Method for preparing composite cross-shaped component through vacuum-assisted forming
The vacuum-assisted forming method is used to lay fiber fabric on the L-shaped mold and perform vacuum forming, which solves the problems of high production cost, poor mechanical properties and long preparation cycle of composite cross-shaped components, achieving efficient and low-cost preparation, and improving the Tensile properties and production adaptability of components.
Patent Information
- Application Number
- CN202411239664.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The composite cross-shaped components in the existing technology have high production costs, poor mechanical properties and long preparation cycles, making it difficult to meet the requirements for use under harsh working conditions.
Using the vacuum-assisted molding method, through the steps of pretreatment, fiber fabric laying, vacuum bag film sealing, vacuum infusion and curing demoulding, fiber fabric is directly laid on a simple L-shaped mold and vacuum formed to prepare composite cross-shaped components. .
It effectively reduces the preparation cost, improves the mechanical properties of the components, especially the tensile properties, shortens the preparation cycle, improves the adaptability of the process, and is suitable for the production of components of different volumes.
Smart Images

Figure CN118752805A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material component preparation, and in particular to a method for preparing a composite material cross-shaped component by vacuum-assisted molding. Background Art
[0002] The cross-shaped joint structure is widely used in many fields such as aviation, aerospace, navigation and rail transportation. Compared with the cross-shaped components made of traditional metal materials, the cross-shaped components made of fiber-reinforced resin-based composite materials have higher specific strength and specific stiffness, and their light weight makes them have a wider application prospect.
[0003] In existing research, the preparation method of cross-shaped joints of composite materials is generally to prepare two T-shaped components in advance, and then combine them by gluing. The mechanical properties, especially the tensile properties, of the cross-shaped components prepared by this process are poor, and it is difficult to meet the use requirements under harsh working conditions. Therefore, it is of great significance to study how to improve the mechanical properties of cross-shaped components, reduce the cost of preparing components, and reduce the preparation cycle of components.
[0004] Invention patent application number CN201310325634.X proposes an integral forming method for a cross-shaped joint of a sewing-enhanced fiber-reinforced resin-based composite material, which uses a method of combining two T-shaped components to prepare a cross-shaped component by using an RTM process and introducing a sewing-enhanced RTM process. The study found that the cross-shaped component prepared by the RTM process has better fatigue resistance than the adhesive bonding process. However, the RTM process requires the preparation of the corresponding mold in advance. When the component is not mass-produced or the component volume is large, the mold cost accounts for a high proportion in the component preparation, and the component preparation process is long.
[0005] Patent publication number CN103518025A mentions an external tensile structural component with energy absorption function, including a cross-section mold, and a certain length of material supplied to the mold has an L-shaped cross-section that matches the contour of the corresponding molding segment. The material of the L-shaped cross-section length is then stacked in a nested relationship at a 90-degree angle of the long axis of each segment molding surface. Under the action of a compression tool or device, the mold is heated and cured to form a cross-shaped carbon fiber skeleton. However, due to the use of this method to prepare a cross-shaped carbon fiber skeleton, when the component is not mass-produced or the component is large in size, the cost of the mold accounts for a high proportion in the component preparation, and the component preparation process is relatively long. Summary of the invention
[0006] In view of this, the present invention aims to propose a method for preparing a composite material cross-shaped component by vacuum-assisted forming, so as to solve the problems of high production cost, poor mechanical properties and long preparation cycle when the existing process is used to prepare the composite material cross-shaped component in the prior art; thereby effectively optimizing the process for preparing the composite material cross-shaped component, reducing the cost of preparing the component, improving the mechanical properties of the prepared component, shortening the preparation cycle of the component, and improving the adaptability of the process, so as to meet the preparation of components of different volumes.
[0007] To achieve the above object, the technical solution of the present invention is achieved as follows: The present invention relates to a method for preparing a composite material cross-shaped component by vacuum-assisted forming, the method comprising the following steps: Step 1: Pretreatment: Select at least four L-shaped molds and cut the fiber fabric into the required size; Step 2, fiber fabric laying: laying the fiber fabrics in sequence, and during the laying process, pre-pressing the laid fiber fabrics at least once to form a cross-shaped sample; Step 3: Vacuum-assisted treatment: Lay out a glue injection pipeline under the cross-shaped sample, and place a vacuum bag film on the outside of the cross-shaped sample for sealing, and then perform an airtightness test; Step 4: Vacuum infusion treatment: prepare the resin and perform vacuum infusion treatment; Step 5, curing and demoulding: After curing through the curing process, remove the vacuum auxiliary equipment to obtain the required cross-shaped component.
