Insulator for spark plug and spark plug
By optimizing the particle distribution in the spark plug insulator, the bending strength and thermal shock resistance of the alumina-based sintered body are improved, and the deficiencies of the insulator in the existing technology in terms of mechanical strength and high temperature stability are solved.
Patent Information
- Application Number
- CN202410335258.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-01
AI Technical Summary
Existing alumina-based sintered body insulators have deficiencies in bending strength and thermal shock resistance, making it difficult to meet the requirements for high mechanical strength and high temperature stability.
By controlling the average area and distribution of particles in the insulator of the spark plug, it is ensured that the average area of the particles is above 4.4 μm2 and below 8.0 μm2, the maximum area is below 600 μm2, and there are more than 0.1/mm2 large particles and 613 particles per unit area. Small particles/mm2 or more to improve the bending strength and thermal shock resistance of the insulator.
The high bending strength and thermal shock resistance of the spark plug insulator is achieved, ensuring stable performance under high temperature and mechanical stress.
Smart Images

Figure CN118739033A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an insulator for a spark plug and a spark plug. Background Art
[0002] Patent Document 1 discloses the following prior art: in order to improve the mechanical strength of a spark plug having an insulator made of an alumina-based sintered body, the average grain size of the insulator is set to 1.5 μm or less and the standard deviation of the grain size distribution is set to 1.2 μm or less.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-57559 Summary of the invention
[0006] Problems to be solved by the invention
[0007] There is a need in the prior art to improve the bending strength and thermal shock resistance of insulators.
[0008] The present invention has been made to meet this need, and an object of the present invention is to provide a spark plug insulator and a spark plug capable of improving bending strength and thermal shock resistance.
[0009] Means for solving problems
[0010] To achieve the object, a first embodiment of the present invention is a spark plug insulator, which is an alumina-based sintered body and has an axial hole extending along an axis. When a force is applied to the spark plug insulator to bend the spark plug insulator and the spark plug insulator is destroyed, in a range including a starting point of destruction among two ranges obtained by dividing a cross section formed by the destruction by a plane perpendicular to the direction of the force and including the axis, the average area of particles appearing in a top view image of the range is 4.4 μm. 2 Above and 8.0μm 2 Below, the maximum area of the particle is 600μm 2 Below. Particle area is 60μm 2 Above and 600μm 2 The number of large particles below 0.1 / mm per unit area in the top view image 2 above.
[0011] The second embodiment is as follows: In the first embodiment, the number of large particles per unit area of the top view image is 6.2 / mm 2 the following.
[0012] The third embodiment is as follows: In the first or second embodiment, the particle inclusion area is 20 μm2 Above and 59μm 2 The following small particles exist in 613 / mm per unit area of the top view image. 2 Above and 2270 pieces / mm 2 the following.
[0013] A fourth aspect is a spark plug including the spark plug insulator according to any one of the first to third aspects.
[0014] Effects of the Invention
[0015] The average area of particles appearing in the top view image of the spark plug insulator is 4.4 μm 2 Above and 8.0μm 2 Below, the maximum area of the particle is 600μm 2 Below, area 60μm 2 Above and 600μm 2 The number of large particles below 0.1 / mm per unit area in the top view image is 2 As a result, the bending strength and thermal shock resistance can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] [ Figure 1 ] is a single-side cross-sectional view of a spark plug in one embodiment.
[0017] [ Figure 2 ] is a schematic diagram of the cross section of the insulator. DETAILED DESCRIPTION
[0018] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. Figure 1 This is a one-side cross-sectional view of the spark plug 10 in one embodiment, which is a combination of an outer shape view and a full cross-sectional view, with the axis C of the shaft hole 12 as the boundary. Figure 1 The lower side of the paper is referred to as the front end side of the spark plug 10, and the upper side of the paper is referred to as the rear end side of the spark plug 10. The spark plug 10 includes an insulator 11 (spark plug insulator). The insulator 11 is a cylindrical member having an axial hole 12 extending along the axis C, and is an alumina-based sintered body having excellent insulation and mechanical properties at high temperatures.
