Three-dimensional structure composite lithium alloy material and preparation method thereof
By using a three-dimensional structure composite lithium alloy material in a lithium metal battery, including a lithium alloy layer, a cellulose/lithium alloy composite layer and a surface protective layer, the problems of lithium dendrites and dead lithium are solved, and the cycle life and mechanical strength of the battery are improved. , simplifying the preparation process, reducing equipment requirements, and achieving stable adsorption and uniform growth of lithium.
Patent Information
- Application Number
- CN202410958608.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Lithium metal anodes are prone to produce dendrites and dead lithium during the charge and discharge process, which affects the safety and cycle life of the battery. The preparation process of the existing technology is complex and the equipment requirements are high, and the composite layer is not uniform and dense enough, resulting in the growth of lithium dendrites. and dead lithium deposition.
A three-dimensional structure composite lithium alloy material is used, including a first lithium alloy layer, a second cellulose/lithium alloy composite layer and a third surface protective layer. The tape is prepared by a smelting-calendering method, and the cellulose nanofibers are pretreated and bonded to The agent solvent is homogenized and dispersed to form a uniformly distributed cellulose/lithium alloy composite layer, which increases the lithium ion conductivity and coats the surface with a protective layer of solid electrolyte powder, simplifying the process and reducing equipment requirements.
Effectively inhibits the side reactions between lithium alloy and electrolyte, improves battery cycle life, enhances mechanical strength, reduces storage environment requirements, ensures stable adsorption and uniform growth of lithium on the alloy surface, significantly increases the diffusion rate of lithium ions, simplifies the preparation process and reduces equipment Require.
Smart Images

Figure CN118748247A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a three-dimensional structured composite lithium alloy material and a preparation method thereof. Background Art
[0002] In recent years, with the increasing requirements for battery energy density in fields such as new energy vehicles, lithium metal anodes have regained attention due to their high energy density. The theoretical specific capacity of metallic lithium is 3860mAh / g, and the electrochemical potential is -3.04V (vs standard hydrogen electrode), making it an ideal negative electrode material for lithium batteries. The research and development of lithium metal batteries aims to further improve battery performance, especially energy density. Companies such as SolidEnergy have developed a new type of lithium metal foil anode that significantly reduces the size of the battery. Lithium metal batteries have a wide range of applications, including drones, 3C electronic products, electric vehicles, etc.
[0003] Lithium metal negative electrodes are prone to problems such as dendrites and dead lithium during the charge and discharge process, which affects the safety and stability of the battery. To use lithium metal as the negative electrode material for lithium-ion batteries, we still face two major challenges: safety and cycle life. One of the main problems plaguing lithium metal negative electrodes is the problem of lithium dendrites. During the cycle process, due to local polarization factors, lithium dendrites grow on the surface of lithium metal. When the lithium dendrites grow to a certain extent, they may penetrate the diaphragm and cause safety problems. If the lithium dendrites break, "dead lithium" will be formed, causing battery capacity loss. In addition, the side reaction problem between lithium metal and electrolyte is also an important and complex technical challenge in lithium metal batteries, which not only affects the cycle life performance of the battery, but also may cause safety hazards.
[0004] To solve the above problems. Patent CN 114784259 A discloses a "lithium metal negative electrode material and its preparation method", which can improve the battery energy density and reduce the generation of lithium dendrites in the lithium deposition process and improve the battery's cycle performance and stability through the design of lithium metal gradient material layer, but it adopts immersion and evaporation to prepare the composite layer in the preparation process, which has the disadvantages of low controllability of chemical reaction, that is, the chemical reaction will preferentially proceed at the edge of the metal grain boundary, and the obtained composite layer is not uniform and dense enough. In the long-term battery cycle process, the non-dense alloy layer will still lead to the growth of lithium dendrites and the deposition of dead lithium, causing battery failure, and its preparation process is complex and has high equipment requirements.
[0005] Therefore, it is of great significance to develop a three-dimensional structured composite lithium alloy material and its preparation method. Summary of the invention
[0006] The task of the present invention is to overcome the deficiencies of the prior art and provide a three-dimensional structured composite lithium alloy material and a preparation method thereof, which can not only completely solve the problem of uneven lithium ion deposition in lithium batteries leading to lithium dendrite growth, but also simplify the preparation process and reduce equipment requirements.
