Preparation method of low-hydroxyl high-purity quartz sand
Through low-temperature freeze-thaw-microwave-assisted thermal shock and surface esterification processes, the problem of difficult removal of structural impurities in quartz ore was solved, and high-purity low-hydroxyl quartz sand was successfully prepared, achieving the goals of high purity and low impurity content.
Patent Information
- Application Number
- CN202410761389.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technology is difficult to effectively remove structural impurities present in quartz ore, especially water molecules and hydroxyl water in gas-liquid inclusions, resulting in high hydroxyl content in high-purity quartz sand, making it difficult to achieve high-purity preparation.
Using low-temperature freeze-thaw-microwave-assisted thermal shock combined with surface esterification process, cracks are generated through rapid cooling and rapid heat treatment, which promotes the escape of water molecules and hydroxyl water in the gas-liquid inclusion, and is separated through the esterification reaction. The final step is microwave calcination to remove the ester. base to prepare low-hydroxyl and high-purity quartz sand.
It achieves high-purity preparation with silica content ≥99.99%, hydroxyl content ≤5ppm, and total impurity content ≤15ppm in quartz sand, avoiding the use of harmful HF and nitric acid, and is environmentally friendly.
Smart Images

Figure CN118754130A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-purity quartz sand production, and specifically relates to a method for preparing low-hydroxyl high-purity quartz sand. Background Art
[0002] High-purity quartz sand refers to quartz sand with a silicon dioxide content of more than 99.9%. Due to its unique physical and chemical properties, it occupies a pivotal position in aviation, aerospace, electronics, machinery and today's rapidly developing IT industry. In particular, its inherent molecular chain structure, crystal shape and lattice change law make it resistant to high temperatures, have a small thermal expansion coefficient, high insulation, corrosion resistance, piezoelectric effect, resonance effect and its unique optical properties, playing an increasingly important role in many high-tech products.
[0003] However, quartz ore contains more impurities, which can be divided into structural impurities and non-structural impurities. Non-structural impurities are impurities outside the quartz ore crystals, such as surface adhesions and associated minerals. At present, impurity removal technologies such as water quenching, flotation, pickling, magnetic separation, chlorination, electrostatic separation, ultrasonic treatment, doping purification and other series of means can basically meet the requirements of quartz glass. Structural impurities refer to impurities formed during the growth of quartz ore crystals, also known as microscopic defects, such as gas-liquid inclusions and lattice impurity ions. It is difficult to fundamentally eliminate such defects with existing process technologies. There are two forms of water in quartz ore. In addition to the water molecule form in the gas-liquid inclusions, the other is in the form of (OH) - The water in the quartz crystal structure is the main factor in the formation of quartz glass bubbles and impurity defects. The residual hydroxyl content of quartz glass after dehydroxylation increases with the increase of water molecules and structural water content in the raw materials. Therefore, the hydroxyl water (OH) in the gas-liquid inclusion - The removal of water molecules in gas-liquid inclusions is the key and difficulty in the preparation of high-purity quartz sand. Currently, differential corrosion and thermal explosion methods are mainly used to remove water molecules in gas-liquid inclusions, but the removal effect is not very ideal. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing low-hydroxyl high-purity quartz sand to solve the problem of high hydroxyl content in high-purity quartz sand.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing low-hydroxyl high-purity quartz sand comprises the following steps:
[0007] S1. Crushing and grinding: crushing and wet grinding the quartz sand raw material into 200-300 mesh quartz sand;
[0008] S2. Magnetic separation: quartz sand is magnetically separated to remove magnetic impurities;
[0009] S3. Pickling: Add the mixed acid solution to the quartz sand obtained in S2, stir for 3-5h at 70-90°C, and collect the acid-washed quartz sand by filtration;
[0010] S4. Low temperature freeze-thaw-microwave assisted thermal shock: The acid washed quartz sand obtained in S3 is immersed in liquid nitrogen for low temperature treatment for 3-5 minutes, then taken out and placed in a high temperature furnace with microwave function, heated to 900-1200°C, and then calcined at a constant temperature for 0.5-1.5h; the above operation is repeated twice;
[0011] S5. Surface esterification: The quartz sand obtained in S4 is added to DMSO containing propionic anhydride, and an acid solution is added to adjust the pH to 4-6. After stirring the reaction at 70-90° C. and vacuum conditions for 12-14 hours, the esterified quartz sand is separated and collected;
[0012] S6. High temperature calcination: Place the esterified quartz sand in a vacuum calcination furnace, raise the temperature to 1400-1450°C, calcine at a constant temperature for 2-4 hours under inert atmosphere conditions, and then cool naturally to room temperature (25-30°C) to obtain low-hydroxyl high-purity quartz sand.
