Rare earth sulfide solid electrolyte, preparation method and application thereof
By doping rare earth elements into the sulfide solid electrolyte, a rare earth sulfide solid electrolyte with high cycle stability and high ion conductivity is prepared, which solves the problem of poor cycle stability of the existing sulfide electrolyte and significantly improves the performance of lithium-ion batteries. Cycling performance and energy density.
Patent Information
- Application Number
- CN202411122345.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-01
AI Technical Summary
The existing sulfide solid electrolytes have poor cycle stability in all-solid-state lithium metal batteries, which limits their application in high-energy-density all-solid-state lithium batteries.
The rare earth element-doped Li10A1-0.75xBxP2S12 type rare earth sulfide solid electrolyte is used, prepared by ball milling and high-temperature sintering in an inert atmosphere, ensuring high ion conductivity and cycle stability.
The high ionic conductivity and excellent cycle performance of the rare earth sulfide solid electrolyte are achieved. The discharge capacity retention rate of the lithium-ion battery is greater than 72%, which significantly improves the cycle stability of the battery.
Smart Images

Figure CN118738536A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a rare earth sulfide solid electrolyte, a preparation method and application thereof. Background Art
[0002] As one of the important technical routes for the next generation of batteries, all-solid-state lithium batteries that use solid electrolytes to replace traditional organic liquid electrolytes are expected to solve the two major problems of safety and energy density at the same time. Since solid electrolytes are stable in nature and do not have problems with combustion, leakage, and volatilization, the assembled all-solid-state lithium batteries have excellent safety performance. In addition, solid electrolytes can also match more high-voltage positive electrode materials to increase energy density, making the application of high-energy-density all-solid-state lithium batteries possible, which is in line with the development direction of energy storage technology.
[0003] Solid electrolytes can be divided into polymer-based electrolytes and inorganic electrolytes. Generally speaking, solid polymer electrolytes have good flexibility and processability, but low room temperature ionic conductivity. Inorganic solid electrolytes can be divided into oxides, halides and sulfides according to their composition. Among them, sulfide solid electrolytes have higher lithium ion conductivity and better application prospects in lithium-ion batteries, so they have always been the focus of academic and industrial circles.
[0004] However, the existing sulfide solid electrolyte full battery cycle stability is poor, which hinders the further development of sulfide electrolyte in all-solid-state lithium metal batteries. Therefore, under the premise of ensuring the high ionic conductivity of the sulfide electrolyte layer, it is of great significance to develop a sulfide solid electrolyte with high cycle stability. Summary of the invention
[0005] The object of the present invention is to provide a rare earth sulfide solid electrolyte with high cycle stability and high ion conductivity; another object of the present invention is to provide a method for preparing the rare earth sulfide solid electrolyte with high cycle stability and high ion conductivity.
[0006] The present invention provides a rare earth sulfide solid electrolyte, the chemical composition of which is: Li 10 A 1-0.75x B x P 2 S 12 , wherein 0.01≤x≤0.2; wherein A is selected from one of silicon and tin; and B is selected from one or more of cerium, lanthanum, neodymium, samarium and scandium.
[0007] Furthermore, its ionic conductivity is greater than 10 mS / cm.
[0008] The present invention also provides a method for preparing a rare earth sulfide solid electrolyte, comprising the following steps:
[0009] S1: Under an inert atmosphere, weigh a lithium source, a compound containing A, a compound containing B, a phosphorus source, and a sulfur source according to a molar ratio of Li:A:B:P:S=10:1-0.75x:x:2:12;
[0010] S2: Under an inert atmosphere, the lithium source, the compound containing A, the compound containing B, the phosphorus source, and the sulfur source weighed in step S1 are mixed uniformly by ball milling;
[0011] S3: sealing the solid mixed powder obtained in step S2 in an inert gas atmosphere and evacuating the mixture;
[0012] S4: Sintering the sealed solid mixed powder to obtain the rare earth sulfide solid electrolyte as described above.
