Efficient utilization method of high-calcium metallic sodium generated by electrolytic preparation of metallic sodium

By reacting high-calcium metal sodium with anhydrous methanol and utilizing the coordination and complexation of polymeric ionic liquids, sodium methoxide and calcium hydroxide are separated, which solves the problem of high-calcium metal sodium waste treatment and improves the economic utilization efficiency of waste materials. , and realize the recycling of materials, which is green and environmentally friendly.

CN118754184APending Publication Date: 2024-10-11NINGXIA BEST PHARMACEUTICAL CHEMICAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411029657.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The high-calcium metallic sodium waste produced during the electrolytic preparation of metallic sodium is difficult to effectively utilize, and its disposal is highly dangerous. The existing technology has low separation efficiency, which affects economic benefits.

Method used

By reacting high-calcium metal sodium with anhydrous methanol to generate a mixed solution of sodium methoxide and calcium methoxide, and using the coordination and complexation of polymeric ionic liquids to perform distillation separation through boiling point difference, sodium methoxide and calcium hydroxide are obtained, realizing the metal Separation of sodium and calcium.

Benefits of technology

The utilization efficiency of high-calcium metallic sodium is improved. The generated sodium methoxide and calcium hydroxide can be used for alkaline catalyst and neutralization and solidification, realizing the economic utilization of waste materials. Methanol is recycled through hydrolysis to achieve a green and environmentally friendly material cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004969576750000061
    Figure BDA0004969576750000061
Patent Text Reader

Abstract

The invention discloses an efficient utilization method of high-calcium metal sodium generated in the process of preparing metal sodium through electrolysis, and belongs to the field of metal waste residue recovery treatment in the fields of non-ferrous metal industry and chemical industry. Comprising the following steps: putting high-calcium metal sodium into a reaction kettle, adding absolute methanol under the protection of inert gas, mixing and reacting to obtain a mixed solution of sodium methoxide and calcium methoxide; adding a polymeric ionic liquid into the mixed solution, mixing and stirring at 30-40 DEG C, and then carrying out distillation separation to obtain a complex of sodium methoxide and calcium methoxide; and mixing and stirring the complex of calcium methoxide and water, and filtering and separating to obtain calcium hydroxide. Methanol reacts with high-calcium metal sodium to prepare a mixed solution of sodium methoxide and calcium methoxide, then coordination complexation of polymeric ionic liquid and calcium methoxide is utilized, sodium methoxide is obtained through distillation, a complex of residual calcium methoxide is hydrolyzed to obtain calcium hydroxide, and separation of metal sodium and metal calcium in the high-calcium metal sodium is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal waste slag recovery and treatment in the fields of non-ferrous metal industry and chemical industry, and specifically relates to a method for efficiently utilizing high-calcium metallic sodium generated in the process of electrolyzing metallic sodium. Background Art

[0002] As an important industrial raw material and chemical reagent, sodium metal is widely used in many fields, such as organic synthesis, metallurgy and nuclear industry. Sodium metal is an alkali metal element with active chemical properties and reducibility. It is mainly prepared from sodium chloride by molten salt electrolysis. This method is to melt sodium chloride at high temperature and separate sodium metal and chlorine by electrolysis. During the electrolysis process, the sodium chloride melt undergoes oxidation and reduction reactions at the anode and cathode respectively. The chloride ions on the anode lose electrons to generate chlorine, and the sodium ions on the cathode gain electrons to generate sodium metal. In order to improve the conductivity of the electrolyte and reduce the melting point of the molten salt, calcium chloride is often added as an auxiliary electrolyte. However, calcium chloride reacts with other components in the sodium chloride melt at high temperature, causing some calcium ions to enter the sodium metal to form high-calcium sodium metal waste. Because high-calcium sodium metal waste contains active sodium and calcium, it cannot be directly treated with water, resulting in high treatment risk and difficulty.

