8; The main components and contents of the positive electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6-2.4 mol / L; sulfuric acid is 2.0-5.0 mol / L; phosphoric acid is 0.05-0.20 mol / L; The main components and contents of the negative electrode vanadium electrolyte of the composite acid medium are: vanadium ions are 1.6-2.4 mol / L; sulfuric acid is 2.0-5.0 mol / L; phosphoric acid is 0.05-0.50 mol / L.
Citation Information
Cited By
Crude vanadium-based all-vanadium redox flow battery negative electrode electrolyte and preparation method thereof
CN120157179A
Method for repairing valence imbalance of all-vanadium electrolyte
CN120970737A
Method for repairing imbalance of all-vanadium electrolyte valence state
CN120970737B