[0019] A rod-shaped metal center electrode 13 is arranged in the axial hole 12 of the insulator 11. In the center electrode 13, a core material having excellent thermal conductivity is buried in a base material. The base material is formed of an alloy mainly composed of Ni or a metal material composed of Ni. The core material is formed of copper or an alloy mainly composed of copper. The core material can be omitted.
[0020] The terminal fitting 14 is a rod-shaped member connected to an ignition device (not shown), and is formed of a conductive metal material (such as low carbon steel). The front end of the terminal fitting 14 is arranged in the axial hole 12 of the insulator 11, and the rear end of the terminal fitting 14 protrudes from the insulator 11. The terminal fitting 14 is electrically connected to the center electrode 13 in the axial hole 12.
[0021] The metallic shell 15 is a substantially cylindrical member formed of a conductive metal material (such as low carbon steel) and is disposed on the outer periphery of the insulator 11. An external thread 16 is provided on the front end side of the metallic shell 15.
[0022] The ground electrode 17 is a rod-shaped metal member (for example, made of a nickel-based alloy) connected to the metallic shell 15. A spark gap is formed between the ground electrode 17 and the center electrode 13.
[0023] The spark plug 10 is manufactured, for example, by the following method. After the center electrode 13 is inserted into the axial hole 12 of the insulator 11, a conductive powder containing a glass component is filled into the axial hole 12. After the terminal fitting 14 is inserted from the rear end side of the axial hole 12, the terminal fitting 14 is pressed in while being heated to a temperature higher than the softening point of the glass component contained in the powder, and an axial load is applied to the powder by the terminal fitting 14. The powder is compressed and sintered, and the center electrode 13 and the terminal fitting 14 are electrically connected in the axial hole 12. Next, after the main body fitting 15 connected with the ground electrode 17 is assembled to the outer periphery of the insulator 11, the ground electrode 17 is bent, and a spark gap is set between the ground electrode 17 and the center electrode 13, thereby obtaining the spark plug 10.
[0024] An example of a method for producing the insulator 11 will be described. The insulator 11 is produced through the steps of slurry preparation, degassing, granulation, molding, grinding, and firing. These steps will be described below in order.
[0025] The slurry preparation step is a step of preparing slurry by mixing raw material powder, a binder and a solvent. The raw material powder uses a powder of a compound that is converted into aluminum oxide by firing (hereinafter referred to as "Al compound powder") as a main component. As the Al compound powder, for example, aluminum oxide powder is used.
[0026] In the slurry preparation process, a pulverizing process for the purpose of mixing and pulverizing the raw material powder is carried out. The pulverizing process is carried out using a wet pulverizer using a ball mill or the like. The diameter of the balls used in the wet pulverizer is not particularly limited as long as it does not impair the purpose of the present invention, and is preferably 2 mm or more and 20 mm or less, more preferably 2 mm or more and 10 mm or less, and further preferably 2 mm or more and 6 mm or less. Two or more balls having different diameters may be combined. Through such a pulverizing process, the raw material powder becomes uneven in particle size (particle diameter) and has a narrow particle size distribution. When using such a raw material powder, in the alumina-based sintered body obtained after sintering, the size of the particles can be controlled and the sintering density can be increased.
[0027] The particle size (particle size after crushing) of the Al compound powder (alumina powder, etc.) is not particularly limited as long as it does not impair the purpose of the present invention. For example, it is preferably 1.5 μm or more, more preferably 1.7 μm or more, preferably 2.5 μm or less, and more preferably 2.0 μm or less. When the particle size of the Al compound powder is in such a range, the number of defects in the insulator is suppressed and a moderate sintering density is obtained. The particle size is the volume-based median particle size (D50) measured by a laser diffraction method (manufactured by Nikkiso Co., Ltd., Microtrac particle size distribution measuring device, product name "MT-3000").