[0013] The inert gas atmosphere is preferably argon, and the rare earth sulfide solid electrolyte is prepared by solid phase ball milling and high temperature sintering.
[0014] Furthermore, when weighing, the weighing error is between 0 and +0.0005 grams.
[0015] In an argon protective atmosphere, the weighed materials were added into a ball mill, sealed, and ground.
[0016] Furthermore, in step S1, the lithium source is lithium sulfide; the phosphorus source is selected from one or more of phosphorus powder, phosphorus oxide, phosphorus nitride, and phosphorus pentasulfide; and the sulfur source is selected from one of sulfur powder, ammonium thiocyanate, and thiourea.
[0017] Furthermore, in step S1, the compound containing A is selected from silicon sulfide and tin disulfide.
[0018] Furthermore, in step S1, the B-containing compound is selected from one or more of cerium sulfide, lanthanum sulfide, neodymium sulfide, samarium sulfide, and scandium sulfide.
[0019] The solid electrolyte is prepared by using lithium sulfide, sulfide containing element A, sulfide containing element B, and phosphorus or phosphorus sulfide to prevent the introduction of impurity elements into the solid electrolyte and reduce the ionic conductivity of the solid electrolyte.
[0020] Furthermore, in step S2, the ball milling medium used in ball milling is zirconium oxide; the diameter of the zirconium oxide ball is 3-10 mm, and the ball-to-material ratio is 20-40:1; the ball milling time is 10-40 h, and the rotation speed is 300-600 r / min.
[0021] During sintering, the sintering furnace is selected from a box furnace, a tube furnace, and a muffle furnace.
[0022] Zirconia has good wear resistance and chemical stability, which can greatly reduce the incorporation of impurities during the ball milling process.
[0023] Furthermore, in step S3, when evacuating the air, the vacuum degree is controlled to be below 0.5 Pa.
[0024] Furthermore, in step S4, the sintering atmosphere is an inert atmosphere, the sintering temperature is 500-1000° C., and the sintering time is 6-24 hours.
[0025] The present invention also provides an application of a rare earth sulfide solid electrolyte, which is prepared by the method described above and is applied to prepare a lithium ion battery. The prepared lithium ion battery has a discharge capacity retention rate of greater than 72%.
[0026] The present invention discloses a rare earth sulfide solid electrolyte, wherein rare earth elements are doped into Li 10 AP 2 S 12 (A is Si, Sn) sulfide solid electrolyte, not only the ionic conductivity of the solid electrolyte is effectively improved, but also excellent cycle performance is exhibited after being assembled into a battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is the impedance spectrum of the rare earth sulfide solid electrolyte prepared in Examples 1-7 and Comparative Examples 1-2 of the present invention. DETAILED DESCRIPTION
[0028] In order to make the technical solution of the present invention clearer, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0029] Example 1
[0030] Preparation of Li 10 Si 0.7 Ce 0.2 Nd 0.2 P 2 S 12 Rare earth sulfide solid electrolyte:
[0031] S1: Under argon atmosphere, weigh 0.9691 g Li according to the stoichiometric ratio. 2 S, 0.2723 g SiS 2 , 0.1588 g Ce 2 S 3 , 0.1623 g Nd 2 S 3 , 0.9376 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0032] S2: Pour the weighed raw materials into a ball mill under an argon atmosphere, add zirconium oxide balls with a diameter of 5 mm, a ball-to-material ratio of 30:1, and ball mill for 40 hours at a rotation speed of 600 r / min.
[0033] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0034] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 800℃ for calcination for 24h. After cooling, Li 10 Si 0.7 Ce 0.2 Nd 0.2 P 2 S 12 Rare earth sulfide solid electrolyte materials.
