Electrolyte additive for improving low-temperature performance of battery and preparation method of electrolyte additive
By using electrolyte additives in lithium batteries to improve the low-temperature performance of batteries, including anhydrous organic solvents, lithium salts and electrolytes, the discharge capacity of lithium batteries under low-temperature conditions is solved by using ingredients such as lithium dicyanoalkoxyhaloborate. It reduces the problem of degradation, improves the low-temperature performance and cycle life of the battery, and expands the scope of applications.
Patent Information
- Application Number
- CN202311328480.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-14
- Publication Date
- 2024-10-01
AI Technical Summary
The discharge capacity of existing lithium batteries decreases under low temperature conditions, especially the low conductivity of lithium salts under ultra-low temperature conditions of -60°C, which limits the low-temperature performance and application range of the battery.
An electrolyte additive is used to improve the low-temperature performance of the battery, including anhydrous organic solvents, stable and water-sensitive lithium salts, and electrolytes, through ingredients such as lithium dicyanoalkoxy haloborate to form high oxidation potential and stable SEI film improves the insertion and extraction efficiency of lithium ions and maintains high ion conductivity at low temperatures.
It significantly improves the low-temperature discharge and cycle performance of lithium-ion batteries, extends the cycle life of the battery, maintains high ion conductivity in an ultra-low temperature environment of -60°C, and broadens the application range of lithium-ion batteries.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to an electrolyte additive for improving the low temperature performance of a battery and a preparation method thereof. Background Art
[0002] Lithium battery is a secondary battery (rechargeable battery) that mainly relies on the movement of lithium ions (Li+) between the positive electrode and the negative electrode to work. During the charging process of lithium battery, Li+ is deintercalated from the positive electrode and embedded into the negative electrode through the electrolyte, making the negative electrode in a lithium-rich state, realizing the conversion of electrical energy into chemical energy, while the discharge process is just the opposite.
[0003] Lithium batteries have been widely used in 3C consumer batteries, power batteries and energy storage batteries due to their advantages such as high operating voltage, high energy density and environmental friendliness. For example, lithium batteries are currently fully used in mobile communication equipment such as mobile phones, 5G base stations, two- and three-wheeled electric vehicles, ships, passenger cars, buses, large energy storage power stations and other fields, and also have broad application prospects in aerospace, national defense and military industries. However, some fields have more stringent requirements on the performance of lithium batteries, such as high and low temperature performance, cycle performance and safety performance, and the electrolyte is one of the key factors that determine these performances. Because, in lithium batteries, the electrolyte is the only material that is in contact with the positive electrode, negative electrode and diaphragm, and it plays a vital role in the battery's specific capacity, operating temperature range, cycle efficiency and safety performance.
[0004] At present, most commercial lithium batteries use carbon materials such as graphite and mesophase carbon microbeads (MCMB) or silicon materials such as silicon oxide as the negative electrode of the battery, and materials such as LiCoO2, LiMn2O4, NCM, NCA, LiFePO4 as the positive electrode of the battery, and then insert a porous polyethylene PE, polypropylene PP and other materials between the positive and negative electrodes. The separator is made of materials, and finally a mixed solution containing a non-aqueous organic solvent and an electrolyte lithium salt is perfused as an electrolyte to complete the manufacture of lithium batteries. Among them, most of the electrolyte lithium salts of commercial electrolytes use lithium hexafluorophosphate (LiPF6), but it is unstable at high temperatures. Generally, it will begin to decompose when it reaches 60°C, producing substances such as PF5, which will destroy the negative electrode SEI film and affect the positive electrode active material, thus greatly restricting the high temperature performance of the battery. In addition, under low temperature conditions (such as -20°C), the discharge capacity of lithium batteries decreases, and the discharge capacity is even less than 70% of the discharge capacity at room temperature, which also restricts the performance of lithium batteries at low temperatures.
[0005] Patent publication number CN108511800A discloses a low-temperature electrolyte that still has high ion conductivity under ultra-low temperature conditions of -40°C by combining conventional lithium salts with film-forming additives, and the additives can form a low-impedance stable SEI film on the surface of the negative electrode, which is conducive to the rapid insertion and extraction of lithium ions under low temperature conditions. Although the battery performance has improved under general low-temperature environmental conditions, the problem of low lithium salt conductivity cannot be solved under ultra-low temperature conditions of -60°C. Therefore, the development of a new ultra-low temperature lithium salt electrolyte is of great significance to broaden the application range of lithium-ion batteries and improve their application value under extreme conditions. Summary of the invention
[0006] The purpose of the present invention is to provide an electrolyte additive for improving the low temperature performance of a battery and a preparation method thereof, in order to solve the problems existing in the above-mentioned background technology.