[0028] When the mass of the fired alumina-based sintered body (in terms of oxide) is set to 100 mass%, the Al compound powder is preferably prepared to be 90 mass% or more in terms of oxide. More preferably, it is 90 mass% or more and 98 mass% or less, and further preferably, it is 90 mass% or more and 97 mass% or less. The raw material powder may contain powders other than the Al compound powder as long as the purpose of the present invention is not impaired.
[0029] For the purpose of improving the formability of the raw material powder, a binder is added to the slurry. As such a binder, hydrophilic binders such as polyvinyl alcohol, aqueous acrylic resin, gum arabic, dextrin, etc. can be cited. These can be used alone or in combination of two or more. The amount of the binder is not particularly limited, as long as it does not damage the purpose of the present invention. For example, relative to 100 parts by mass of the raw material powder, it is mixed in a ratio of 1-10 parts by mass, preferably in a ratio of 3-7 parts by mass.
[0030] For the purpose of dispersing raw material powders, etc., a solvent is used. Examples of the solvent include water and alcohol. These can be used alone or in combination of two or more. The amount of the solvent is not particularly limited as long as it does not impair the purpose of the present invention. For example, the amount of the solvent is 23-40 parts by mass, preferably 25-35 parts by mass, relative to 100 parts by mass of the raw material powder. Other ingredients other than the raw material powder, the binder and the solvent can be added to the slurry as needed. The slurry can be mixed using a known stirring or mixing device.
[0031] The prepared slurry can be degassed as needed. In the degassed process, for example, a container containing the mixed (kneaded) slurry is placed in a vacuum degassing device, decompressed and placed in a low pressure environment, thereby removing bubbles contained in the slurry. By comparing the density of the slurry before and after degassed, the amount of bubbles in the slurry can be determined.
[0032] The granulation step is a step of making spherical granulated powder from a slurry containing a raw material powder and the like. There is no particular limitation on the method for making granulated powder from a slurry, as long as the purpose of the present invention is not impaired, and an example thereof may be a spray drying method. In the spray drying method, the slurry is spray dried using a predetermined spray drying device, thereby obtaining granulated powder having a predetermined particle size. There is no particular limitation on the particle size of the granulated powder, as long as the purpose of the present invention is not impaired, and for example, a pass rate of 212 μm ≥ 95% or less is preferred, and a pass rate of 180 μm ≥ 95% or less is more preferred.
[0033] The forming process is a process of forming the granulated powder into a predetermined shape using a forming die to obtain a formed body. The forming process is performed by rubber compression molding, mold compression molding, etc. In the case of the present embodiment, the pressure (pressing and increasing speed) applied to the forming die (e.g., the inner rubber die and the outer rubber die of the rubber compression molding machine) from the outer peripheral side is adjusted in a step-by-step manner. In addition, it is preferably adjusted to a higher pressure range than before (e.g., above 100 MPa). It should be noted that the upper limit of the pressure is not particularly limited, as long as it does not impair the purpose of the present invention, and for example, it can be adjusted to below 200 MPa.
[0034] The grinding process is a process for removing the machining allowance of the molded body obtained after the molding process, grinding the surface of the molded body, etc. In the grinding process, the machining allowance is removed, the surface of the molded body is ground, etc. by grinding with a resin bonded grinding wheel, etc. The shape of the molded body is adjusted by such a grinding process.
[0035] The firing step is a step of firing the molded body whose shape is adjusted in the grinding step to obtain an insulator. In the firing step, for example, the molded body is fired at 1450° C. to 1650° C. for 1 to 8 hours in an air atmosphere. After firing, the molded body is cooled to obtain an insulator 11 composed of an alumina-based sintered body.
[0036] The insulator 11 is a brittle material with weak tensile stress. When a force is applied to bend the insulator 11, cracks develop from pores and defects existing inside the insulator 11. By observing the structure of the cross section formed by breaking the insulator 11, it is possible to clearly identify defects existing inside the insulator 11. The insulator 11 can be broken by applying tensile force to it using various means such as the three-point bending test and the four-point bending test specified in JIS R1601:2008 and the insulator bending strength test specified in JIS B8031:2006, so as to form a cross section in the insulator 11.
