Glass tube for lead-free ultraviolet-transmitting lamp
Through the design of glass tubes for lead-free UV lamps, specific chemical raw material composition and process processing are used to solve the problem of reduced UV penetration effect and environmental pollution caused by lead content, and achieve efficient sterilization and environmentally friendly UV transmission.
Patent Information
- Application Number
- CN202410758327.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The glass tube of the existing UV lamp contains a large amount of heavy metal lead, which causes the UV penetration effect to deteriorate, reduces the sterilization effect, and causes pollution to the environment and human body after being scrapped.
It adopts lead-free transparent UV lamp glass tube. The chemical raw materials include Li2O, B2O3, Na2O, MgO, Al2O3, SiO2, K2O, CaO, BaO, Co2O3, NiO, Fe2O3, ZrO2, SrO, MnO, SO3 and ZnO. Smelting and annealing in an electric furnace creates a high-transmittance, heat-resistant glass tube.
It achieves ultraviolet transmission with high transmittance, enhances the sterilization effect, reduces production energy consumption, reduces environmental pollution, extends the service life of the lamp tube, and improves the physical properties and environmental protection of the glass tube.
Smart Images

Figure CN118754432A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultraviolet-transmitting electric light sources, and more specifically to a lead-free glass tube for an ultraviolet-transmitting lamp. Background Art
[0002] Ultraviolet lamps (UV transmission lamps) are devices that use ultraviolet (UV) radiation for disinfection and sterilization. They are usually composed of ultraviolet lamps and electronic control systems; the inside of the ultraviolet lamp is filled with inert gas, and when excited by electric current, it will produce ultraviolet radiation. Ultraviolet light is part of invisible light, located outside the violet visible light in the electromagnetic spectrum, with a wavelength between 10 and 400 nanometers. According to different properties, it is usually divided into several bands such as vacuum ultraviolet, short-wave ultraviolet, medium-wave ultraviolet, and long-wave ultraviolet.
[0003] There are two main types of ultraviolet lamps: UV-C and UV-B; UV-C has a wavelength range of 100 to 280 nanometers and is one of the most effective sterilization wavelengths; UV-C can destroy the nucleic acids of bacteria, viruses and other microorganisms, thereby making them lose their ability to grow and reproduce; UV-B has a wavelength range of 280 to 315 nanometers and also has a certain sterilization effect, but its sterilization effect is weaker than that of UV-C.
[0004] Ultraviolet lamps are widely used in current life and production. Their excellent environmental protection and sterilization effects are loved by people, so the production of ultraviolet lamps is also increasing year by year; but the glass tubes used in ultraviolet lamps contain a large amount of heavy metal lead, which leads to poor penetration of ultraviolet light and reduces its sterilization effect. At the same time, after the glass tube is scrapped, the large amount of heavy metals in the lamp tube cause great pollution to the external environment and cause great harm to the human body.
[0005] In view of this, the present invention provides a lead-free glass tube for ultraviolet-transmitting lamp to solve the above problems. Summary of the invention
[0006] In order to overcome the above defects of the prior art, the present invention provides a lead-free glass tube for ultraviolet-transmitting lamp to solve the problems existing in the above background technology.
[0007] The present invention provides the following technical scheme: a lead-free glass tube for ultraviolet light, wherein the chemical raw material components are as follows: Li2O is 0.3%-0.7%, B2O3 is 0.3%-1.3%, Na2O is 8%-11%, MgO is 0.8%-1.5%, Al2O3 is 2.5%-4.0%, SiO2 is 63-68, K2O is 2.0%-5.0%, CaO is 0.8%-2.5%, BaO is 6.0%-10.0%, Co2O3 is 0.4%-0.8%, NiO is 1.3%-1.9%, Fe2O3 is 0.1%-0.2%, ZrO2 is less than 0.6%, SrO is less than 0.7%, MnO is less than 0.06%, SO3 is less than 0.1%, ZnO is less than 0.06%, and P2O5 is less than 0.5%;
[0008] In a preferred embodiment, the mass percentages of the chemical raw material components are: Li2O is 0.5-5%, B2O3 is 0.1-5%, Na2O is 6-14%, MgO is 0.01-5%, Al2O3 is 1-6%, SiO2 is 60-66%, K2O is 1-6%, CaO is 0.01-5%, BaO is 0.01-8%, Co2O3 is 0.01-0.5%, NiO is 1.3%-1.9%, Fe2O3 is 0.1%-0.2%, ZrO2 is less than 0.6%, SrO is less than 0.7%, MnO is 0.01-0.1%, SO3 is less than 0.1%, ZnO is less than 0.06%, and P2O5 is 0.01-1%.