[0013] Furthermore, the magnetic field strength of the magnetic separation in S2 is 100-10000GS.
[0014] Furthermore, the mixed acid solution in S3 is a solution formed by mixing 1M oxalic acid and 1M hydrochloric acid in a volume ratio of 1:1.
[0015] Furthermore, the heating rate in S4 is 20-40°C / s.
[0016] Furthermore, the microwave output power in S4 is 2500W and the frequency is 2.45GHz±25Hz.
[0017] Furthermore, the usage ratio of quartz sand, propionic anhydride and DMSO in S5 is 100g:12-20g:1L.
[0018] Furthermore, the acid in S5 includes hydrochloric acid or sulfuric acid.
[0019] Furthermore, the stirring speed in S5 is 200-400 rpm.
[0020] Furthermore, the heating rate in S6 is 20-40°C / s.
[0021] Furthermore, the inert atmosphere in S6 includes nitrogen or argon.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention provides a method for preparing low-hydroxyl high-purity quartz sand, wherein the prepared quartz sand has a silicon dioxide content of ≥99.99%, a hydroxyl content of ≤5ppm, and a total impurity content of ≤15ppm.
[0024] 2. The present invention adopts low-temperature freeze-thaw-microwave-assisted thermal shock to rapidly cool and heat the quartz sand after magnetic separation, so that a huge temperature difference is generated inside the quartz, and freeze-thaw cracks are generated in the quartz through freeze-thaw. After high-frequency electromagnetic wave-assisted heating, a huge pressure is generated at the interface between the gas-liquid inclusions in the quartz sand and the quartz matrix, so that the gas-liquid inclusions burst and further generate a large number of cracks at the interface; low-temperature freeze-thaw and electromagnetic wave-assisted heating are performed again, cracks are generated around the gas-liquid inclusions, and the width and depth of the cracks are increased, and the gas-liquid inclusions effectively escape from the microcracks, so that the water molecules and hydroxyl water (OH) in the gas-liquid inclusions - With SiO 2 The hydroxyl groups formed by the reaction are loaded onto the quartz surface, increasing the hydroxyl content on the quartz surface. At this time, the electronegativity of the quartz surface increases, and the solid affinity of quartz is strong; that is to say, the first low-temperature freeze-thaw-microwave-assisted thermal shock creates larger gas-liquid inclusions inside the quartz sand, and the second low-temperature freeze-thaw-microwave-assisted thermal shock widens and deepens the cracks inside the quartz sand, causing smaller gas-liquid inclusions to crack and escape, thereby loading hydroxyl water in the form of hydroxyl groups; surface esterification is then used to allow the hydroxyl groups on the surface of the quartz sand to undergo an esterification reaction with the carbonyl groups in propionic anhydride to generate esters and water, thereby separating the quartz sand to obtain esterified quartz sand; finally, microwave one-step calcination is used to remove the ester groups on the quartz surface by high-temperature thermal decomposition, thereby obtaining a low-hydroxyl, high-purity quartz sand product.
[0025] 3. The present invention adopts fluorine-free and nitrate-free acid leaching, which effectively avoids the harm to the environment caused by fluorine ions in HF and nitrate ions in nitric acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The present invention will be further described below in conjunction with the accompanying drawings.
[0027] Figure 1 The present invention is a schematic diagram of the preparation process of low-hydroxyl high-purity quartz sand. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] A method for preparing low-hydroxyl high-purity quartz sand comprises the following steps:
[0030] S1. Crushing and grinding: crushing and wet grinding the quartz sand raw material into 200-300 mesh quartz sand;
[0031] S2. Magnetic separation: quartz sand is magnetically separated at a magnetic field strength of 100-10000GS to remove magnetic impurities;
[0032] S3. Pickling: Add a mixed acid solution (a solution prepared by mixing 1M oxalic acid and 1M hydrochloric acid in a volume ratio of 1:1) to the quartz sand obtained in S2, stir for 3-5h at 70-90°C, and collect the acid-washed quartz sand by filtration;
[0033] S4. Low temperature freeze-thaw-microwave assisted thermal shock: The quartz sand obtained in S2 was immersed in liquid nitrogen for low temperature treatment for 3-5 minutes, then taken out and placed in a high temperature furnace with microwave function, and heated to 900-1200°C at a rate of 20-40°C / s, and then calcined at a constant temperature for 0.5-1.5h; the above operation was repeated twice; the microwave output power was 2500W, and the frequency was 2.45GHz±25Hz;
[0034] S5. Surface esterification: add the quartz sand obtained in S4 to DMSO containing propionic anhydride, add acid solution to adjust the pH to 4-6, stir and react at 70-90°C and vacuum conditions at a speed of 200-400 rpm for 12-14 hours, and separate and collect the esterified quartz sand; the amount ratio of quartz sand, propionic anhydride and DMSO is 100g:12-20g:1L;
[0035] S6. High temperature calcination: Place the esterified quartz sand in a vacuum calcination furnace, heat it to 1400-1450°C at a rate of 20-40°C / s, calcine it at a constant temperature for 2-4 hours under an inert atmosphere, and then cool it naturally to room temperature to obtain low-hydroxyl high-purity quartz sand.