[0037] See also Figure 1 , the insulator bending strength test specified in JIS B8031: 2006 is described. After the external thread 16 of the spark plug 10 is tightened to the iron clamp 18 with a specified maximum torque, the spark plug 10 is fixed to the clamp 18, and a force F perpendicular to the axis C is applied to a position within 5 mm from the rear end of the insulator 11. No impact is applied to the insulator 11, but the force F is pressed at a speed of 10 mm / min or less to break the insulator 11 and form a cross section.
[0038] Figure 2 FIG. 1 is a schematic diagram of a cross section of the insulator 11. When the force F (see FIG. 11 ) is applied to the insulator 11, Figure 1 ) direction and containing the axis C, the cross section (the circular ring around the axial hole 12) is divided into two ranges 21 and 22. The range 21 containing the starting point of destruction is a surface formed mainly by applying tensile force. The range 22 is a surface formed by the development of cracks formed in the range 21. The particles that grow abnormally during firing are one of the defects existing inside the insulator 11. Using a scanning electron microscope (SEM), the structure of the range 21 containing the starting point of destruction (in this embodiment, the surface including the side where the force F is applied) is observed to investigate the size and distribution of the particles in the range 21.
[0039] Since the size of the particles cannot be confirmed even if the entire range 21 is included in one SEM image, the entire range 21 is divided into a plurality of parts, and an SEM image (top view image) is obtained for each part. For the SEM image, an image is exemplified in which the range 21 is divided into rectangular parts with a size of 985 μm in length and 1231 μm in width and magnified at a low magnification (e.g., 100 times). The range 21 is a shape obtained by cutting a circular ring in half, so in the SEM image, the axial hole 12 inside the range 21 and the space outside the range 21 sometimes become part of the rectangular image, but the SEM image of the entire range 21 is obtained, in which the image of a blank space outside the range 21 in a part of the image is also included.
[0040] After obtaining a low-magnification SEM image of the entire range 21, image analysis is performed using known image analysis software (e.g., WinROOF (registered trademark), manufactured by Mitani Shoji Co., Ltd.). In the image analysis, after the size of the SEM image is corrected based on the scale marked in the SEM image, the SEM image is binarized in order to extract the edge of the image. In the binarization process, the luminance (brightness) of each pixel of the SEM image is grayscaled (binarized) using a predetermined threshold value (e.g., a threshold value of 0-25). By grayscaleing the pixels and eliminating the intermediate grayscale, a binary image in which the grain boundaries are emphasized can be obtained.
[0041] The binary image of range 21 is used to determine the area of the particles using a known image analysis method. The area of all particles included in range 21 is 60 μm. 2 Above and 600μm 2 The number of the following particles (hereinafter referred to as "large particles") is counted. Particles that grow abnormally during firing are one of the defects that are likely to become the starting point of destruction. Since the place where defects are concentrated in the insulator 11 will become the starting point of destruction, if there are particles that grow abnormally during firing, they will appear in range 21.
[0042] In order to reduce defects caused by abnormally grown particles and ensure the bending strength of the insulator 11, the maximum area of the particles present in the top view image of the range 21 is 600 μm. 2 The maximum area of the particles present in the top view image of range 21 is 60 μm 2 The above is ideal for ensuring the toughness of the insulator 11 and ensuring thermal shock resistance.
[0043] In the top view image of the range 21, the number of insulators 11 is 0.1 / mm per unit area. 2 The presence of the large particles can ensure the toughness of the insulator 11. The presence of the large particles is preferably 6.2 particles / mm per unit area in the top view image of the range 21.2 This is to ensure the bending strength of the insulator 11.