[0007] The task of the present invention is accomplished by the following technical solutions:
[0008] A three-dimensional structured composite lithium alloy material; in order to solve the problems of easy generation of dendrites and dead lithium, the material comprises a first lithium alloy layer, a second cellulose / lithium alloy composite layer, and a third surface protective layer; the second cellulose / lithium alloy composite layer is arranged above the first lithium alloy layer, and the third surface protective layer is arranged above the second cellulose / lithium alloy composite layer.
[0009] The preparation method of the three-dimensional structure composite lithium alloy negative electrode material includes the following process steps and condition steps:
[0010] S1. A first lithium alloy strip having a thickness of 50 to 150 μm is prepared by a melting-rolling method;
[0011] S2. A second lithium alloy strip having a thickness of 50 to 150 μm is prepared by a melting-rolling method;
[0012] S3. Pre-treat the cellulose nanofibers to obtain a lithium ion conductivity ≥ 1×10 -4 S / cm modified cellulose nanofibers;
[0013] S4. The modified cellulose nanofibers obtained in step S3 are homogenized and dispersed with a binder and a solvent, and then the cellulose nanofibers are coated on the surface of the second lithium alloy strip obtained in step S2 to preliminarily obtain a cellulose / lithium alloy composite strip semi-finished product;
[0014] S5. The cellulose / lithium alloy composite strip semi-finished product prepared in step S4 is further compounded by a rolling and calendering method, so that the cellulose is evenly distributed in the lithium alloy to form a three-dimensional structure of the cellulose / lithium alloy composite strip;
[0015] S6. The first lithium alloy strip obtained in step S1 and the cellulose / lithium alloy composite strip obtained in step S5 are rolled and composited by a rolling method to prepare a first lithium alloy layer-second cellulose / lithium alloy composite layer strip;
[0016] S7. Coating a surface protection layer on the upper layer of the first lithium alloy layer-second cellulose / lithium alloy composite layer strip prepared in step S6.
[0017] Compared with the prior art, the present invention has the following advantages or effects:
[0018] Because the third surface protective layer in the three-dimensional composite lithium alloy material of a specific structure prepared by the composition and process of the present invention is arranged on the surface of the three-dimensional composite lithium alloy, it can effectively inhibit the side reaction between the lithium alloy and the electrolyte, or even water and oxygen, thereby improving the cycle life of the battery and reducing its storage environment requirements; at the same time, since the solid electrolyte powder dispersed inside the third protective layer contains cellulose nanofibers with high lithium ion conductivity uniformly distributed at the second cellulose / lithium alloy composite layer, it helps to transport lithium ions to the second cellulose / lithium alloy composite layer to start deposition, and can further transport lithium ions to the first lithium metal layer. Lithium ions are attracted to the negative electrode and nucleated there; in addition, since the cellulose nanofibers and the lithium alloy form an interlaced layout in the three-dimensional composite lithium alloy negative electrode, the mechanical strength of the entire negative electrode system can be effectively toughened and increased, and the integrity of the structure as a whole can be guaranteed; in addition, since there are a large number of uniform lithium-philic sites in the first lithium alloy layer, these sites can reduce the nucleation overpotential of lithium, so that lithium can be stably adsorbed and uniformly grown on the alloy surface, so the diffusion rate of lithium in lithium alloys such as Li13In3, LiZn, Li9Al4, Li22Sn5, etc. is faster, and the preparation process is simple and the equipment requirements are low. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the structure of the three-dimensional composite lithium alloy material proposed in the present invention.
[0020] Figure 2 is used for Figure 1 Schematic diagram of the process flow of the preparation method of the three-dimensional composite lithium alloy material structure shown.
[0021] The present invention is further described in detail below in conjunction with the accompanying drawings. DETAILED DESCRIPTION
[0022] like Figure 1 As shown, the three-dimensional structure of the composite lithium alloy material structure, in order to solve the problems of easy generation of dendrites and dead lithium, includes a first lithium alloy layer, a second cellulose / lithium alloy composite layer, and a third surface protection layer; the second cellulose / lithium alloy composite layer is arranged above the first lithium alloy layer, and the third surface protection layer is arranged above the second cellulose / lithium alloy composite layer.
[0023] The structure of the three-dimensional composite lithium alloy material of the present invention is further:
[0024] The alloy elements in the first lithium alloy layer include one or more of aluminum Al, zinc Zn, indium In, tin Sn, boron B, silver Ag and the like.
[0025] The alloy element of the second cellulose / lithium alloy composite layer is magnesium Mg, the cellulose is cellulose nanofiber, and the lithium ion conductivity is ≥1×10 -4 S / cm.