[0003] Patent CN116949515A discloses a method for preparing high-purity sodium and safely treating high-calcium sodium slag. The invention obtains high-purity sodium and high-calcium sodium slag by ultra-gravity separation of liquid sodium obtained by electrolysis. The high-calcium sodium slag is converted into sodium oxide and calcium oxide by high-temperature roasting, and then treated with low-concentration hydrated hydroxide alkali solution to obtain sodium hydroxide solution and calcium hydroxide solution, thereby realizing the treatment and utilization of high-calcium sodium slag.

[0004] Patent CN115852168A discloses a high-calcium sodium treatment process, which heats high-calcium sodium by electricity to make the calcium embrittled, and then separates the calcium from the sodium by a physical method of extrusion to increase the amount of sodium precipitation.

[0005] High-calcium metallic sodium will inevitably be produced during the preparation process of metallic sodium. The waste has great economic value. Therefore, studying a method to separate sodium and calcium in high-calcium metallic sodium and improving the utilization efficiency of high-calcium metallic sodium will significantly enhance the economic benefits of the enterprise. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention prepares a mixed solution of sodium methoxide and calcium methoxide by mixing high-calcium sodium metal with anhydrous methanol, and then uses the coordination complexation of polymerized ionic liquid and calcium methoxide to increase the boiling point of calcium methoxide, and distills the sodium methoxide by boiling point difference, and the remaining mixture of calcium methoxide and polymerized ionic liquid complexed to obtain calcium hydroxide by hydrolysis, thereby achieving the separation of metallic sodium and metallic calcium in high-calcium sodium metal, improving the utilization efficiency of high-calcium sodium metal waste, and solving the problems raised in the background technology. Specifically, the technical solution of the present invention includes the following content structure:

[0007] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, the method comprising the following steps:

[0008] Putting high calcium metal sodium into a reaction kettle, adding anhydrous methanol under the protection of inert gas for mixed reaction to obtain a mixed solution of sodium methoxide and calcium methoxide;

[0009] Adding polymeric ionic liquid to the mixed solution of sodium methoxide and calcium methoxide, mixing and stirring at 30° C. to 40° C., and then separating by distillation to obtain a complex of sodium methoxide and calcium methoxide;

[0010] The complex of calcium methoxide is mixed with water and stirred, and calcium hydroxide is obtained by filtration and separation.

[0011] Furthermore, the mass ratio of the high-calcium metallic sodium to the anhydrous methanol is 1:1-3.

[0012] Furthermore, the inert gas includes helium or nitrogen.

[0013] Furthermore, the preparation method of the polymeric ionic liquid comprises the following steps:

[0014] 1-vinyl imidazole and alkyl halide are mixed in an ether solution to form a reaction system, and the reaction system is subjected to a temperature-raising reaction to obtain an imidazole-based ionic liquid;

[0015] The imidazole-based ionic liquid and the unsaturated olefinic aldehyde are mixed in equal amounts and then reacted by a free radical initiator to obtain the polymerized ionic liquid.

[0016] Furthermore, the molar ratio of 1-vinylimidazole:alkyl halide is 1:1.

[0017] Furthermore, the alkyl halide includes 1-chloropropane or 2-chloropropane.

[0018] Furthermore, the conditions of the temperature-raising reaction include a reaction temperature of 70° C. to 80° C. and a reaction time of 12 h to 16 h.

[0019] Furthermore, the unsaturated olefinic aldehyde includes acrolein.

[0020] Furthermore, the free radical initiator includes azobisisobutyronitrile, benzoyl peroxide or azobisisoheptanenitrile.

[0021] Furthermore, the mass ratio of the free radical initiator to the unsaturated olefinic aldehyde is 0.02-0.03:1.