[0044] In addition to the low-magnification SEM image for investigating the number of large particles, 10 high-magnification SEM images were randomly obtained in which a rectangular portion of range 21 with a size of 100 μm in length and 163 μm in width was enlarged. For the high-magnification SEM image, the position of the image acquisition was set in such a way that a blank outside range 21 did not appear in range 21 as a whole or in a part of the image. After the high-magnification SEM image was acquired, the same image analysis as that performed on the low-magnification SEM image was performed to obtain a binary image in which the grain boundary was emphasized.
[0045] Using the binarized image of range 21, the known image analysis method is used to find the area of all particles appearing in the 10 images and the area of each particle (average). Even if a large particle is included in the 10 images, the large particle is included in the area as one particle. In the case where a particle is cut off at the edge of the image, the portion that appears in the image is included in the area as one particle. In insulator 11, the average area of the particles is 4.4 μm 2 Above and 8.0μm 2 This is to improve the bending strength and thermal shock resistance of the insulator 11.
[0046] It should be noted that when the average area of the particles is less than 4.4 μm 2 When the average area of the particles is larger than 8.0 μm, the toughness of the insulator 11 decreases and the thermal shock resistance tends to decrease. 2 When the porosity is 5%, the porosity between particles becomes larger and the bending strength tends to decrease. In order to ensure the bending strength, the porosity of the insulator 11 is preferably 5% or less.
[0047] Using a known image analysis method, all particles with an area of 20 μm in the 10 images were analyzed. 2 Above and 59μm 2 The number of the following particles (hereinafter referred to as "small particles") is counted. Preferably, the insulator 11 is present at 613 particles / mm per unit area in 10 images. 2 Above and 2270 pieces / mm 2 The following small particles are used to improve the thermal shock resistance and bending strength of the insulator 11 by the presence of the small particles.
[0048] Example
[0049] The present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.
[0050] (Insulator production)
[0051] In samples No. 1 to No. 12, two insulators having the same basic structure as the insulator 11 of the spark plug 10 illustrated in the embodiment were prepared by the same method as in the embodiment. For the insulator of sample No. 4, when the raw material powder was pulverized by a wet pulverizer in the slurry preparation process, balls with a diameter of 2 mm and balls with a diameter of 6 mm were mixed at a ratio of 50 mass % and 50 mass %, respectively. For the insulators of samples No. 3 and No. 5 to No. 8, in the slurry preparation process, the ratio of balls used when pulverizing the raw material powder was appropriately changed, and they were prepared in the same way as sample No. 4.
[0052] For the insulator of sample No. 1, when the raw material powder was pulverized by a wet pulverizer in the slurry preparation process, balls with a diameter of 8 mm and balls with a diameter of 12 mm were mixed at a ratio of 50 mass % and 50 mass %, respectively. For the insulators of samples No. 2 and No. 9 to No. 12, in the slurry preparation process, the ratio of balls used when pulverizing the raw material powder was appropriately changed, and they were prepared in the same manner as sample No. 1.
[0053] (Insulator bending strength test)
[0054] Using one insulator each of the samples No. 1 to No. 12, two of which were produced, one sample of the spark plug 10 described in the embodiment was produced. For the samples, after the spark plug 10 was fastened to the clamp 18 with a predetermined maximum torque in accordance with the insulator bending strength test specified in JIS B8031: 2006, a force F perpendicular to the axis C was applied to a position within 5 mm from the rear end of the insulator 11, and no impact was applied to the insulator 11, but the insulator 11 was pressed at a speed of 10 mm / min or less until the insulator 11 was broken. The sample with a force F (bending strength) of 7.5 kN or more when the insulator 11 was broken was judged as A, and the sample with a bending strength of less than 7.5 kN was judged as C.
[0055] [Table 1]
[0056]
[0057] (Cross-sectional observation of insulator)
[0058] The cross section of the insulator 11 destroyed in the insulator bending strength test is divided into two parts using a plane 20 that is perpendicular to the direction of the force F applied to the insulator 11 and includes the axis C, and is set as two ranges 21 and 22. Then, the structure of the range 21 including the starting point of destruction between the ranges 21 and 22 is observed using an SEM (JEM-IT300LA, manufactured by JEOL Ltd.).