[0008] Further, step one includes: Step S11: Pretreatment: Select four L-shaped molds, cover the outer sides of the four molds with release cloths, and wipe the outer sides of the release cloths with a cleaning agent for standby use; Step S12: cutting the fiber fabric into a required size, placing the cut fiber fabric in an oven, and drying it at a preset drying temperature T0° C. and a preset drying time t1.
[0009] Furthermore, the L-shaped mold includes a first side surface and a second side surface, the first side surface and the second side surface are vertically arranged, and the first side surface and the second side surface constitute an outer side wall of the L-shaped mold.
[0010] Furthermore, the length of the first side surface is H1 mm, and the length of the second side surface is H2 mm; H1 and H2 are both positive numbers, the value range of H1 is 3 mm-20 mm, and the value range of H2 is 150 mm-750 mm.
[0011] Furthermore, the preset drying temperature T0 has a value range of 60° C.-120° C.; the preset drying time t1 has a value range of 0.5 h-4 h.
[0012] Further, in step S11, the material of the L-shaped mold includes any one or more materials selected from the group consisting of carbon steel, alloy steel, stainless steel, aluminum alloy, titanium alloy, PVC foam, and hardwood board.
[0013] Further, step two includes: Step S21: laying fiber fabric: laying fiber fabric of a first size outside four L-shaped molds; and performing pre-pressing treatment; Step S22: taking any two L-shaped molds as a group to form two sets of molds, arranging the outer sides of the two L-shaped molds in the two sets opposite to each other; laying fiber fabrics of the second size between the two L-shaped molds in the two sets of molds respectively, and performing pre-pressing treatment; Step S23: After the two sets of molds are arranged opposite to each other, a fiber fabric of a third size is laid between the two sets of molds and pre-pressed to form a cross-shaped sample.
[0014] Furthermore, at least one layer of the fiber fabric of the first size, the fiber fabric of the second size, and the fiber fabric of the third size are provided.
[0015] Further, step three includes: Step S31: vacuum-assisted processing: laying out a glue injection pipeline under the cross-shaped sample; Step S32: a vacuum bag film is arranged on the outside of the cross-shaped sample, and at least one layer of the vacuum bag film is arranged, and each layer of the vacuum bag film is sealed; when sealing, the wrinkles of the vacuum bag film need to be arranged away from the surface of the product; Step S33: air tightness test: the vacuum pump drives the vacuum pipe connected to it to evacuate the inside of the vacuum bag film. After the vacuum pump works stably, the working air pressure inside the vacuum bag film is K1. The vacuum pump is turned off. After the preset pressure holding time t2, the air pressure inside the vacuum bag film is tested. Step S34: Determine whether the current air pressure K2 inside the vacuum bag film is ≤ the preset air pressure value K0. If yes, the air tightness of the vacuum bag film is qualified, and execute step 4; if no, the air tightness of the vacuum bag film is unqualified, and return to step S32.
[0016] Furthermore, K1≤-0.097Mpa.
[0017] Compared with the prior art, the method for preparing a composite material cross-shaped component by vacuum-assisted molding described in the present invention has the following beneficial effects: The method can effectively optimize the process of preparing composite cross-shaped components, reduce the cost of preparing components, improve the mechanical properties of prepared components, shorten the preparation cycle of components, and increase the adaptability of the process to meet the preparation of components of different volumes. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings, which constitute part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention. In the accompanying drawings: Figure 1 It is a schematic diagram of the L-shaped mold structure; Figure 2a A schematic diagram of laying a first size fiber fabric; Figure 2b A schematic diagram for laying a second size fiber fabric; Figure 2c A schematic diagram for laying a third-dimensional fiber fabric; Figure 2d To complete the schematic diagram of laying the cross-shaped member; Figure 3 This is a schematic diagram of the actual image of the prepared composite cross-shaped component. DETAILED DESCRIPTION
[0019] The inventive concepts of the present disclosure will be described below using terms commonly used by those skilled in the art to convey the essence of their work to other persons skilled in the art. However, these inventive concepts can be embodied in many different forms and should not be considered limited to the embodiments described herein.
[0020] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0021] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0022] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.
[0023] In the prior art, the traditional composite cross-shaped component is prepared by bonding two T-shaped components, and its mechanical properties, especially tensile properties, are relatively weak. In existing studies, composite cross-shaped components are prepared by using RTM process and RTM process with sewing reinforcement. This method requires the T-shaped component and the mold required by the RTM process to be prepared in advance, and its preparation cycle is long and the preparation cost is high.