[0026] The third surface protective layer is mainly composed of at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyvinylidene fluoride-hexafluoropropylene, and polyperfluoroethylene propylene, and the protective layer contains nano-scale solid electrolyte powder.
[0027] The solid electrolyte powder is lithium lanthanum zirconium oxide and its doped and modified powder.
[0028] The thickness of the first lithium alloy is 20-50 μm.
[0029] The thickness of the second cellulose / lithium alloy composite layer is 10-25 μm.
[0030] The thickness of the third surface protection layer is 0.1-5 μm.
[0031] The content of alloying elements in the first lithium alloy does not exceed 1.5 at.%.
[0032] The content of alloying elements in the second cellulose / lithium alloy composite layer is in the range of 0.1 to 10 at.%.
[0033] The second cellulose nanofiber has a diameter of 5 to 50 nm, a length of 0.2 to 3 μm, and a cellulose nanofiber content in the range of 0.1 to 20 wt.%.
[0034] like Figure 2 As shown, the preparation method of the three-dimensional structure composite lithium alloy negative electrode material includes the following process steps and conditions:
[0035] S1. A first lithium alloy strip having a thickness of 50 to 150 μm is prepared by a melting-rolling method;
[0036] S2. A second lithium alloy strip having a thickness of 50 to 150 μm is prepared by a melting-rolling method;
[0037] S3. Pre-treat the cellulose nanofibers to obtain a lithium ion conductivity ≥ 1×10 -4 S / cm modified cellulose nanofibers;
[0038] S4. The modified cellulose nanofibers obtained in step S3 are homogenized and dispersed with a binder and a solvent, and then the cellulose nanofibers are coated on the surface of the second lithium alloy strip obtained in step S2 to preliminarily obtain a cellulose / lithium alloy composite strip semi-finished product;
[0039] S5. The cellulose / lithium alloy composite strip semi-finished product prepared in step S4 is further compounded by a rolling and calendering method, so that the cellulose is evenly distributed in the lithium alloy to form a three-dimensional structure of the cellulose / lithium alloy composite strip;
[0040] S6. The first lithium alloy strip obtained in step S1 and the cellulose / lithium alloy composite strip obtained in step S5 are rolled and composited by a rolling method to prepare a first lithium alloy layer-second cellulose / lithium alloy composite layer strip;
[0041] S7. Coating a surface protection layer on the upper layer of the first lithium alloy layer-second cellulose / lithium alloy composite layer strip prepared in step S6.
[0042] The process and conditions of the present invention may further be:
[0043] The lithium alloy melting temperature in steps S1 and S2 should be higher than the melting point of the equilibrium phase diagram.
[0044] In the step S1, the lithium alloy is cooled by a rapid cooling method with a cooling rate of >200°C / min or by a forced cooling mold.
[0045] The cellulose nanofibers are pretreated in step S3 by at least one of ion coordination and functional group grafting.
[0046] In step S3, the ion coordination is carried out by adding copper ions Cu 2+ Coordinated with one-dimensional cellulose nanofibers, the crystal structure of cellulose is changed, so that the spacing between polymer chains is expanded to provide lithium ions Li + Molecular channels for embedding and rapid transport.
[0047] In step S3, the functional group grafting is carried out by further reacting the isocyanate with the hydroxyl groups of the cellulose nanofibers to obtain small molecular structures such as -CN, -CF3 and -COO groups, and at the same time, urea bonds are generated to enhance the conduction of lithium ions.
[0048] The binder used in step S4 includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, polypropylene, styrene-butadiene rubber, polyacrylonitrile, polyethylene, etc.
[0049] The solvent used in step S4 includes at least one of N-methylpyrrolidone, tetrahydrofuran, ethylene glycol dimethyl ether, dimethyl carbonate, dimethyl sulfoxide, N,N-dimethylformamide, etc.,
[0050] The mass ratio of the cellulose nanofibers to the binder used in step S4 is 50-98:2-50.
[0051] The mass ratio of the cellulose nanofibers to the binder used in step S4 is 90-98:2-10.
[0052] The coating method in step S4 includes any one of cast coating, blade coating, spray coating and the like.
[0053] In step S5, the stacking and rolling includes cellulose / lithium alloy composite layer materials, which are stacked in an AB / AB manner, wherein A represents the fiber side and B represents the lithium alloy side;
[0054] The number of times of the roll bonding used in the step S5 is 4 to 6 times; the final thickness of the roll bonding is 20 to 100 μm, and the final thickness of the roll bonding is 20 to 50 μm.