[0059] The entire range 21 was divided into multiple parts, and multiple SEM images of rectangular parts with a size of 985 μm in length and 1231 μm in width were obtained at a low magnification (100 times). After the image processing software WinROOF2013 (WinROOF is a registered trademark) was used to obtain a binary image, the area of the largest particle and the area of 60 μm were obtained through image analysis. 2 Above and 600μm 2 The following are the numbers of large particles per unit area (numbers rounded to the second decimal place): The area of the largest particle is recorded in the "largest" column of Table 1, and the number of large particles per unit area is recorded in the "number of large particles" column of Table 1.
[0060] Ten locations in the range 21 were randomly selected, and 10 high-magnification SEM images of a rectangular portion with a size of 100 μm in length and 163 μm in width were obtained. After obtaining a binary image through image processing, the area of each particle (the average value rounded off to the second decimal place) and the area of 20 μm were calculated by image analysis. 2 Above and 59μm 2 The number of small particles per unit area (rounded to the first decimal place) is shown in the “Average” column of Table 1. The number of small particles per unit area is shown in the “Number of Small Particles” column of Table 1.
[0061] (Thermal shock test)
[0062] After the insulators 11 of samples No. 1 to No. 12 are stored in a thermostatic bath maintained at a predetermined temperature for 30 minutes, they are immediately put into water at 20°C for rapid cooling. The posture of the insulator 11 when put into the water is set so that the axis C of the insulator 11 is parallel to the water surface. The presence or absence of cracks in the insulator 11 taken out of the water is visually confirmed by applying a penetrant flaw detection liquid. The temperature of the thermostatic bath storing the insulator 11 is increased from 150°C in increments of 10°C until cracks are found on the insulator 11. The thermal shock properties of the samples whose temperature difference (critical temperature difference) between the thermostatic bath temperature and the water temperature (20°C) when cracks are found on the insulator 11 is 240°C or more are judged as A, those whose temperature is 230°C or more and less than 240°C are judged as B, and those whose temperature is less than 220°C are judged as C.
[0063] As shown in Table 1, the average area of the particles is 4.4 μm 2 Above and 8.0μm 2 Below, maximum area is 600μm 2 Below, the number of large particles is 0.1 / mm 2 The above samples No. 3 to No. 8 were judged as A in bending strength and A or B in thermal shock resistance.
[0064] On the other hand, although the average particle area is 4.4 μm 2 Above and 8.0μm 2 Below, maximum area is 600μm 2 Below, but the number of large particles is less than 0.1 / mm 2 Sample No. 2 was judged as A in bending strength, but was judged as C in thermal shock resistance. It was confirmed that the presence of an appropriate number of large particles is effective in ensuring thermal shock resistance. It is inferred that the toughness of the insulator is improved when the large particles are present in an appropriate amount.
[0065] For sample No. 2, the maximum area of the particles is less than 60 μm 2 , so the number of large particles is 0 / mm 2 It is also believed that sample 2 has a maximum particle area of less than 60 μm. 2 , so the thermal shock resistance is judged as C. The estimated maximum area is 60μm 2 The above is effective for improving the toughness of the insulator.
[0066] Although the maximum area of the particles is 600 μm 2 Below, the number of large particles is 0.1 / mm 2 Above, but with an average area less than 4.4μm 2 Sample No. 1 was judged as A in bending strength, but C in thermal shock resistance. It was confirmed that when the average area is less than 4.4 μm 2 When the thermal shock resistance is reduced.
[0067] Although the average particle size is 4.4 μm 2 Above and 8.0μm 2 Below, the number of large particles is 0.1 / mm 2 Above, but the maximum area is greater than 600μm 2 Samples 9 and 10 were judged as A in thermal shock resistance, but C in bending strength. It was confirmed that when the maximum area is larger than 600 μm 2 When , a tendency of lowering of bending strength was observed.