[0009] In a preferred embodiment, the lead-free glass tube for ultraviolet lamp contains 0.6% Li2O, 1.2% B2O3, 11% Na2O, 1.2% MgO, 3.6% Al2O3, 66% SiO2, 3.73% K2O, 0.9% CaO, 8% BaO, 0.48% Co2O3, 1.6% NiO, 0.12% Fe2O3, 0.4% ZrO2, 0.6% SrO, 0.05% MnO, 0.08% SO3, 0.05% ZnO and 0.39% P2O5.
[0010] In a preferred embodiment, the purity of the chemical raw material components used in the lead-free ultraviolet-transmitting lamp glass tube is 99.9% or above.
[0011] In a preferred embodiment, the chemical raw material components of the lead-free ultraviolet lamp glass tube are weighed according to mass percentage, put into a blender and stirred for about 5 to 7 minutes, the crushed and cleaned broken glass is put into the blender and stirred together with the powder for about three minutes, and then the mixture is taken out.
[0012] In a preferred embodiment, the mixing ratio of the chemical raw materials and the cullet of the lead-free ultraviolet lamp glass tube is 1:9.
[0013] In a preferred embodiment, the mixture of the lead-free glass tube for ultraviolet lamp is smelted in an all-electric furnace with a smelting temperature between 1400 and 1480°C, a melting time of 6 to 10 hours, and a retention time in the smelting zone of 60 to 90 minutes, to ensure that all raw materials can be completely melted and mixed evenly to form a homogeneous glass liquid.
[0014] In a preferred embodiment, after the lead-free glass tube for ultraviolet-transmitting lamp is melted, the glass liquid is made into a lead-free ultraviolet-transmitting glass tube by a vertical or horizontal tube drawing method, and then annealing treatment is performed.
[0015] In a preferred embodiment, the annealing temperature of the lead-free UV-transmitting lamp glass tube is between 500 and 600° C., and the heat preservation time is 60 to 120 minutes.
[0016] In a preferred embodiment, the lead-free glass tube for ultraviolet lamp does not contain lead, has a maximum ultraviolet transmittance of >85%, an expansion coefficient of 85-105*10^-6 / °C, a softening point of (620±20°C), and a water resistance grade of HGB1.
[0017] In the present invention, Li2O is used to improve the durability and chemical stability of glass, and enhance the thermal shock resistance of glass, so that it is not easy to break when the temperature changes;
[0018] B2O3 helps it form a grid structure of glass, improves the stability and durability of glass, and reduces the melting temperature of glass, thereby saving energy and reducing energy consumption in the production process, and increasing the service life and stability of UV lamps;
[0019] Na2O is a co-solvent that lowers the melting temperature of glass raw materials, reduces energy consumption in the production process, makes the glass production process more economical and efficient, changes the structure of the glass network, and thus affects a series of physical properties of the glass, such as thermal expansion coefficient, softening point, etc., helps to improve the stability of the glass, especially when ultraviolet rays pass through, it can keep the performance of the glass tube intact;
[0020] MgO is a network modifier that adjusts the glass network structure, thereby affecting the physical properties of the glass, such as thermal expansion coefficient, softening point, etc. This helps to improve the heat resistance and mechanical strength of the glass tube, and improve the stability of the glass, especially when ultraviolet rays pass through, to keep the performance of the glass tube undamaged, which is very important for ensuring the service life and stability of the UV lamp;
[0021] Al2O3 can form aluminum-oxygen tetrahedrons in the glass structure, which can be connected with silicon-oxygen tetrahedrons, thereby strengthening the network structure of the glass, improving its chemical resistance and wear resistance, and improving the hardness and thermal shock resistance of the glass, making the glass tube more durable;
[0022] SiO2 forms silicon-oxygen tetrahedrons in glass. These tetrahedrons are connected into a network through shared oxygen atoms at the vertices, forming the skeleton of the glass, which makes the glass have high chemical and thermal stability. SiO2 has good light transmittance, especially in the ultraviolet region, it can effectively transmit ultraviolet rays without too much absorption or loss. SiO2 has good mechanical strength and chemical resistance, and does not contain harmful substances such as lead. SiO2 has a high melting point, which helps to improve the heat resistance of glass, so that it can remain stable in high temperature environments and is not easily deformed or damaged.