[0007] To achieve the above object, the technical solution adopted by the present invention is: an electrolyte additive for improving the low temperature performance of a battery, the electrolyte additive comprising an anhydrous organic solvent, a lithium salt and an electrolyte; the anhydrous organic solvent comprises the following components in parts by weight: 5-10 parts of ethyl vinyl phosphate, 5-10 parts of polyvinyl alcohol, 0.05-0.10 parts of anionic surfactant, 0.5-1 parts of dopamine, 1-3 parts of fluoroethylene carbonate, 5-10 parts of ethylene glycol, 5-10 parts of ammonium pentaborate, 5-10 parts of trifluoropropylene carbonate, 5-10 parts of diethylene glycol, 2-4 parts of dodecanedionate ammonium, 2-4 parts of ammonium hypophosphite, 2-4 parts of o-nitroanisole, 2-4 parts of mercaptobenzothiazole, 2-4 parts of citric acid, 2-4 parts of diammonium phosphate, and 30-40 parts of deionized water;
[0008] 20-30 parts of the lithium salt;
[0009] The electrolyte is 10-20 parts.
[0010] Furthermore, the lithium salt is a stable lithium salt, and the aqueous phase can be separated and then purified to obtain the stable lithium salt for subsequent use in lithium-ion batteries. The stable lithium salt includes LiSO3CF3 and LTFSI. The lithium salt is a water-sensitive lithium salt, and the aqueous phase can be separated and then lithium hydroxide is added and heated at 180°C for 24 hours, then taken out, allowed to stand and cool, and then the precipitate is separated, and then washed three times with deionized water and dried.
[0011] Furthermore, the concentration of the lithium salt is 1 mol / L-1.5 mol / L.
[0012] Furthermore, the electrolyte is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorooxalatoborate), lithium bis(trifluoromethanesulfonylimide), and lithium bis(fluorosulfonylimide).
[0013] Furthermore, the amount of the electrolyte in the electrolyte additive is 1%-5% of the total mass of the electrolyte.
[0014] Furthermore, in the electrolyte additive, the anhydrous organic solvent accounts for 75%-85% of the total mass of the high-voltage electrolyte.
[0015] Furthermore, the amount of the lithium salt in the electrolyte additive is 10%-20% of the total mass of the electrolyte.
[0016] Furthermore, a method for preparing an electrolyte additive for improving the low temperature performance of a battery comprises the following steps:
[0017] The lithium dicyanoalkoxy halide borate and trifluoromethanesulfonic acid in the electrolyte with a molar ratio of 1:(3.0-4.0) are dissolved in dichloromethane, and then a saturated solution of NaHCO3 is added thereto, and then ethyl vinyl phosphate, polyvinyl alcohol, anionic surfactant, dopamine, fluoroethylene carbonate, ethylene glycol, ammonium pentaborate, trifluoropropylene carbonate, diethylene glycol, dodecanedionium, ammonium hypophosphite, o-nitroanisole, citric acid, ammonium dihydrogen phosphate and deionized water in an anhydrous organic solvent are added, and the mixture is stirred at 0-5°C for 8h-24h, and then a lithium salt is added and the stirring is continued for 3-5h. The obtained mixed solution is rotary evaporated at 40°C-50°C to obtain the electrolyte additive.
[0018] Beneficial effects of the present invention: By adopting the above technical scheme, the electrolyte additive and preparation method thereof for improving the low temperature performance of the battery of the present invention, the novel electrolyte additive designed by the present invention contains abundant electron-withdrawing groups, based on which, it has a high oxidation potential (greater than 4.5V). The electrolyte containing such additive of the present invention has a high oxidation potential, matches the high-voltage positive electrode material, can increase the voltage of the lithium-ion battery, thereby achieving the purpose of increasing the energy density of the lithium-ion battery, and at the same time, the additive helps to form a stable SEI film, thereby extending the cycle performance of the battery and greatly improving the cycle performance of the lithium-ion battery.