[0035] Example 2
[0036] Preparation of Li 10 Si 0.97 Nd 0.04 P 2 S 12 Rare earth sulfide solid electrolyte:
[0037] S1: Under argon atmosphere, weigh 1.0458 g Li according to the stoichiometric ratio. 2 S, 0.4072 g SiS 2 , 0.0350 g Nd 2 S 3 , 1.0119 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0038] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 5 mm, a ball-to-material ratio of 30:1, and ball mill for 20 hours at a rotation speed of 500 r / min.
[0039] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0040] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 580°C for calcination for 10 hours. After cooling, Li 10 Si 0.97 Nd 0.04 P 2 S 12 Rare earth sulfide solid electrolyte materials.
[0041] Example 3
[0042] Preparation of Li 10 Sn 0.94 La 0.08 P 2 S 12 Rare earth sulfide solid electrolyte:
[0043] S1: Under argon atmosphere, weigh 0.8990 g Li according to the stoichiometric ratio. 2 S, 0.6725 g SnS 2 , 0.0585 g La 2 S 3 , 0.8698 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0044] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 3 mm, a ball-to-material ratio of 40:1, and ball mill for 25 hours at a rotation speed of 530 r / min.
[0045] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0046] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 600°C for calcination for 12 hours. After cooling, Li 10 Sn 0.94 La 0.08 P 2 S 12 Rare earth sulfide solid electrolyte materials.
[0047] Example 4
[0048] Preparation of Li 10 Sn 0.7 La 0.2 Ce 0.2 P 2 S 12 Rare earth sulfide solid electrolyte:
[0049] S1: Under argon atmosphere, weigh 0.8768 g Li according to the stoichiometric ratio. 2 S, 0.4884 g SnS 2 , 0.1428 g La 2 S 3 , 0.1437 g Ce 2 S 3 , 0.8483 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0050] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 3 mm, a ball-to-material ratio of 40:1, and ball mill for 32 hours at a rotation speed of 550 r / min.
[0051] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0052] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 700°C for calcination for 16 hours. After cooling, Li 10 Sn 0.7 La 0.2 Ce 0.2 P 2 S 12 Rare earth sulfide solid electrolyte materials.
[0053] Example 5
[0054] Preparation of Li 10 Sn 0.9925 Ce 0.01 P 2 S 12 Rare earth sulfide solid electrolyte:
[0055] S1: Under argon atmosphere, weigh 0.9740 g Li according to the stoichiometric ratio. 2 S, 0.5756 g SnS 2 , 0.0080 g Ce 2 S 3 , 0.9424 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0056] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 3 mm, a ball-to-material ratio of 40:1, and ball mill for 16 hours at a rotation speed of 450 r / min.
[0057] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0058] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 570°C for calcination for 8 hours. After cooling, Li 10 Sn 0.9925 Ce 0.01 P 2 S 12 Rare earth sulfide solid electrolyte materials.
[0059] Example 6
[0060] Preparation of Li 10 Si 0.85 Sm 0.2 P 2 S 12 Sulfide solid electrolyte:
[0061] S1: Under argon atmosphere, weigh 0.9766 g Li according to the stoichiometric ratio. 2 S, 0.4942 g SiS 2 , 0.0842 g Sm 2 S 3 , 0.9449 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0062] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 5 mm, a ball-to-material ratio of 30:1, and ball mill for 22 hours at a rotation speed of 590 r / min.
[0063] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0064] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 800°C for calcination for 18 hours. After cooling, Li 10 Si 0.85 Sm 0.2 P 2 S 12 Sulfide solid electrolyte materials.
[0065] Example 7
[0066] Preparation of Li 10 Sn 0.955 Sc 0.06 P 2 S 12 Sulfide solid electrolyte:
[0067] S1: Under argon atmosphere, weigh 0.9764 g Li according to the stoichiometric ratio. 2 S, 0.5552 g SnS 2 , 0.0123 g Sc 2 S 3 , 0.9447 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0068] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 3 mm, a ball-to-material ratio of 40:1, and ball mill for 24 hours at a rotation speed of 600 r / min.