[0055] In the step S6, the first lithium alloy layer and the second cellulose / lithium alloy composite layer are more closely combined by rolling, and the thickness is further reduced.
[0056] In the step S7, the coating method of the protective layer includes any one of cast coating, blade coating, spray coating, gravure coating, micro gravure coating, spin coating, extrusion coating, etc.
[0057] Example 1
[0058] Battery-grade lithium metal and high-purity aluminum metal (≥ purity 99.99%) were weighed and sampled at a molar ratio of 99:1, stirred and melted under an argon protective atmosphere at a melting temperature of 690°C. After stirring evenly, they were cast and cooled to obtain the first lithium-aluminum alloy (the cooling mold was pure copper and cooled to below 80°C for 3 minutes), and then the lithium-aluminum alloy was rolled and thinned to 100μm.
[0059] Battery-grade lithium metal and high-purity magnesium metal (≥99.99% purity) were weighed and sampled at a molar ratio of 97:3, stirred and melted under an argon protective atmosphere at a melting temperature of 450°C, and cast and cooled after stirring to obtain a lithium-magnesium alloy, and then the lithium-aluminum alloy was rolled and thinned to 100μm. Copper ion (Cu2+) coordination treated cellulose nanofibers (diameter 50nm, length 1μm~3μm) and polyvinylidene fluoride were mixed at a mass ratio of 95:5 and dissolved in dimethyl carbonate at a solid content of 30%. After the slurry was evenly dispersed, it was coated on a 100μm thick lithium-magnesium alloy by a doctor blade coating method and dried. The thickness of the cellulose nanofiber film layer was ~20μm. The semi-finished cellulose / lithium-magnesium alloy composite material was laminated and rolled 6 times to obtain a second cellulose / lithium-magnesium alloy composite material with uniform three-dimensional distribution and a thickness of 50μm.
[0060] The obtained lithium aluminum alloy and cellulose / lithium magnesium alloy composite material are rolled and compounded, and the oxide layer on the bonding surface of the material is removed before rolling. The roller gap spacing is gradually reduced during rolling until the overall thinning is reduced to 60μm. Finally, a protective layer of rubidium-doped tantalum-lithium lanthanum zirconium oxide / polyvinylidene fluoride-hexafluoropropylene is coated on the surface of the composite material. The protective layer thickness is 3μm, and the particle size of rubidium tantalum-lithium lanthanum zirconium oxide is ~300nm, accounting for 20wt%. Finally, a three-dimensional structure composite lithium alloy negative electrode is obtained.
[0061] Example 2
[0062] The same as Example 1, except that the first lithium alloy uses battery metal lithium and high-purity zinc metal (≥ purity 99.99%), and the molar ratio is 99.5:0.5, the melting temperature is 500°C, and it takes 2 minutes to cool to below 80°C during casting.
[0063] Example 3
[0064] The same as Example 1, except that the first lithium alloy uses battery metal lithium and high-purity indium metal (≥ purity 99.99%), and the molar ratio is 99.5:0.5, the melting temperature is 450°C, and it takes 1.5 minutes to cool to below 80°C during casting.
[0065] Example 4
[0066] The same as Example 1, except that the first lithium alloy uses battery metal lithium and high-purity silver metal (≥ purity 99.99%), and the molar ratio is 99:1, the melting temperature is 450°C, and it takes 1.5 minutes to cool to below 80°C during casting.
[0067] Example 5
[0068] The same as Example 1, except that the first lithium alloy uses battery metal lithium and high-purity zinc metal (≥ purity 99.99%), and the molar ratio is 99.5:0.5, the melting temperature is 500°C, and it takes 2 minutes to cool to below 80°C during casting.
[0069] Comparative Example 1
[0070] The method is the same as Example 1, except that, during the preparation process, the pretreated cellulose nanofibers are not composited into the lithium-magnesium alloy, and the final composite lithium alloy negative electrode does not have three-dimensionally distributed cellulose nanofibers.
[0071] Comparative Example 2
[0072] The same as Example 1, except that a protective layer of rubidium-doped tantalum-lithium lanthanum zirconium oxide / polyvinylidene fluoride-hexafluoropropylene is not coated on the surface of the composite material, and there is no surface protective layer structure in the final composite lithium alloy negative electrode.