[0036] In the following examples and comparative examples, the quartz sand raw material is SiO 2 Raw materials with a content of ≤99.000% and a hydroxyl content of ≥500ppm.
[0037] Example 1
[0038] A method for preparing low-hydroxyl high-purity quartz sand comprises the following steps:
[0039] S1. Crushing and grinding: crushing the quartz sand raw material into 250 mesh quartz sand by wet grinding;
[0040] S2. Magnetic separation: quartz sand is magnetically separated at a magnetic field strength of 5000GS to remove magnetic impurities;
[0041] S3. Pickling: Add a mixed acid solution (a solution prepared by mixing 1M oxalic acid and 1M hydrochloric acid in a volume ratio of 1:1) to the quartz sand obtained in S2, stir at 80°C for 4h, and collect the acid-washed quartz sand by filtration;
[0042] S4. Low temperature freeze-thaw-microwave assisted thermal shock: The acid-washed quartz sand obtained in S3 was immersed in liquid nitrogen for low temperature treatment for 4 minutes, then taken out and placed in a high temperature furnace with microwave function, heated to 1100°C at a rate of 30°C / s, and then calcined at a constant temperature for 1 hour; the above operation was repeated twice; the microwave output power was 2500W, and the frequency was 2.45GHz±25Hz;
[0043] S5. Surface esterification: The quartz sand obtained in S4 was added to DMSO containing propionic anhydride, and dilute hydrochloric acid was added to adjust the pH to 5. The mixture was stirred at 80°C and vacuum at a speed of 300 rpm for 13 h, and the esterified quartz sand was separated and collected; the amount ratio of quartz sand, propionic anhydride and DMSO was 100 g:15 g:1 L;
[0044] S6. High-temperature calcination: Place the esterified quartz sand in a vacuum calcination furnace, raise the temperature to 1430°C at a rate of 30°C / s, calcine at a constant temperature for 3 hours under an inert atmosphere, and then cool naturally to room temperature to obtain low-hydroxyl high-purity quartz sand.
[0045] Example 2
[0046] A method for preparing low-hydroxyl high-purity quartz sand, wherein S1, S2, S3, S4 and S6 in the preparation process are the same as those in Example 1, except that:
[0047] S4. Low temperature freeze-thaw-microwave assisted thermal shock: The quartz sand obtained in S3 was immersed in liquid nitrogen for low temperature treatment for 4 minutes, then taken out and placed in a high temperature furnace with microwave function, heated to 1100°C at a rate of 20°C / s, and then calcined at a constant temperature for 1.5 hours; the above operation was repeated twice; the microwave output power was 2500W, and the frequency was 2.45GHz±25Hz;
[0048] The remaining steps remain unchanged.
[0049] Example 3
[0050] A method for preparing low-hydroxyl high-purity quartz sand, wherein S1, S2, S3, S4 and S6 in the preparation process are the same as those in Example 1, except that:
[0051] S4. Low temperature freeze-thaw-microwave assisted thermal shock: The quartz sand obtained in S3 was immersed in liquid nitrogen for low temperature treatment for 4 minutes, then taken out and placed in a high temperature furnace with microwave function, heated to 1100°C at a rate of 40°C / s, and then calcined at a constant temperature for 0.5h; the above operation was repeated twice; the microwave output power was 2500W, and the frequency was 2.45GHz±25Hz;
[0052] The remaining steps remain unchanged.