[0019] The lithium biscyanoalkoxy halide borate used in the present invention can form a low-impedance stable SEI film on the surface of the negative electrode, which is beneficial to the rapid insertion and extraction of lithium ions under low temperature conditions, and effectively solves the problem of lithium precipitation at the negative electrode caused by too low temperature. The lithium biscyanoalkoxy halide borate is more easily dissolved in the solvent system at low temperature and has better compatibility with the solvent system. It will not cause lithium salt precipitation due to too low temperature, and can ensure high ionic conductivity and low-temperature discharge and cycle performance in an ultra-low temperature environment of -60°C. DETAILED DESCRIPTION
[0020] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0021] Embodiment 1: An electrolyte additive for improving the low-temperature performance of a battery, the electrolyte additive comprising an anhydrous organic solvent, a lithium salt and an electrolyte; the anhydrous organic solvent comprises the following components in parts by weight: 5 parts of ethyl vinyl phosphate, 5 parts of polyvinyl alcohol, 0.05 parts of anionic surfactant, 0.5 parts of dopamine, 1 part of fluoroethylene carbonate, 5 parts of ethylene glycol, 5 parts of ammonium pentaborate, 5 parts of trifluoropropylene carbonate, 5 parts of diethylene glycol, 2 parts of dodecanedionate ammonium, 2 parts of ammonium hypophosphite, 2 parts of o-nitroanisole, 2 parts of mercaptobenzothiazole, 2 parts of citric acid, 2 parts of diammonium phosphate, and 30 parts of deionized water; 20 parts of lithium salt; and 10 parts of electrolyte.
[0022] In this embodiment, the lithium salt is a stable lithium salt, and the aqueous phase can be separated and then purified to obtain a stable lithium salt for subsequent use in a lithium-ion battery. The stable lithium salt includes LiSO3CF3 and LTFSI. The lithium salt is a water-sensitive lithium salt, and the aqueous phase can be separated and then lithium hydroxide is added and heated at 180°C for 24 hours, then taken out, allowed to stand and cool, and then the precipitate is separated, and it is washed three times with deionized water and then dried.
[0023] In this embodiment, the concentration of the lithium salt is 1 mol / L, and the electrolyte is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorooxalatoborate), lithium bis(trifluoromethanesulfonylimide), and lithium bis(fluorosulfonylimide).
[0024] In this embodiment, the amount of electrolyte in the electrolyte additive is 5% of the total mass of the electrolyte, and in the electrolyte additive, the anhydrous organic solvent accounts for 75% of the total mass of the high-voltage electrolyte.
[0025] In this embodiment, the amount of lithium salt in the electrolyte additive is 20% of the total mass of the electrolyte.
[0026] In this embodiment, a method for preparing an electrolyte additive for improving low temperature performance of a battery comprises the following steps:
[0027] The lithium dicyanoalkoxy halide borate and trifluoromethanesulfonic acid in the electrolyte with a molar ratio of 1:3.0 are dissolved in dichloromethane, and then a saturated solution of NaHCO3 is added thereto, and then ethyl vinyl phosphate, polyvinyl alcohol, anionic surfactant, dopamine, fluoroethylene carbonate, ethylene glycol, ammonium pentaborate, trifluoropropylene carbonate, diethylene glycol, dodecanedionium, ammonium hypophosphite, o-nitroanisole, citric acid, diammonium phosphate and deionized water in an anhydrous organic solvent are added and stirred at 0°C for 8h, and then lithium salt is added and stirred for 3h. The obtained mixed solution is rotary evaporated at 40°C to obtain an electrolyte additive.
[0028] Embodiment 2: An electrolyte additive for improving the low-temperature performance of a battery, the electrolyte additive comprising an anhydrous organic solvent, a lithium salt and an electrolyte; the anhydrous organic solvent comprising the following components in parts by weight: 8 parts of ethyl vinyl phosphate, 8 parts of polyvinyl alcohol, 0.08 parts of anionic surfactant, 0.8 parts of dopamine, 2 parts of fluoroethylene carbonate, 8 parts of ethylene glycol, 5-10 parts of ammonium pentaborate, 8 parts of trifluoropropylene carbonate, 8 parts of diethylene glycol, 3 parts of dodecanedionate ammonium, 3 parts of ammonium hypophosphite, 3 parts of o-nitroanisole, 3 parts of mercaptobenzothiazole, 3 parts of citric acid, 3 parts of diammonium phosphate, and 35 parts of deionized water; 25 parts of lithium salt; and 15 parts of electrolyte.