[0073] Comparative Example 3
[0074] Lithium aluminum alloy, thickness 60μm. Metal lithium and high-purity aluminum metal (≥ purity 99.99%) are weighed and sampled at a molar ratio of 99:1, stirred and melted under an argon protective atmosphere at a melting temperature of 690°C, and cast and cooled after stirring to obtain the first lithium aluminum alloy (the cooling mold is pure copper, cooled to below 80°C for 3 minutes), and then the lithium aluminum alloy is rolled and thinned to 60μm.
[0075] Comparative Example 4
[0076] Lithium-magnesium alloy, thickness 60μm. Metallic lithium and high-purity magnesium metal (≥99.99% purity) are weighed and sampled at a molar ratio of 97:3, stirred and smelted under an argon protective atmosphere at a smelting temperature of 450°C, stirred evenly, and then cast and cooled to obtain a lithium-magnesium alloy, which is then rolled and thinned to 60μm.
[0077] Comparative Example 5
[0078] Commercial battery grade pure lithium metal, 60μm thick.
[0079] Test Case
[0080] (1) Cycle capacity retention rate
[0081] The lithium-ion batteries prepared in the above-mentioned embodiments and comparative examples were tested for cycle capacity retention. At room temperature, they were first activated with a current of 0.1C, and then charged and discharged at a constant current density of 1C. The charge and discharge cut-off voltages were 4.5V and 3V, respectively. The positive electrode was a commercial NCM811 positive electrode material, and the electrolyte was a commercial ternary electrolyte. The test results are as follows:
[0082] Test results table
[0083]
[0084] From the experimental data test results of the above embodiments and comparative examples, it can be seen that embodiments 1 to 5 all have a better capacity retention rate, and the cycle performance of the three-dimensional structure composite lithium alloy prepared by the composition and process of the present invention is significantly better than the cycle performance of the material not using the composition and process of the invention.
[0085] As described above, the present invention can be better implemented. The above embodiments are only the best implementation methods of the present invention, but the implementation methods of the present invention are not limited by the above embodiments. Other changes, modifications, replacements, combinations, and simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. Three-dimensional structure composite lithium alloy material, to solve the problems of easy generation of dendrites and dead lithium, characterized by It comprises a first lithium alloy layer, a second cellulose / lithium alloy composite layer, and a third surface protection layer; the second cellulose / lithium alloy composite layer is arranged above the first lithium alloy layer, and the third surface protection layer is arranged above the second cellulose / lithium alloy composite layer.
2. The composite lithium alloy material according to claim 1, characterized in that The alloy elements in the first lithium alloy layer include one or more of aluminum Al, zinc Zn, indium In, tin Sn, boron B, silver Ag and the like.
3. The composite lithium alloy material according to claim 1, characterized in that The alloy element of the second cellulose / lithium alloy composite layer is magnesium Mg, the cellulose is cellulose nanofiber, and the lithium ion conductivity is ≥1×10 -4 S / cm.
4. The composite lithium alloy material according to claim 1, characterized in that The third surface protective layer is mainly composed of at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyvinylidene fluoride-hexafluoropropylene, and polyperfluoroethylene propylene, and the protective layer contains nano-scale solid electrolyte powder.
5. The composite lithium alloy material according to claim 4, characterized in that The solid electrolyte powder is lithium lanthanum zirconium oxide and its doped and modified powder.
6. The composite lithium alloy material according to claim 1 or 2, characterized in that The thickness of the first lithium alloy is 20-50 μm.
7. The composite lithium alloy material according to claim 1 or 3, characterized in that The thickness of the second cellulose / lithium alloy composite layer is 10-25 μm.
8. The composite lithium alloy material according to claim 1 or 4, characterized in that The thickness of the third surface protection layer is 0.1-5 μm.
9. The composite lithium alloy material according to claim 1 or 2, characterized in that The content of alloying elements in the first lithium alloy does not exceed 1.5 at.%.
10. The composite lithium alloy material according to claim 1 or 3, characterized in that The content of alloying elements in the second cellulose / lithium alloy composite layer is in the range of 0.1 to 10 at.%.
11. The composite lithium alloy material according to claim 1, characterized in that The second cellulose nanofiber has a diameter of 5 to 50 nm, a length of 0.2 to 3 μm, and a cellulose nanofiber content in the range of 0.1 to 20 wt.%.