[0024] In order to solve the problems of high production cost, poor mechanical properties and long preparation cycle when using the existing process to prepare a composite cross-shaped component in the prior art, this embodiment provides a method for preparing a composite cross-shaped component by vacuum assisted molding, and the method comprises the following steps: Step 1: Pretreatment: Select at least four L-shaped molds and cut the fiber fabric into the required size; Step 2, fiber fabric laying: laying the fiber fabrics in sequence, and during the laying process, pre-pressing the laid fiber fabrics at least once to form a cross-shaped sample; Step 3: Vacuum-assisted treatment: Lay out a glue injection pipeline under the cross-shaped sample, and place a vacuum bag film on the outside of the cross-shaped sample for sealing, and then perform an airtightness test; Step 4: Vacuum infusion treatment: prepare the resin and perform vacuum infusion treatment; Step 5, curing and demoulding: After curing through the curing process, remove the vacuum auxiliary equipment to obtain the required cross-shaped component.
[0025] In this embodiment, four L-shaped molds are provided, but the specific number is not limited thereto.
[0026] Different from the prior art that uses T-shaped components or adhesive settings, which are prone to high preparation costs, long cycles, and poor mechanical properties, the present application uses the method to set up four simple L-shaped molds without the need for T-shaped components. The required number of layers of fiber fabric are directly laid on four simple L-shaped molds, and then they are directly combined and spliced, and vacuum-assisted molding, i.e., vacuum infusion, is used for one-time molding to prepare a cross-shaped component of a fiber-reinforced resin-based composite material. This can effectively optimize the process of preparing a cross-shaped component of a composite material, reduce the cost of preparing the component, and improve the mechanical properties of the prepared component, especially the tensile properties. The preparation cycle of the component is shortened, and the adaptability of the process is improved to facilitate the preparation of components of different volumes. It can also have broad application prospects in the fields of aviation, aerospace, navigation, and rail transportation.
[0027] Step one includes: Step S11: Pretreatment: Select four L-shaped molds, cover the outside of the four molds with release cloth, and use a cleaning agent to wipe the outside of the release cloth clean for use; wherein, the release cloth is set in close contact with the outside of the mold to ensure that the contact surface between the mold covered with the release cloth and the fiber fabric is flat. The cleaning agent is ethanol or acetone. Figure 1As shown, the L-shaped mold includes a first side surface and a second side surface, the first side surface and the second side surface are vertically arranged, and the first side surface and the second side surface constitute the outer side wall of the L-shaped mold. The length of the first side surface is H1mm, and the length of the second side surface is H2mm. H1 and H2 are both positive numbers, the value range of H1 is 3mm-20mm, the value range of H2 is 150mm-750mm, and the specific values of H1 and H2 are set according to the needs.
[0028] Step S12: cutting the fiber fabric into the required size, placing the cut fiber fabric in an oven, and drying it at a preset drying temperature T0°C and a preset drying time t1; the preset drying temperature T0 ranges from 60°C to 120°C; the preset drying time t1 ranges from 0.5h to 4h.
[0029] In step S11, the material of the L-shaped mold includes any one or more materials selected from carbon steel, alloy steel, stainless steel, aluminum alloy, titanium alloy, PVC foam, and hardwood. This is beneficial to greatly reduce the cost of component preparation and improve the efficiency of component preparation. The surface of the L-shaped mold needs to be polished and smoothed, and the flatness of the L-shaped mold surface is ≤0.2mm.
[0030] The types of fiber fabrics in step S12 include any one or more of E-glass fiber fabrics, S-glass fiber fabrics, polyacrylonitrile-based carbon fiber fabrics, asphalt-based carbon fiber, boron fiber, Kevlar fiber, PBO fiber, silicon carbide fiber, and plant fiber. The types of polyacrylonitrile-based carbon fiber fabrics include any one or more of T300, T700, T800, T1000, M40, M45, and M50.
[0031] Through the setting of pretreatment, the preparation cycle can be shortened. The setting of the demoulding cloth can also facilitate the multiple use of the L-shaped mold and reduce the waste of resources. In addition, it is also convenient for the demoulding of the cross-shaped component to prevent the component from sticking to the mold, making it inconvenient to demould or causing damage to the component during the demoulding process. In addition, cleaning the demoulding cloth with a cleaning agent is conducive to improving the quality of the component and reducing the adhesion of impurities. By cutting the fiber fabric of the required size, it is conducive to increasing the speed of preparing the component and improving the efficiency of component preparation. This is conducive to preparing components with excellent mechanical properties under the premise of a shorter production cycle and lower production costs.