[0022] Furthermore, the conditions of the catalytic reaction include a reaction temperature of 60° C. to 80° C. and a reaction time of 6 h to 8 h.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention creatively utilizes anhydrous methanol to react with calcium and sodium metal elements in high-calcium sodium metal to obtain a mixed solution of sodium methoxide and calcium methoxide, the boiling points of which are relatively low and close. Then, based on the difference that calcium atoms have a metal coordination effect while sodium atoms do not have a metal coordination effect, the high thermal stability of ionic liquids is utilized to design a polymeric ionic liquid having a coordination effect with metal atoms. The boiling point of calcium methoxide is increased by the metal coordination complexation between the polymeric ionic liquid and calcium methoxide. The large boiling point difference is utilized to separate the complex of sodium methoxide and calcium methoxide to obtain sodium methoxide, and the complex of calcium methoxide is hydrolyzed to obtain calcium hydroxide and methanol, thereby achieving the separation of calcium and sodium in high-calcium sodium metal to obtain sodium methoxide that can be used as an alkaline catalyst and calcium hydroxide that can be used for neutralization and solidification, so that the high-calcium sodium metal waste generated by the molten electrolysis of metallic sodium is largely economically utilized, and the methanol generated in the preparation of calcium hydroxide can be reused in the reaction with high-calcium sodium metal after dehydration by distillation, thereby achieving the recycling of materials and being green and environmentally friendly.

[0025] (2) It can be seen from the results of Example 4 and Comparative Examples 1 to 3 that although the conventional imidazolyl ionic liquids 1-methyl-3-butyl imidazolyl chloride, 1-ethyl-3-methyl imidazolyl ethyl sulfate and 1-ethyl-3-methyl imidazolyl hexafluorophosphate contain atoms with strong coordination ability such as chlorine atoms, oxygen atoms and fluorine atoms, the coordination ability of chlorine atoms, oxygen atoms and fluorine atoms with calcium ions is weak after they are combined with cations through anion-cation bonds, and the effect of separating calcium methoxide from sodium methoxide is poor. Therefore, the present invention introduces aldehyde oxygen with a lone electron pair into the side chain of the imidazolyl ionic liquid through a polymerization reaction of a carbon-carbon double bond, thereby enhancing the coordination ability with calcium ions and thus improving the ability to separate calcium methoxide from sodium methoxide. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be clearly and completely described below through the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0027] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.

[0028] Preparation Example 1:

[0029] The preparation method of polymerized ionic liquid specifically comprises the following steps:

[0030] Weigh 10 mol of 1-vinyl imidazole and 10 mol of 1-chloropropane on a balance and place them in a three-necked flask, then add 1.5 L of ether solution and mix and stir to form a reaction system, then heat the reaction system to 70°C and time the reaction for 16 hours. After the reaction is completed, cool to room temperature to obtain an imidazole-based ionic liquid, take 1 kg of imidazole-based ionic liquid and mix with 1 kg of acrolein, then add 20 g of azobisisobutyronitrile and mix, then heat to 60°C and time the reaction for 6 hours, cool to room temperature after the reaction is completed, pour into a rotary evaporator for vacuum rotary evaporation to obtain a polymerized ionic liquid.

[0031] Preparation Example 2:

[0032] The preparation method of polymerized ionic liquid specifically comprises the following steps:

[0033] Weigh 10 mol of 1-vinyl imidazole and 10 mol of 1-chloropropane on a balance and place them in a three-necked flask, then add 1.5 L of ether solution and stir to form a reaction system, then heat the reaction system to 75°C and time the reaction for 18 hours. After the reaction is completed, cool to room temperature to obtain an imidazole-based ionic liquid, take 1 kg of imidazole-based ionic liquid and mix with 1 kg of acrolein, then add 25 g of azobisisoheptanenitrile and mix, then heat to 65°C and time the reaction for 6 hours, cool to room temperature after the reaction is completed, pour into a rotary evaporator for vacuum rotary evaporation to obtain a polymerized ionic liquid.