[0053] Example 4
[0054] A method for preparing low-hydroxyl high-purity quartz sand, wherein S1, S2, S3, S4 and S6 in the preparation process are the same as those in Example 1, except that:
[0055] S5. Surface esterification: Add the quartz sand obtained in S4 to DMSO containing propionic anhydride, add dilute hydrochloric acid to adjust the pH to 5, stir the reaction at 80°C and 300 rpm under vacuum conditions for 13 hours, and then separate and collect the esterified quartz sand; the dosage ratio of quartz sand, propionic anhydride and DMSO is 100g:12g:1L.
[0056] Example 5
[0057] A method for preparing low-hydroxyl high-purity quartz sand, wherein S1, S2, S3, S4 and S6 in the preparation process are the same as those in Example 1, except that:
[0058] S5. Surface esterification: The quartz sand obtained in S4 was added to DMSO containing propionic anhydride, and dilute hydrochloric acid was added to adjust the pH to 5. After stirring at 80°C and vacuum conditions at a speed of 300 rpm for 13 hours, the esterified quartz sand was separated and collected; the amount ratio of quartz sand, propionic anhydride and DMSO was 100 g: 20 g: 1 L;
[0059] The remaining steps remain unchanged.
[0060] Comparative Example 1
[0061] A method for preparing high-purity quartz sand, wherein S1, S2, S3, S5 and S6 in the preparation process are the same as those in Example 1, except that:
[0062] S4. Microwave-assisted thermal shock: The quartz sand obtained in S3 was placed in a high-temperature furnace with microwave function, heated to 1100°C at a rate of 30°C / s, and then calcined at a constant temperature for 1h; the above operation was repeated twice; the microwave output power was 2500W, and the frequency was 2.45GHz±25Hz.
[0063] The remaining steps remain unchanged.
[0064] Comparative Example 2
[0065] A method for preparing high-purity quartz sand, wherein S1, S2, S3, S5 and S6 in the preparation process are the same as those in Example 1, except that:
[0066] S4. Immerse the quartz sand obtained in S3 in liquid nitrogen for low-temperature treatment for 4 minutes, then take it out and repeat the above operation twice; the rest of the steps remain unchanged.
[0067] Comparative Example 3
[0068] A method for preparing high-purity quartz sand. In the preparation process, S1, S2, S3, S5 and S6 are the same as those in Example 1, except that S4 only undergoes one low-temperature freeze-thaw-microwave-assisted thermal shock; the other steps remain unchanged.
[0069] Comparative Example 4
[0070] A method for preparing high-purity quartz sand, wherein S1, S2, S3, S4 and S6 in the preparation process are the same as those in Example 1, except that:
[0071] S5. The quartz sand obtained in S4 is added to DMSO, and dilute hydrochloric acid is added to adjust the pH to 5. After stirring at 80°C and vacuum conditions at a speed of 300 rpm for 13 hours, the quartz sand is separated and collected; the amount ratio of quartz sand to DMSO is 100 g: 1 L;
[0072] The remaining steps remain unchanged.
[0073] Comparative Example 5
[0074] A method for preparing low-hydroxyl high-purity quartz sand comprises the following steps:
[0075] S1. Crushing and grinding: crushing the quartz sand raw material into 250 mesh quartz sand by wet grinding;
[0076] S2. Calcination-water quenching: the temperature was raised by 6°C per minute from room temperature to 500°C, and by 3°C per minute from 500°C. The calcination temperature was maintained at 750°C for 30 minutes, at 900°C for 30 minutes, and at 1300°C for 30 minutes. Then, the quartz sand was rinsed with 0°C water for 60 seconds, and then the quartz sand was placed in 20°C water for 10 minutes while applying ultrasound.
[0077] S3. Pickling - drying: The quartz sand was soaked in a 60wt% acetic acid solution containing 4wt% ethylenediaminetetraacetic acid for pickling, the pH value of the solution was 4, the temperature was 50°C, ultrasound was applied and the solution was stirred for 4 hours, the quartz sand was separated by filtration, the quartz sand was rinsed three times with deionized water, the quartz sand was dried at 300°C for 2 hours and then cooled to room temperature;
[0078] S4. Surface esterification: The quartz sand obtained in S3 was added to anhydrous ether containing propionic anhydride, and dilute hydrochloric acid was added to adjust the pH to 5. The mixture was stirred at 80°C and vacuum conditions at a speed of 300 rpm for 13 h, and the esterified quartz sand was separated and collected; the amount ratio of quartz sand, propionic anhydride and anhydrous ether was 100 g:15 g:1 L;
[0079] S5. Calcination: Place quartz sand in a calcination furnace filled with nitrogen, and use programmed temperature increase from room temperature to 1100°C per minute at 8°C, and from 1100°C per minute at 4°C. The calcination temperature is maintained at 1200°C for 20 minutes and at 1300°C for 30 minutes, and then cooled to room temperature in a nitrogen atmosphere.