[0032] Step 2 includes: Step S21: laying fiber fabric: laying fiber fabric of a first size outside four L-shaped molds; and performing pre-pressing treatment; Step S22: any two L-shaped molds are taken as a group to form two groups of molds, and the outer sides of the two L-shaped molds in the two groups are arranged opposite to each other, that is, the two L-shaped molds in each group are arranged opposite to each other on the sides where the fiber fabric layer is laid; the fiber fabric of the second size is laid between the two L-shaped molds in the two groups of molds, and a pre-pressing treatment is performed; Step S23: After the two sets of molds are arranged opposite to each other, a fiber fabric of a third size is laid between the two sets of molds and pre-pressed to form a cross-shaped sample.
[0033] Among them, at least one layer of fiber fabric of the first size, fiber fabric of the second size, and fiber fabric of the third size are provided. The first size is the length of the outside of the bending part of the L-shaped mold, recorded as L1mm, L1=H1+H2+α1, the second size is recorded as L2mm, L2=H1+L1+α2, and the third size is recorded as L3mm, L3=2(H2+L1)+L2+α3. α1, α2, and α3 are all deviation values, L1, L2, and L3 are all positive numbers, and the specific values of L1, L2, L3, α1, α2, and α3 are set according to the needs. The number of pre-pressing treatment operations is 1-5 times, and the pre-pressing time for each time is 5min-30min.
[0034] The laying of fiber fabric will affect the final forming effect of the cross-rib products. Adjusting the uniformity of the cross ribs through pre-pressing during the laying process can effectively ensure the verticality of the two ribs in the component, which is beneficial to improving the flatness of the internal structure of the cross-shaped component, improving the quality of the cross-shaped component, and avoiding the possibility of defects in the internal structure of the cross-shaped component.
[0035] Step three includes: Step S31: vacuum-assisted processing: a glue injection pipeline is arranged below the cross-shaped sample, and at least one glue injection port is provided. Preferably, the number of the glue injection ports is 1-3; Step S32: a vacuum bag film is arranged on the outside of the cross-shaped sample, and at least one layer of the vacuum bag film is arranged, and each layer of the vacuum bag film is sealed; wherein the number of layers of the vacuum bag film is set to 1-2 layers; when sealing, the wrinkles generated by the vacuum bag film need to be arranged away from the surface of the product; Step S33: air tightness test: after the sealing of each layer of vacuum bag film is completed, the vacuum pump drives the vacuum pipe connected thereto to evacuate the inside of the vacuum bag film. After the vacuum pump works stably, the working air pressure inside the vacuum bag film is K1. The vacuum pump is turned off. After the preset pressure holding time t2, the air pressure inside the vacuum bag film is tested. Step S34: Determine whether the current air pressure K2 inside the vacuum bag film is ≤ the preset air pressure value K0. If yes, the air tightness of the vacuum bag film is qualified, and execute step 4; if no, the air tightness of the vacuum bag film is unqualified, and return to step S32.
[0036] Among them, K1≤-0.097Mpa, the preset holding time t2 has a value range of 5min-20min; and the preset air pressure value K0 is -0.095MPa.
[0037] Through the setting of vacuum-assisted processing, the setting of glue injection pipeline can pave the way for the subsequent preparation of cross-shaped components, which is convenient for the glue injection operation of the components. Setting the glue injection pipeline below the cross-shaped component can also help to avoid the glue injection pipeline from exerting pressure on the surface of the cross-shaped component, thereby affecting the flatness of the component. Through airtightness testing, it can help to prevent glue leakage during the glue injection process, which can not only ensure the safety and stability of component preparation, but also save resources.
[0038] Step 4 includes: Step S41: vacuum infusion treatment: select resin and additives as required; Step S42: according to the selected resin type and auxiliary agent type, the resin is prepared in a required proportion, and after being stirred evenly, it is allowed to stand for defoaming and then used for later use; Step S43: using a vacuum infusion process to inject the spare resin into the cross-shaped sample inside the vacuum bag film through the injection tube.
[0039] Among them, the resin types in step S41 include any one or more of epoxy resin, cyanate resin, bismaleimide resin, vinyl ester resin, polyurethane resin, phenolic resin, silicone resin, polyimide resin, polyethylene resin, polypropylene resin, polystyrene resin, polycarbonate resin, polyvinyl chloride resin, and polyamide resin.