[0034] Preparation Example 3:

[0035] The preparation method of polymerized ionic liquid specifically comprises the following steps:

[0036] Weigh 10 mol of 1-vinyl imidazole and 10 mol of 2-chloropropane on a balance and place them in a three-necked flask, then add 1.5 L of ether solution and mix and stir to form a reaction system, then heat the reaction system to 75°C and time the reaction for 18 hours. After the reaction is completed, cool to room temperature to obtain an imidazole-based ionic liquid, take 1 kg of imidazole-based ionic liquid and mix with 1 kg of acrolein, then add 25 g of azobisisoheptanenitrile and mix and stir, then heat to 75°C and time the reaction for 7 hours, cool to room temperature after the reaction is completed, pour into a rotary evaporator for vacuum rotary evaporation to obtain a polymerized ionic liquid.

[0037] Preparation Example 4:

[0038] The preparation method of polymerized ionic liquid specifically comprises the following steps:

[0039] Use a balance to weigh 10 mol of 1-vinylimidazole and 10 mol of 2-chloropropane and place them in a three-necked flask, then add 1.5 L of ether solution and mix and stir to form a reaction system, then heat the reaction system to 80°C and time the reaction for 20 hours. After the reaction is completed, cool to room temperature to obtain an imidazole-based ionic liquid, take 1 kg of imidazole-based ionic liquid and 1 kg of acrolein, mix and stir, then add 30 g of benzoyl peroxide and mix and stir, then heat to 80°C and time the reaction for 8 hours, cool to room temperature after the reaction is completed, pour into a rotary evaporator for vacuum rotary evaporation to obtain a polymerized ionic liquid.

[0040] Preparation Example 5:

[0041] The preparation method of polymerized ionic liquid specifically comprises the following steps:

[0042] The acrolein in Preparation Example 4 was replaced by acrylic acid, and the other conditions remained the same as those in Preparation Example 4.

[0043] The thermal stability of the polymerized ionic liquids of Preparation Examples 1 to 5 was analyzed by a thermogravimetric analyzer. The thermogravimetric analysis test conditions were as follows: temperature range: 50°C to 600°C, heating rate: 50°C / min, atmosphere: 99.9% high-purity nitrogen, gas flow rate: 50 mL / min, and the weight retention of the polymerized ionic liquids was recorded at 50°C, 100°C, 150°C and 200°C, respectively. The results are shown in the following table:

[0044]

[0045] It can be seen from the results in the above table that polymeric ionic liquids have good thermal stability.

[0046] Embodiment 1:

[0047] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0048] 1 kg of high calcium sodium metal was put into a reactor, helium was introduced into the reactor to exhaust the air inside the reactor, and then 1 kg of anhydrous methanol was pumped into the reactor through a pipeline to mix with the high calcium sodium metal, stirred at a speed of 50 r / min for 15 minutes, cooled to 30°C for insulation, and then 1 kg of the polymerized ionic liquid of Preparation Example 1 was added and continued to be stirred at a speed of 50 r / min for 30 minutes at 30°C. After the stirring was completed, sodium methoxide was distilled and collected in an environment of 68°C. According to the test standard of "HG / T2561-2014 Industrial Grade Sodium Methanol Methanol Solution", the content of sodium methoxide was determined to be 29.4%, which met the requirements.

[0049] The remaining calcium methanol complex after the distillation is mixed with an equal volume of water and stirred until no white precipitate is produced, and then filtered to obtain a white filter residue. The white filter residue is placed in an oven at 50°C and dried for 10 hours to obtain white calcium hydroxide. The weight is weighed on a balance and the weight is 202.32 g. The calculated recovery rate is 20.23%. The calcium hydroxide content is determined to be 90.7% in accordance with the test standard "HG / T4120-2009 Industrial Calcium Hydroxide", which meets the requirements.

[0050] Embodiment 2:

[0051] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0052] 1 kg of high calcium sodium metal was put into the reactor, helium was introduced into the reactor to exhaust the air inside the reactor, and then 1 kg of anhydrous methanol was pumped into the reactor through a pipeline to mix with the high calcium sodium metal, stirred at a speed of 50 r / min for 20 minutes, cooled to 35°C for insulation, and then 1 kg of the polymerized ionic liquid of Preparation Example 2 was added and continued to be stirred at a speed of 50 r / min for 30 minutes at 35°C. After the stirring was completed, sodium methoxide was distilled and collected in an environment of 68°C. According to the test standard of "HG / T2561-2014 Industrial Grade Sodium Methanol Methanol Solution", the content of sodium methoxide was determined to be 29.7%, which met the requirements.