[0080] Comparative Example 6
[0081] A method for preparing high-purity quartz sand, wherein S1, S2, S3, S5 and S6 in the preparation process are the same as those in Example 1, except that S4 is subjected to three times of low-temperature freeze-thaw-microwave-assisted thermal shock; and the remaining steps remain unchanged.
[0082] The quartz sand products in Example 1 to Example 5 and Comparative Example 1 to Comparative Example 6 were tested, and the hydroxyl content was tested according to the method in GB / T12442-2019; SiO 2 The purity is tested according to GB / T3284-2015 method; the impurity elements are tested according to GB / T32650-2016 method; the test results are shown in Table 1:
[0083] Table 1
[0084] <![CDATA[SiO 2 (%)]]> Hydroxyl content (ppm) Total impurity content (ppm) Example 1 99.995 4.87 14.37 Example 2 99.997 4.83 14.28 Example 3 99.993 4.91 14.41 Example 4 99.994 4.91 14.33 Example 5 99.995 4.89 14.42 Comparative Example 1 99.828 13.24 31.63 Comparative Example 2 99.912 12.37 25.48 Comparative Example 3 99.944 10.64 19.27 Comparative Example 4 99.571 248.57 38.46 Comparative Example 5 99.995 6.68 16.81 Example 6 99.994 4.86 14.34
[0085] As can be seen from Table 1, the present invention uses two consecutive low-temperature freeze-thaw-microwave-assisted thermal shock treatments on quartz sand, which can effectively promote the deep cracking of gas-liquid inclusions, expand the depth and width of the cracks, and make the water molecules and hydroxyl water (OH) in the gas-liquid inclusions - With SiO 2 The hydroxyl groups formed by the reaction are loaded onto the quartz surface, thereby increasing the hydroxyl content on the quartz surface and the removal rate of hydroxyl groups in the quartz sand. The purity of the quartz sand finally prepared is ≥99.99%, the hydroxyl content is ≤5ppm, and the total impurity content is ≤15ppm.
[0086] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0087] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing low-hydroxyl high-purity quartz sand, It is characterized in that The following steps are involved: S1. Crushing and grinding: crushing and wet grinding the quartz sand raw material into 200-300 mesh quartz sand; S2. Magnetic separation: quartz sand is magnetically separated to remove magnetic impurities; S3. Pickling: Add the mixed acid solution to the quartz sand obtained in S2, stir for 3-5h at 70-90°C, and collect the acid-washed quartz sand by filtration; S4. Low temperature freeze-thaw-microwave assisted thermal shock: The acid washed quartz sand obtained in S3 is immersed in liquid nitrogen for low temperature treatment for 3-5 minutes, then taken out and placed in a high temperature furnace with microwave function, heated to 900-1200°C, and then calcined at a constant temperature for 0.5-1.5h; the above operation is repeated twice; S5. Surface esterification: The quartz sand obtained in S4 is added to DMSO containing propionic anhydride, and an acid solution is added to adjust the pH to 4-6. After stirring the reaction at 70-90° C. and vacuum conditions for 12-14 hours, the esterified quartz sand is separated and collected; S6. High temperature calcination: Place the esterified quartz sand in a vacuum calcination furnace, raise the temperature to 1400-1450°C, calcine at a constant temperature for 2-4 hours under inert atmosphere conditions, and then naturally cool to room temperature to obtain low-hydroxyl high-purity quartz sand.
2. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The magnetic field strength of the magnetic separation in S2 is 100-10000GS.
3. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The mixed acid solution in S3 is a solution of 1M oxalic acid and 1M hydrochloric acid mixed in a volume ratio of 1:
1.
4. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The heating rate in S4 and S6 is 20-40°C / s.
5. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The microwave output power in S4 is 2500W and the frequency is 2.45GHz±25Hz.
6. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The usage ratio of quartz sand, propionic anhydride and DMSO in S5 is 100g:12-20g:1L.
7. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The acid in S5 includes hydrochloric acid or sulfuric acid.
8. A method for preparing low-hydroxyl high-purity quartz sand according to claim 1, It is characterized in that The stirring speed in S5 is 200-400 rpm.
Citation Information
Cited By
High-purity quartz sand for semiconductor and preparation method of high-purity quartz sand
CN122324818A
High-purity quartz sand for semiconductor and method for producing the same
CN122324818B