[0040] Injecting resin by vacuum infusion can help reduce defects in the components to be prepared, improve the surface quality of the components, enhance the structural strength of the components, while ensuring that the components are light in weight, improve the production efficiency of component preparation, enhance the repeatability of the component preparation method, and also help reduce pollution and protect the environment.
[0041] Step five includes: Step S51: curing and demoulding: curing and post-curing treatment are performed according to the curing process recommended by the selected resin to obtain a cross-shaped test piece; Step S52: removing vacuum auxiliary equipment, namely removing the release cloth, vacuum bag film, glue injection pipeline, and L-shaped mold; Step S53: removing the flash on the cross-shaped specimen to obtain a cross-shaped component; Step S54: Check the molding quality of the cross-shaped component to determine whether the prepared cross-shaped component meets any one or more defects of no bubbles and no glue deficiency. If yes, the desired cross-shaped component is obtained; otherwise, the prepared cross-shaped component is unqualified.
[0042] In step S54, the length H3 of the ribs in the cross-shaped member of the fiber-reinforced resin-based composite material is in the range of 5 mm to 40 mm. Figure 3 As shown; the height H4 of the cross-shaped member ranges from 60mm to 80mm; the total length H5 of the cross-shaped member ranges from 300mm to 1500mm.
[0043] It should be noted that by selecting different fiber fabrics and resin types, fiber-reinforced resin-based composite cross-shaped components with different mechanical properties can be prepared.
[0044] By curing according to the curing process recommended by the selected resin, targeted curing treatment is carried out, which is beneficial to improving the curing efficiency of the component. After removing the vacuum auxiliary equipment, component quality inspection is carried out, which is beneficial to avoid the mixing of unqualified components and improve the qualification rate of the components.
[0045] Example 1
[0046] Step 1: Wrap four simple L-shaped molds made of alloy steel with demoulding cloth, and ensure that the surface in contact with the fiber fabric is flat, then wipe the surface clean with ethanol for standby use; among them, the dimensions of the four simple L-shaped molds are H1 8mm, height 90mm, and H2 150mm.
[0047] Cut the E-glass fiber fabric to match the dimensions of the L-shaped mold, and place it in an oven at 60°C-100°C for 1h-5h; Step 2: Fabric laying: First, lay 5-15 layers of fabric of appropriate size on four L-shaped molds, then use two L-shaped molds as a group, lay 5-20 layers of fabric between the two molds, and then lay 5-15 layers of fabric between the two groups. The schematic diagram of fabric laying is as follows: Figure 2a-2d As shown, the pre-pressing is performed 1-3 times during the spreading process, the pre-pressing time is 10min-20min, and the uniformity of the cross ribs is adjusted during the pre-pressing process. The prepared cross rib length H3 is between 3mm-15mm; Step 3: Pipeline setting and vacuum bag film sealing: The injection tube is arranged along the bottom of the cross-shaped component, and the number of injection ports is set to 1-3; 1-2 layers of bag film are used for sealing. When sealing, it is necessary to prevent the wrinkles of the vacuum bag film from appearing on the surface of the product.
[0048] Air tightness test: After the bag film is sealed, an air tightness test is carried out. After the vacuum pump works stably, the pressure is ≤-0.097MPa. After the vacuum pump is turned off and the pressure is maintained for 5min-30min, the pressure is ≤-0.095MPa, which is considered qualified. Step 4: Resin preparation and infusion: According to the selected type of epoxy resin that can be cured at room temperature and the corresponding curing agent, the resin is prepared in a certain proportion, stirred evenly, and then allowed to stand for defoaming and standby, and the preparation is carried out by vacuum infusion process; Step 5. Curing and demoulding: Carry out curing and post-curing treatment according to the curing process recommended by the resin, then remove the vacuum auxiliary materials and flash, check the molding quality of the test piece to ensure that there are no bubbles, glue deficiency or any one or more defects, and obtain the required cross-shaped component.
[0049] Example 2
[0050] Step 1: Wrap four simple L-shaped molds made of PVC foam with release cloth, and ensure that the surface in contact with the fiber fabric is flat, then wipe the surface clean with ethanol for standby use; the dimensions of the four simple L-shaped molds are H1 20 mm, height 90 mm, and H2 1500 mm.