[0068] Although the maximum area of the particles is 600 μm 2 Below, the number of large particles is 0.1 / mm 2 Above, but the average area is greater than 8.0μm 2 Samples 11 and 12 were judged as A in thermal shock resistance, but C in bending strength. 2 When , a tendency of lowering of bending strength was observed.
[0069] For sample No. 12, the number of large particles is 7.8 / mm 2 , the number of large particles is large, so the average particle area including large particles is 10.1μm 2 In order to make the average area of the particles 4.4μm 2 Above and 8.0μm 2 In the range below, the number of large particles is 6.2 / mm, such as sample No. 8. 2 The following are preferred.
[0070] The average particle size is 4.4 μm. 2 Above and 8.0μm 2 Below, maximum area is 600μm 2 Below, the number of large particles is 0.1 / mm 2 Above, and the number of small particles is 613 / mm 2 Above and 2270 pieces / mm 2 The following samples No. 4 to No. 8 were judged as A in both bending strength and thermal shock resistance. It was found that there were 613 small particles / mm 2 Above and 2270 pieces / mm 2 The following are effective for improving the thermal shock resistance.
[0071] The present invention has been described above based on the embodiment, but the present invention is not limited to the above embodiment at all, and it can be easily estimated that various improvements and modifications can be made without departing from the scope of the present invention. For example, the shape of the insulator 11 is an example and can be set appropriately.
[0072] In the embodiment, the insulator 11 is broken and formed into a cross section in accordance with the insulator bending strength test of the spark plug specified in JIS B8031:2006, but it is not necessarily limited to this. The insulator 11 before the center electrode 13, the metal shell 15, etc. are attached to form the spark plug posture can of course be broken and formed into a cross section in accordance with the three-point bending test or the four-point bending test specified in JIS R1601:2008.
[0073] In the three-point bending test and the four-point bending test specified in JIS R1601: 2008, a force is applied between the supporting points of the insulator 11 supported by two supporting points to break the insulator 11. The side where the supporting points contact is a range 21 including the starting point of the breakage.
[0074] In the embodiment, the spark plug 10 is described in which the ground electrode 17 is exposed in the combustion chamber when the spark plug 10 is installed in the engine (not shown), but it is not necessarily limited to this. Of course, the structure of the embodiment can be applied to a spark plug in which the ground electrode 17 is covered by a cap having a through hole (a spark plug having a sub chamber in the combustion chamber).
[0075] In the embodiment, the spark plug 10 that generates spark discharge between the center electrode 13 and the ground electrode 17 is described, but the present invention is not necessarily limited thereto. The configuration of the embodiment can of course be applied to a spark plug that utilizes non-equilibrium plasma generated around the center electrode 13 .
[0076] Explanation of symbols
[0077] 10 Spark plug
[0078] 11Insulator (spark plug insulator)
[0079] 12 Axis hole
[0080] 20 Plane
[0081] 21 Scope
[0082] C axis
Claims
1. A spark plug insulator, comprising an alumina-based sintered body and having an axial hole extending along an axis. When a force that bends the spark plug insulator is applied to the spark plug insulator to cause the spark plug insulator to be broken, In the range including the starting point of the failure, of the two ranges obtained by dividing the cross section formed by the failure by a plane perpendicular to the direction of the force and including the axis, The average area of particles appearing in the top view image of the above range is 4.4 μm 2 Above and 8.0μm 2 Below, the maximum area of the particles is 600 μm 2 the following, The particle contains an area of 60 μm 2 Above and 600μm 2 The following large particles, The number of large particles per unit area of the top view image is 0.1 / mm 2 above.
2. The spark plug insulator according to claim 1, wherein: The number of large particles per unit area of the top view image is 6.2 / mm. 2 the following.
3. The spark plug insulator according to claim 1 or 2, wherein: The particle contains an area of 20 μm 2 Above and 59μm 2 The following small particles, The number of small particles per unit area of the top view image is 613 / mm. 2 Above and 2270 pieces / mm 2 the following. 4 . A spark plug comprising the spark plug insulator according to claim 1 .