[0053] The remaining calcium methoxide complex after the distillation is mixed with an equal volume of water and stirred until no more white precipitate is produced, and then filtered to obtain a white filter residue, which is placed in an oven at 50°C and dried for 10 hours to obtain white calcium hydroxide, which is weighed on a balance to obtain a weight of 227.05 g. The calculated recovery rate is 22.71%, and the calcium hydroxide content is determined to be 92.5% in accordance with the test standard "HG / T4120-2009 Industrial Calcium Hydroxide", which meets the requirements.

[0054] Embodiment 3:

[0055] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0056] 1 kg of high calcium sodium metal was put into the reactor, nitrogen was introduced into the reactor to exhaust the air inside the reactor, and then 1 kg of anhydrous methanol was pumped into the reactor through a pipeline to mix with the high calcium sodium metal, stirred at a speed of 60 r / min for 25 min, cooled to 35° C. for insulation, and then 1 kg of the polymerized ionic liquid of Preparation Example 3 was added and continued to be stirred at a speed of 60 r / min for 35 min at 35° C. After the stirring was completed, sodium methoxide was distilled and collected in an environment of 70° C. According to the test standard of "HG / T2561-2014 Industrial Grade Sodium Methanol Methanol Solution", the content of sodium methoxide was determined to be 30.1%, which met the requirements.

[0057] The remaining calcium methoxide complex after the distillation is mixed with an equal volume of water and stirred until no white precipitate is produced, and then filtered to obtain a white filter residue. The white filter residue is placed in an oven at 50°C and dried for 12 hours to obtain white calcium hydroxide. The weight is weighed on a balance and the weight is 251.17 g. The calculated recovery rate is 25.12%. According to the test standard "HG / T4120-2009 Industrial Calcium Hydroxide", the content of calcium hydroxide is determined to be 93.1%, which meets the requirements.

[0058] Embodiment 4:

[0059] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0060] 1 kg of high calcium sodium metal was put into the reactor, nitrogen was introduced into the reactor to exhaust the air inside the reactor, and then 1 kg of anhydrous methanol was pumped into the reactor through a pipeline to mix with the high calcium sodium metal, stirred at a speed of 60 r / min for 30 min, cooled to 40°C for insulation, and then 1 kg of the polymerized ionic liquid of Preparation Example 4 was added and continued to be stirred at a speed of 60 r / min for 40 min at 40°C. After the stirring was completed, sodium methoxide was distilled and collected in an environment of 70°C, and the content of sodium methoxide was determined to be 30.2% according to the test standard of "HG / T2561-2014 Industrial Grade Sodium Methanol Solution" and met the requirements.

[0061] The remaining calcium methoxide complex after the distillation is mixed with an equal volume of water and stirred until no white precipitate is produced, and then filtered to obtain a white filter residue. The white filter residue is placed in an oven at 50°C and dried for 12 hours to obtain white calcium hydroxide. The weight is weighed on a balance to obtain a weight of 265.74 g, and the calculated recovery rate is 26.57%. According to the test standard "HG / T4120-2009 Industrial Calcium Hydroxide", the calcium hydroxide content is determined to be 93.7%, which meets the requirements.

[0062] Embodiment 5:

[0063] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0064] The polymerized ionic liquid in Example 4 was replaced with the polymerized ionic liquid of Preparation Example 5, and the other conditions were kept consistent with Example 4. The sodium methoxide content was measured to be 11.8%, which was quite different from the standard content range; the weight of calcium hydroxide was 209.41g, the recovery rate was 20.94%, and the content of calcium hydroxide was 71.26%, which was quite different from the use standard of industrial sodium hydroxide. Sodium methoxide and calcium hydroxide do not meet the industrial grade standard, which may be because the carboxyl structure on the polymerized ionic liquid generated by acrylic acid polymerization can react with sodium methoxide and calcium methoxide, producing by-products such as formate, resulting in separation difficulties, more impurities, and reduced content. Therefore, the structure of the polymerized ionic liquid cannot contain functional groups that can react with calcium methoxide and sodium methoxide.