[0051] Cut the S-shaped glass fiber fabric to match the dimensions of the L-shaped mold, and place it in an oven at 60°C-100°C for 1h-5h; Step 2: Fabric laying: First, lay 5-15 layers of fabric of appropriate size on four L-shaped molds, then use two L-shaped molds as a group, lay 5-20 layers of fabric between the two molds, and then lay 5-15 layers of fabric between the two groups. The schematic diagram of fabric laying is as follows: Figure 2a-2d As shown, the pre-pressing is performed 1-3 times during the spreading process, the pre-pressing time is 10min-20min, and the uniformity of the cross ribs is adjusted during the pre-pressing process. The thickness of the prepared cross ribs is between 3mm-15mm; Step 3: Pipeline setting and vacuum bag film sealing: The injection tube is arranged along the bottom of the cross-shaped component, and the number of injection ports is set to 1-3; 1-2 layers of bag film are used for sealing. When sealing, it is necessary to prevent the wrinkles of the vacuum bag film from appearing on the surface of the product.
[0052] Air tightness test: After the bag film is sealed, an air tightness test is carried out. After the vacuum pump works stably, the pressure is ≤-0.097MPa. After the vacuum pump is turned off and the pressure is maintained for 5min-30min, the pressure is ≤-0.095MPa, which is considered qualified. Step 4: Resin preparation and infusion: According to the selected high-strength vinyl ester resin type and the corresponding curing agent, the resin is prepared in a certain proportion, stirred evenly, and then allowed to stand for defoaming and standby, and the preparation is carried out by vacuum infusion process; Step 5. Curing and demoulding: Carry out curing and post-curing treatment according to the curing process recommended by the resin, then remove the vacuum auxiliary materials and flash, check the molding quality of the test piece to ensure that there are no bubbles, glue deficiency or any one or more defects, and obtain the required cross-shaped component.
[0053] Example 3
[0054] Step 1: Wrap four simple L-shaped molds made of aluminum alloy with demoulding cloth, and make sure that the surface in contact with the fiber fabric is flat. Wipe the surface with ethanol for later use; the dimensions of the four simple L-shaped molds are H1 10mm, height 90mm, and H2 150mm.
[0055] Cut T300 grade carbon fiber fabric to match the L-shaped size and place it in an oven at 60℃-100℃ for 1h-5h; Step 2: Fabric laying: First, lay 5-15 layers of fabric of appropriate size on four L-shaped molds, then use two L-shaped molds as a group, lay 5-20 layers of fabric between the two molds, and then lay 5-15 layers of fabric between the two groups. The schematic diagram of fabric laying is as follows: Figure 2a-2d As shown, the pre-pressing is performed 1-3 times during the spreading process, the pre-pressing time is 10min-20min, and the uniformity of the cross ribs is adjusted during the pre-pressing process. The thickness of the prepared cross ribs is between 3min-15mm; Step 3: Pipeline setting and vacuum bag film sealing: The injection tube is arranged along the bottom of the cross-shaped component, and the number of injection ports is set to 1-3; 1-2 layers of bag film are used for sealing. When sealing, it is necessary to prevent the wrinkles of the vacuum bag film from appearing on the surface of the product.
[0056] Air tightness test: After the bag film is sealed, an air tightness test is carried out. After the vacuum pump works stably, the pressure is ≤-0.097MPa. After the vacuum pump is turned off and the pressure is maintained for 5-30 minutes, the pressure is ≤-0.095MPa, which is considered qualified. Step 4: Resin preparation and infusion: According to the selected high-strength vinyl ester resin type and the corresponding curing agent, the resin is prepared in a certain proportion, stirred evenly, and then allowed to stand for defoaming and standby, and the preparation is carried out by vacuum infusion process; Step 5. Curing and demoulding: Carry out curing and post-curing treatment according to the curing process recommended by the resin, then remove the vacuum auxiliary materials and flash, check the molding quality of the test piece to ensure that there are no bubbles, glue deficiency or any one or more defects, and obtain the required cross-shaped component.
[0057] Example 4
[0058] Step 1: Wrap four simple L-shaped molds made of carbon steel with demoulding cloth, and ensure that the surface in contact with the fiber fabric is flat, then wipe the surface clean with ethanol for standby use; the dimensions of the four simple L-shaped molds are H1 8mm, height 90mm, and H2 150mm.