[0069] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0070] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 1000°C for calcination for 24 hours. After cooling, Li 10 Sn 0.955 Sc 0.06 P 2 S 12 Sulfide solid electrolyte materials.
[0071] Comparative Example 1
[0072] Preparation of Li 10 SnP 2 S 12 Sulfide solid electrolyte:
[0073] S1: Under argon atmosphere, weigh 0.9047 g Li according to the stoichiometric ratio. 2 S, 0.7201 g SnS 2 , 0.8753 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0074] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 8 mm and a ball-to-material ratio of 20:1, and ball mill for 17 hours at a rotation speed of 580 r / min.
[0075] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0076] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 540°C for calcination for 18 hours. After cooling, Li 10 SnP 2 S 12 Lithium-tin-phosphorus-sulfur solid electrolyte material.
[0077] Comparative Example 2
[0078] Preparation of Li 10 SiP 2 S 12 Sulfide solid electrolyte:
[0079] S1: Under argon atmosphere, weigh 1.0553 g Li according to the stoichiometric ratio. 2 S, 0.4236 g SiS 2 , 1.0210 g P 2 S 5 , the weighing error is between 0 and +0.0005 grams.
[0080] S2: Under argon atmosphere, pour the weighed raw materials into a ball mill, add zirconium oxide balls with a diameter of 8 mm and a ball-to-material ratio of 20:1, and ball mill for 30 hours at a rotation speed of 550 r / min.
[0081] S3: The ball-milled powder sample is placed in a quartz glass tube under an argon atmosphere, evacuated to a vacuum degree of 0.2 Pa, and sealed with a hydrogen-oxygen flame gun.
[0082] S4: Place the quartz glass tube containing the powder into a muffle furnace and set the temperature to 600°C for calcination for 12 hours. After cooling, Li 10 SiP 2 S 12 Sulfide solid electrolyte materials.
[0083] Performance Test:
[0084] Conductivity test:
[0085] Take 120 mg of the sulfide solid electrolytes prepared in Examples 1-7 and Comparative Examples 1-2, grind them evenly in a mortar, and pour them into The tablets were pressed into a tablet in a mold with a tablet press machine, the pressing force was 300Mpa, and the pressing time was 15min. The tablet materials obtained in the above Examples 1-7 and Comparative Examples 1-2 were loaded into a pressure battery test mold, and the assembled pressure battery (the positive and negative electrodes were both stainless steel, and the electrolyte was the obtained tablet material) was subjected to impedance testing at a test temperature of 25°C. The impedance diagram obtained by the test is shown in FIG. Figure 1 The test results are shown in Table 1.
[0086] Testing the cycling stability of sulfide solid-state batteries:
[0087] The sulfide solid electrolytes prepared in Examples 1-7 and Comparative Examples 1-2 were assembled into all-solid-state batteries (the positive electrode was a mixture of 5 mg of lithium cobalt oxide and the prepared sulfide solid electrolyte, according to the mass ratio of LiCoO 2 : sulfide solid electrolyte = 7:3, the negative electrode is a lithium sheet, and the electrolyte is the prepared sulfide solid electrolyte) was tested at a constant current charge and discharge at 0.1C, the charge and discharge range was 3V-4.2V, and the test temperature was room temperature of 25°C. The discharge capacity retention rate of the lithium ion batteries assembled in Examples 1-7 and Comparative Examples 1-2 after 40 cycles was tested, and the test results are shown in Table 1.
[0088] Table 1 Test results of Examples 1-7 and Comparative Examples 1-2
[0089] Details Ionic conductivity (mS / cm) Capacitance retention rate (%) Example 1 13.2 72 Example 2 12.8 86 Example 3 12 78 Example 4 10.2 75 Example 5 16 87 Example 6 15 83 Example 7 14.7 81 Comparative Example 1 8.5 61 Comparative Example 2 6.6 59
[0090] Result analysis:
[0091] like Figure 1 As shown in Table 1, the solid electrolytes obtained in Examples 1-7 have higher conductivity than that in Comparative Examples 1-2.