[0029] In this embodiment, the lithium salt is a stable lithium salt, and the aqueous phase can be separated and then purified to obtain a stable lithium salt for subsequent use in a lithium-ion battery. The stable lithium salt includes LiSO3CF3 and LTFSI. The lithium salt is a water-sensitive lithium salt, and the aqueous phase can be separated and then lithium hydroxide is added and heated at 180°C for 24 hours, then taken out, allowed to stand and cool, and then the precipitate is separated, and it is washed three times with deionized water and then dried.
[0030] In this embodiment, the concentration of lithium salt is 1.2 mol / L.
[0031] In this embodiment, the electrolyte is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorooxalatoborate), lithium bis(trifluoromethanesulfonylimide), and lithium bis(fluorosulfonylimide).
[0032] In this embodiment, the amount of electrolyte in the electrolyte additive is 5% of the total mass of the electrolyte.
[0033] In this embodiment, in the electrolyte additive, the anhydrous organic solvent accounts for 80% of the total mass of the high-voltage electrolyte.
[0034] In this embodiment, the amount of lithium salt in the electrolyte additive is 15% of the total mass of the electrolyte.
[0035] In this embodiment, a method for preparing an electrolyte additive for improving low temperature performance of a battery comprises the following steps:
[0036] The lithium dicyanoalkoxy halide borate and trifluoromethanesulfonic acid in the electrolyte with a molar ratio of 1:3.5 are dissolved in dichloromethane, and then a saturated solution of NaHCO3 is added thereto, and then ethyl vinyl phosphate, polyvinyl alcohol, anionic surfactant, dopamine, fluoroethylene carbonate, ethylene glycol, ammonium pentaborate, trifluoropropylene carbonate, diethylene glycol, dodecanedionium, ammonium hypophosphite, o-nitroanisole, citric acid, diammonium phosphate and deionized water in an anhydrous organic solvent are added and stirred at 3°C for 16h, and then lithium salt is added and stirred for 4h. The obtained mixed solution is rotary evaporated at 45°C to obtain an electrolyte additive.
[0037] Embodiment 3: An electrolyte additive for improving the low-temperature performance of a battery, the electrolyte additive comprising an anhydrous organic solvent, a lithium salt and an electrolyte; the anhydrous organic solvent comprising the following components in parts by weight: 10 parts of ethyl vinyl phosphate, 10 parts of polyvinyl alcohol, 0.10 parts of anionic surfactant, 1 part of dopamine, 3 parts of fluoroethylene carbonate, 5-10 parts of ethylene glycol, 10 parts of ammonium pentaborate, 10 parts of trifluoropropylene carbonate, 10 parts of diethylene glycol, 4 parts of dodecanedionate ammonium, 4 parts of ammonium hypophosphite, 4 parts of o-nitroanisole, 4 parts of mercaptobenzothiazole, 4 parts of citric acid, 4 parts of diammonium phosphate, and 40 parts of deionized water; 30 parts of lithium salt; 20 parts of electrolyte.
[0038] In this embodiment, the lithium salt is a stable lithium salt, and the aqueous phase can be separated and then purified to obtain a stable lithium salt for subsequent use in a lithium-ion battery. The stable lithium salt includes LiSO3CF3 and LTFSI. The lithium salt is a water-sensitive lithium salt, and the aqueous phase can be separated and then lithium hydroxide is added and heated at 180°C for 24 hours, then taken out, allowed to stand and cool, and then the precipitate is separated, and it is washed three times with deionized water and then dried.
[0039] In this embodiment, the concentration of lithium salt is 1.5 mol / L.
[0040] In this embodiment, the electrolyte is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorooxalatoborate), lithium bis(trifluoromethanesulfonylimide), and lithium bis(fluorosulfonylimide).
[0041] In this embodiment, the amount of electrolyte in the electrolyte additive is 5% of the total mass of the electrolyte.
[0042] In this embodiment, among the electrolyte additives, the anhydrous organic solvent accounts for 85% of the total mass of the high-voltage electrolyte.
[0043] In this embodiment, the amount of lithium salt in the electrolyte additive is 10% of the total mass of the electrolyte.