[0059] Cut T700 grade carbon fiber fabric to match the L-shaped size and place it in an oven at 80℃-120℃ to dry for 1h-5h; Step 2: Fabric laying: First, lay 5-15 layers of fabric of appropriate size on four L-shaped molds, then use two L-shaped molds as a group, lay 5-20 layers of fabric between the two molds, and then lay 5-15 layers of fabric between the two groups. The schematic diagram of fabric laying is as follows: Figure 2a-2d As shown, the pre-pressing is performed 1-3 times during the spreading process, the pre-pressing time is 10min-20min, and the uniformity of the cross ribs is adjusted during the pre-pressing process. The thickness of the prepared cross ribs is between 3min-15mm; Step 3: Pipeline setting and vacuum bag film sealing: The glue injection pipe is arranged along the bottom of the cross-shaped component, and the number of glue injection ports is set to 1-3; 1-2 layers of bag film are used for sealing. When sealing, it is necessary to prevent the wrinkles of the vacuum bag film from appearing on the surface of the product; Air tightness test: After the bag film is sealed, an air tightness test is carried out. After the vacuum pump works stably, the pressure is ≤-0.097MPa. After the vacuum pump is turned off and the pressure is maintained for 5-30 minutes, the pressure is ≤-0.095MPa, which is considered qualified. Step 4: Resin preparation and infusion: According to the selected high-strength vinyl ester resin type and the corresponding curing agent, the resin is prepared in a certain proportion, stirred evenly, and then allowed to stand for defoaming and standby, and the preparation is carried out by vacuum infusion process; Step 5. Curing and demoulding: Carry out curing and post-curing treatment according to the curing process recommended by the resin, then remove the vacuum auxiliary materials and flash, check the molding quality of the test piece to ensure that there are no bubbles, glue deficiency or any one or more defects, and obtain the required cross-shaped component.
[0060] Example 5
[0061] Step 1: Cover four simple L-shaped molds made of hardwood boards with release cloth, and ensure that the surface in contact with the fiber fabric is flat, then wipe the surface clean with ethanol for standby use; among them, the dimensions of the four simple L-shaped molds are H1 is 20mm, height is 90mm, and H2 is 150mm.
[0062] Cut the Kevlar fabric to match the L-shaped size and place it in an oven at 60℃-100℃ for 1h-5h; Step 2: Fabric laying: First, lay 5-15 layers of fabric of appropriate size on four L-shaped molds, then use two L-shaped molds as a group, lay 5-20 layers of fabric between the two molds, and then lay 5-15 layers of fabric between the two groups. The schematic diagram of fabric laying is as follows: Figure 2a-2dAs shown, the pre-pressing is performed 1-3 times during the spreading process, the pre-pressing time is 10min-20min, and the uniformity of the cross ribs is adjusted during the pre-pressing process. The thickness of the prepared cross ribs is between 3min-15mm; Step 3: Pipeline setting and vacuum bag film sealing: The glue injection pipe is arranged along the bottom of the cross-shaped component, and the number of glue injection ports is set to 1-3; 1-2 layers of bag film are used for sealing. When sealing, it is necessary to prevent the wrinkles of the vacuum bag film from appearing on the surface of the product; Air tightness test: After the bag film is sealed, an air tightness test is carried out. After the vacuum pump is working stably, the pressure is ≤-0.097MPa. After the vacuum pump is turned off and the pressure is maintained for 5-30 minutes, the pressure is ≤-0.095MPa, which is considered qualified. Step 4: Resin preparation and infusion: According to the selected low-viscosity room-temperature curing epoxy resin type and the corresponding curing agent, the resin is prepared in a certain proportion, stirred evenly, and then allowed to stand for defoaming and standby, and the preparation is carried out by vacuum infusion process; Step 5. Curing and demoulding: Carry out curing and post-curing treatment according to the curing process recommended by the resin, then remove the vacuum auxiliary materials and flash, check the molding quality of the test piece to ensure that there are no bubbles, glue deficiency or any one or more defects, and obtain the required cross-shaped component.
[0063] Comparative Example: First, two T-shaped components are prepared using a required mold, and then the two prepared T-shaped components are bonded using an adhesive to obtain the required cross-shaped component.