12. A method for preparing a three-dimensional structured composite lithium alloy negative electrode material, characterized in that The process steps and conditions are as follows: S1. A first lithium alloy strip having a thickness of 50 to 150 μm is prepared by a melting-rolling method; S2. A second lithium alloy strip having a thickness of 50 to 150 μm is prepared by a melting-rolling method; S3. Pre-treat the cellulose nanofibers to obtain a lithium ion conductivity ≥ 1×10 -4 S / cm modified cellulose nanofibers; S4. The modified cellulose nanofibers obtained in step S3 are homogenized and dispersed with a binder and a solvent, and then the cellulose nanofibers are coated on the surface of the second lithium alloy strip obtained in step S2 to preliminarily obtain a cellulose / lithium alloy composite strip semi-finished product; S5. The cellulose / lithium alloy composite strip semi-finished product prepared in step S4 is further compounded by a rolling and calendering method, so that the cellulose is evenly distributed in the lithium alloy to form a three-dimensional structure of the cellulose / lithium alloy composite strip; S6. The first lithium alloy strip obtained in step S1 and the cellulose / lithium alloy composite strip obtained in step S5 are rolled and composited by a rolling method to prepare a first lithium alloy layer-second cellulose / lithium alloy composite layer strip; S7. Coating a surface protection layer on the upper layer of the first lithium alloy layer-second cellulose / lithium alloy composite layer strip prepared in step S6.
13. The method according to claim 12, characterized in that The lithium alloy melting temperature in steps S1 and S2 should be higher than the melting point of the equilibrium phase diagram.
14. The method according to claim 12, characterized in that In the step S1, the lithium alloy is cooled by a rapid cooling method with a cooling rate of >200°C / min or by a forced cooling mold.
15. The method according to claim 12, characterized in that The cellulose nanofibers are pretreated in step S3 by at least one of ion coordination and functional group grafting.
16. The method according to claim 12, characterized in that In step S3, the ion coordination is carried out by adding copper ions Cu 2+ Coordinated with one-dimensional cellulose nanofibers, the crystal structure of cellulose is changed, so that the spacing between polymer chains is expanded to provide lithium ions Li + Molecular channels for embedding and rapid transport.
17. The method according to claim 12 or 16, characterized in that In step S3, the functional group grafting is carried out by further reacting the isocyanate with the hydroxyl groups of the cellulose nanofibers to obtain small molecular structures such as -CN, -CF3 and -COO groups, and at the same time, urea bonds are generated to enhance the conduction of lithium ions.
18. The method according to claim 12, characterized in that The binder used in step S4 includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, polypropylene, styrene-butadiene rubber, polyacrylonitrile, polyethylene, etc.
19. The method according to claim 12, characterized in that The solvent used in step S4 includes at least one of N-methylpyrrolidone, tetrahydrofuran, ethylene glycol dimethyl ether, dimethyl carbonate, dimethyl sulfoxide, N,N-dimethylformamide, etc.
20. The method according to claim 12, characterized in that The mass ratio of the cellulose nanofibers to the binder used in step S4 is 50-98:2-50.
21. The method according to claim 12, characterized in that The mass ratio of the cellulose nanofibers to the binder used in step S4 is 90-98:2-10.
22. The method according to claim 12 or 18 or 19 or 20 or 21, characterized in that The coating method in step S4 includes any one of cast coating, blade coating, spray coating and the like.
23. The method according to claim 12, characterized in that The stacking and rolling in step S5 includes cellulose / lithium alloy composite layer materials, which are stacked in an AB / AB manner, wherein A represents the fiber side and B represents the lithium alloy side.
24. The method according to claim 12 or 23, characterized in that The number of times of the roll bonding used in the step S5 is 4 to 6 times; the final thickness of the roll bonding is 20 to 100 μm, and the final thickness of the roll bonding is 20 to 50 μm.
25. The method according to claim 12, characterized in that In the step S6, the first lithium alloy layer and the second cellulose / lithium alloy composite layer are more closely combined by rolling, and the thickness is further reduced.
26. The method according to claim 12, characterized in that In the step S7, the coating method of the protective layer includes any one of cast coating, blade coating, spray coating, gravure coating, micro gravure coating, spin coating, extrusion coating, etc.
Citation Information
Patent Citations
Flexible self-supporting lithium-tin alloy composite nanofiber lithium metal battery negative electrode material
CN112615009A
Uniformly-distributed three-dimensional lithium alloy negative electrode and preparation method thereof
CN114300654A
Three-dimensional carbon nanofiber silver modified lithium metal negative electrode material and preparation method thereof
CN116169293A
Mixed conductive 3D current collector and preparation method and application thereof
CN117317246A
Negative electrode for lithium secondary battery
JP1988274060A
Cited By
Negative electrode sheet and preparation method therefor, and metal battery cell, battery device and electric device