[0065] Comparative Example 1:

[0066] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0067] The polymeric ionic liquid in Example 4 was replaced by 1-methyl-3-butylimidazolium chloride, and the other conditions were kept consistent with Example 4. The sodium methoxide content was measured to be 22.3%; the weight of calcium hydroxide was 198.75 g, the recovery rate was 19.86%, and the calcium hydroxide content was 84.05%.

[0068] Comparative Example 2:

[0069] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0070] The polymeric ionic liquid in Example 4 was replaced by 1-ethyl-3-methylimidazole ethyl sulfate, and the other conditions were consistent with Example 4. The sodium methoxide content was measured to be 20.1%; the weight of calcium hydroxide was 198.75 g, the recovery rate was 19.86%, and the calcium hydroxide content was 81.82%.

[0071] Comparative Example 3:

[0072] A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolyzing metallic sodium, specifically comprising the following processes:

[0073] The polymeric ionic liquid in Example 4 was replaced by 1-ethyl-3-methylimidazolium hexafluorophosphate, and the other conditions were kept consistent with Example 4. The sodium methoxide content was measured to be 24.1%; the weight of calcium hydroxide was 206.89 g, the recovery rate was 20.69%, and the calcium hydroxide content was 87.02%.

[0074] The above-described embodiments provide a detailed description of the technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected.

Claims

1. A method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium, characterized in that: The efficient utilization method comprises the following steps: Putting high calcium metal sodium into a reaction kettle, adding anhydrous methanol under the protection of inert gas for mixed reaction to obtain a mixed solution of sodium methoxide and calcium methoxide; Adding polymeric ionic liquid to the mixed solution of sodium methoxide and calcium methoxide, mixing and stirring at 30° C. to 40° C., and then separating by distillation to obtain a complex of sodium methoxide and calcium methoxide; The complex of calcium methoxide is mixed with water and stirred, and calcium hydroxide is obtained by filtration and separation.

2. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 1, characterized in that: The mass ratio of the high calcium metallic sodium to the anhydrous methanol is 1:1-3.

3. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 1, characterized in that: The inert gas includes helium or nitrogen.

4. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 1, characterized in that: The preparation method of the polymeric ionic liquid comprises the following steps: 1-vinyl imidazole and alkyl halide are mixed in an ether solution to form a reaction system, and the reaction system is subjected to a temperature-raising reaction to obtain an imidazole-based ionic liquid; The imidazole-based ionic liquid and the unsaturated olefinic aldehyde are mixed in equal amounts and then reacted by a free radical initiator to obtain the polymerized ionic liquid.

5. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 4, characterized in that: The molar ratio of 1-vinylimidazole to alkyl halide is 1:

1.

6. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 4, characterized in that: The alkyl halide includes 1-chloropropane or 2-chloropropane.

7. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 4, characterized in that: The conditions of the temperature-raising reaction include a reaction temperature of 70° C. to 80° C. and a reaction time of 16 h to 20 h.

8. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 4, characterized in that: The unsaturated olefinic aldehyde includes acrolein.

9. The method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium according to claim 4, characterized in that: The free radical initiator includes azobisisobutyronitrile, benzoyl peroxide or azobisisoheptanenitrile.

10. According to the method for efficiently utilizing high-calcium metallic sodium produced in the process of electrolytically preparing metallic sodium as claimed in claim 4, the conditions of the catalytic reaction include a reaction temperature of 60°C to 80°C and a reaction time of 6h to 8h.

Citation Information

Cited By

  • Method for preparing sodium alkoxide by using sodium slag

    CN118930406A