[0044] In this embodiment, a method for preparing an electrolyte additive for improving low temperature performance of a battery comprises the following steps:
[0045] The lithium dicyanoalkoxy halide borate and trifluoromethanesulfonic acid in the electrolyte with a molar ratio of 1:4.0 are dissolved in dichloromethane, and then a saturated solution of NaHCO3 is added thereto, and then ethyl vinyl phosphate, polyvinyl alcohol, anionic surfactant, dopamine, fluoroethylene carbonate, ethylene glycol, ammonium pentaborate, trifluoropropylene carbonate, diethylene glycol, dodecanedionium, ammonium hypophosphite, o-nitroanisole, citric acid, diammonium phosphate and deionized water in an anhydrous organic solvent are added and stirred at 5°C for 24h, and then lithium salt is added and stirred for 5h. The obtained mixture is rotary evaporated at 50°C to obtain an electrolyte additive.
[0046] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0047] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An electrolyte additive for improving the low temperature performance of a battery, characterized in that: The electrolyte additive comprises an anhydrous organic solvent, a lithium salt and an electrolyte; the anhydrous organic solvent comprises the following components in parts by weight: 5-10 parts of ethyl vinyl phosphate, 5-10 parts of polyvinyl alcohol, 0.05-0.10 parts of anionic surfactant, 0.5-1 parts of dopamine, 1-3 parts of fluoroethylene carbonate, 5-10 parts of ethylene glycol, 5-10 parts of ammonium pentaborate, 5-10 parts of trifluoropropylene carbonate, 5-10 parts of diethylene glycol, 2-4 parts of dodecanedionate ammonium, 2-4 parts of ammonium hypophosphite, 2-4 parts of o-nitroanisole, 2-4 parts of mercaptobenzothiazole, 2-4 parts of citric acid, 2-4 parts of diammonium phosphate, and 30-40 parts of deionized water; 20-30 parts of the lithium salt; The electrolyte is 10-20 parts.
2. The electrolyte additive for improving the low temperature performance of a battery according to claim 1, characterized in that: The lithium salt is a stable lithium salt and can be purified after separating the aqueous phase, and the stable lithium salt can be subsequently used in a lithium-ion battery. The stable lithium salt includes LiSO3CF3 and LTFSI. The lithium salt is a water-sensitive lithium salt and can be separated from the aqueous phase and lithium hydroxide is added and heated at 180°C for 24 hours, then taken out, allowed to stand and cool, and the precipitate is separated, and then washed three times with deionized water and dried.
3. The electrolyte additive for improving low temperature performance of a battery according to claim 1, characterized in that: The concentration of the lithium salt is 1 mol / L-1.5 mol / L.
4. The electrolyte additive for improving low temperature performance of a battery according to claim 1, characterized in that: The electrolyte is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorooxalatoborate), lithium bis(trifluoromethanesulfonyl imide), and lithium bis(fluorosulfonyl imide).
5. The electrolyte additive for improving low temperature performance of a battery according to claim 1, characterized in that: The amount of the electrolyte in the electrolyte additive is 1%-5% of the total mass of the electrolyte.
6. The electrolyte additive for improving low temperature performance of a battery according to claim 1, characterized in that: In the electrolyte additive, the anhydrous organic solvent accounts for 75%-85% of the total mass of the high-voltage electrolyte.
7. The electrolyte additive for improving low temperature performance of a battery according to claim 1, characterized in that: The amount of the lithium salt in the electrolyte additive is 10%-20% of the total mass of the electrolyte.
8. A method for preparing an electrolyte additive for improving low temperature performance of a battery, characterized in that: The following steps are involved: The lithium dicyanoalkoxy halide borate and trifluoromethanesulfonic acid in the electrolyte with a molar ratio of 1:(3.0-4.0) are dissolved in dichloromethane, and then a saturated solution of NaHCO3 is added thereto, and then ethyl vinyl phosphate, polyvinyl alcohol, anionic surfactant, dopamine, fluoroethylene carbonate, ethylene glycol, ammonium pentaborate, trifluoropropylene carbonate, diethylene glycol, dodecanedionium, ammonium hypophosphite, o-nitroanisole, citric acid, ammonium dihydrogen phosphate and deionized water in an anhydrous organic solvent are added, and the mixture is stirred at 0-5°C for 8h-24h, and then a lithium salt is added and the stirring is continued for 3-5h. The obtained mixed solution is rotary evaporated at 40°C-50°C to obtain the electrolyte additive.
Citation Information
Patent Citations
Superlow-temperature lithium ion battery electrolyte and lithium ion battery using same
CN108511800A
Cited By
Zinc-iodine battery electrolyte additive with pH buffering and multi-iodide shuttle effect inhibiting capabilities
CN119361860A