[0064] By measuring the mechanical properties of the cross-shaped components prepared in Examples 1-5 and the comparative example, the maximum tensile force value data of the cross-shaped components of different systems were obtained, as shown in Table 1 below: Table 1
[0065] It can be seen from Table 1 that the maximum tensile force value of the cross-shaped member prepared by the preparation method of the present application is much greater than the maximum tensile force value of the cross-shaped member prepared by bonding T-shaped members commonly used in the prior art. Therefore, it is further explained that the cross-shaped member prepared in the present application has good tensile properties and can solve the problem of poor mechanical properties faced by the preparation of cross-shaped members in the prior art.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite cross-shaped component by vacuum-assisted molding, characterized in that: The method comprises the following steps: Step 1: Pretreatment: Select at least four L-shaped molds and cut the fiber fabric into the required size; Step 2, fiber fabric laying: laying the fiber fabrics in sequence, and during the laying process, pre-pressing the laid fiber fabrics at least once to form a cross-shaped sample; Step 3: Vacuum-assisted treatment: Lay out a glue injection pipeline under the cross-shaped sample, and place a vacuum bag film on the outside of the cross-shaped sample for sealing, and then perform an airtightness test; Step 4: Vacuum infusion treatment: prepare the resin and perform vacuum infusion treatment; Step 5, curing and demoulding: After curing through the curing process, remove the vacuum auxiliary equipment to obtain the required cross-shaped component.
2. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 1, characterized in that: The step one comprises: Step S11: Pretreatment: Select four L-shaped molds, cover the outer sides of the four molds with release cloths, and wipe the outer sides of the release cloths with a cleaning agent for standby use; Step S12: cutting the fiber fabric into a required size, placing the cut fiber fabric in an oven, and drying it at a preset drying temperature T0° C. and a preset drying time t1.
3. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 2, characterized in that: The L-shaped mold comprises a first side surface and a second side surface, the first side surface and the second side surface are vertically arranged, and the first side surface and the second side surface constitute an outer side wall of the L-shaped mold.
4. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 3, characterized in that: The length of the first side surface is H1 mm, and the length of the second side surface is H2 mm; H1 and H2 are both positive numbers, the value range of H1 is 3 mm-20 mm, and the value range of H2 is 150 mm-750 mm.
5. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 2, characterized in that: The preset drying temperature T0 has a value range of 60° C.-120° C.; the preset drying time t1 has a value range of 0.5 h-4 h.
6. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 2, characterized in that: In the step S11, the material of the L-shaped mold includes any one or more materials selected from the group consisting of carbon steel, alloy steel, stainless steel, aluminum alloy, titanium alloy, PVC foam, and hardwood.
7. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 2, characterized in that: The second step comprises: Step S21: laying fiber fabric: laying fiber fabric of a first size outside four L-shaped molds; and performing pre-pressing treatment; Step S22: taking any two L-shaped molds as a group to form two sets of molds, arranging the outer sides of the two L-shaped molds in the two sets opposite to each other; laying fiber fabrics of the second size between the two L-shaped molds in the two sets of molds respectively, and performing pre-pressing treatment; Step S23: After the two sets of molds are arranged opposite to each other, a fiber fabric of a third size is laid between the two sets of molds and pre-pressed to form a cross-shaped sample.
8. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 7, characterized in that: The fiber fabric of the first size, the fiber fabric of the second size, and the fiber fabric of the third size are all provided with at least one layer.
9. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 7, characterized in that: The step three comprises: Step S31: vacuum-assisted processing: laying out a glue injection pipeline under the cross-shaped sample; Step S32: a vacuum bag film is arranged on the outside of the cross-shaped sample, and at least one layer of the vacuum bag film is arranged, and each layer of the vacuum bag film is sealed; when sealing, the wrinkles of the vacuum bag film need to be arranged away from the surface of the product; Step S33: air tightness test: the vacuum pump drives the vacuum pipe connected to it to evacuate the inside of the vacuum bag film. After the vacuum pump works stably, the working air pressure inside the vacuum bag film is K1. The vacuum pump is turned off. After the preset pressure holding time t2, the air pressure inside the vacuum bag film is tested. Step S34: Determine whether the current air pressure K2 inside the vacuum bag film is ≤ the preset air pressure value K0. If yes, the air tightness of the vacuum bag film is qualified, and execute step 4; if no, the air tightness of the vacuum bag film is unqualified, and return to step S32.
10. The method for preparing a composite material cross-shaped component by vacuum-assisted molding according to claim 9, characterized in that: The K1≤-0.097Mpa.
Citation Information
Patent Citations
Process for manufacturing preform and apparatus therefor
CN101394988A
Integral forming method for sewing enhanced cross connector made of fiber reinforced resin matrix composite
CN103407171A
High-efficiency integrally-forming method of T-shaped joint made of fiber reinforced resin matrix composites
CN103407172A
Exotensioned structural members with energy-absorbing effects
CN103518025A
Method for increasing fiber volume content of vacuum infusion composite product
CN107322953A
Cited By
Composite material cross I-beam and forming die and manufacturing method thereof
CN119820885A