[0092] As can be seen from Table 1, compared with Comparative Examples 1-2, the ionic conductivity of the sulfide solid electrolyte of Examples 1-7 and the discharge capacity retention rate of the prepared sulfide solid battery after 40 cycles are improved to varying degrees. This shows that Examples 1-7 can improve the full battery cycle stability and the ionic conductivity by doping the sulfide solid electrolyte with rare earth elements.
[0093] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A rare earth sulfide solid electrolyte, characterized in that: Chemical composition: Li 10 A 1-0.75x B x P2S 12 , wherein 0.01≤x≤0.2; wherein A is selected from one of silicon and tin; and B is selected from one or more of cerium, lanthanum, neodymium, samarium and scandium.
2. A rare earth sulfide solid electrolyte according to claim 1, characterized in that: Its ionic conductivity is greater than 10mS / cm.
3. A method for preparing a rare earth sulfide solid electrolyte, characterized in that: The following steps are involved: S1: Under an inert atmosphere, weigh a lithium source, a compound containing A, a compound containing B, a phosphorus source, and a sulfur source according to a molar ratio of Li:A:B:P:S=10:1-0.75x:x:2:12; S2: Under an inert atmosphere, the lithium source, the compound containing A, the compound containing B, the phosphorus source, and the sulfur source weighed in step S1 are mixed uniformly by ball milling; S3: sealing the solid mixed powder obtained in step S2 in an inert gas atmosphere and evacuating the mixture; S4: Sintering the sealed solid mixed powder to obtain the rare earth sulfide solid electrolyte as described in any one of claims 1-2.
4. The method for preparing a rare earth sulfide solid electrolyte according to claim 3, characterized in that: In step S1, the lithium source is lithium sulfide; the phosphorus source is selected from one or more of phosphorus powder, phosphorus oxide, phosphorus nitride, and phosphorus pentasulfide; and the sulfur source is selected from one of sulfur powder, ammonium thiocyanate, and thiourea.
5. The method for preparing a rare earth sulfide solid electrolyte according to claim 3, characterized in that: In the step S1, the compound containing A is selected from silicon sulfide and tin disulfide.
6. The method for preparing a rare earth sulfide solid electrolyte according to claim 3, characterized in that: In the step S1, the B-containing compound is selected from one or more of cerium sulfide, lanthanum sulfide, neodymium sulfide, samarium sulfide, and scandium sulfide.
7. The method for preparing a rare earth sulfide solid electrolyte according to claim 3, characterized in that: In the step S2, the ball milling medium used in the ball milling is zirconium oxide; the diameter of the zirconium oxide ball is 3-10 mm, and the ball-to-material ratio is 20-40:1; the ball milling time is 10-40 hours, and the rotation speed is 300-600 r / min.
8. The method for preparing a rare earth sulfide solid electrolyte according to claim 3, characterized in that: In the step S3, when evacuating, the vacuum degree is controlled to be below 0.5 Pa.
9. The method for preparing a rare earth sulfide solid electrolyte according to claim 3, characterized in that: In the step S4, the sintering atmosphere is an inert atmosphere, the sintering temperature is 500-1000° C., and the sintering time is 6-24 hours.
10. An application of a rare earth sulfide solid electrolyte, characterized in that: The method as claimed in any one of claims 4 to 9 is used to prepare a lithium-ion solid-state battery, and the discharge capacity retention rate of the prepared lithium-ion solid-state battery is greater than 72%.
Citation Information
Cited By
Sulfide solid electrolyte and all-solid-state lithium battery
CN120809941A
A sulfide solid electrolyte and an all-solid-state lithium battery
CN120809941B