[0023] K2O is a flux that can effectively reduce the melting temperature of glass raw materials, which helps reduce energy consumption in the production process, making the glass production process more economical and efficient. It can effectively improve other properties of glass, such as enhancing the light transmittance and chemical corrosion resistance of glass, and it is very important to increase the service life and stability of UV lamps.
[0024] CaO can improve the chemical stability of glass, making it more resistant to chemical corrosion. CaO can adjust the thermal expansion coefficient of glass, making it more stable when the temperature changes, reducing the stress and cracking risk caused by temperature changes. When CaO is used outdoors, it can improve its weather resistance and prevent damage to the glass caused by natural environments such as sun and rain. Since it does not contain heavy metals such as lead, the use of CaO helps protect the environment.
[0025] BaO makes the glass reach a higher UV transmittance, especially at a wavelength of 365nm, the transmittance can reach 85% or higher, ensuring that the glass can cut off the transmission of visible light, that is, the average transmittance in the wavelength range of 425nm to 675nm is less than 0.1%, which helps to concentrate the irradiation of ultraviolet rays and avoid the interference of visible light. BaO can replace traditional lead-containing glass, reduce environmental pollution, improve the chemical stability of glass, extend the service life, and improve the optical properties of glass;
[0026] Co2O3 is usually used as a colorant in glass tubes. This coloring effect is sometimes intentional and is used to filter specific wavelengths of visible light to optimize the transmission efficiency of ultraviolet rays. It can also improve the stability of the glass, keep the performance of the glass intact under high temperature and ultraviolet radiation, and increase the service life of the ultraviolet lamp;
[0027] NiO is used to enhance the chemical stability of glass and optimize the ultraviolet transmittance of glass, making it have a higher transmittance within a specific wavelength range, thereby improving the disinfection and lighting effects of lamps and extending the service life of glass tubes;
[0028] Fe2O3 requires extremely precise control to ensure the UV transmittance of the glass tube and avoid unnecessary coloration, thereby improving the disinfection effect and service life of the lamp;
[0029] ZrO2 can improve the wear resistance and impact resistance of glass, and can replace materials containing lead glass. It has good chemical stability and increases the service life of the product.
[0030] The presence of SrO helps to promote the formation of a specific glass network structure, thereby strengthening the network structure of the glass and increasing its characteristic temperature, which helps to ensure the efficiency and stability of the lamp in ultraviolet transmission, reduce harm to the human body and the environment, and at the same time helps to improve the optical properties of the glass tube, meeting environmental protection and safety requirements;
[0031] MnO acts as a colorant, affecting the color of glass and is used to improve the color and optical properties of glass;
[0032] SO3 removes bubbles and impurities in the glass melt during the glass clarification process, thereby improving the transparency and quality of the glass;
[0033] ZnO can enhance the resistance of glass to chemicals, making it more durable, and help improve the weather resistance of glass, that is, the ability to adapt to the external environment (such as ultraviolet rays, humidity, temperature changes, etc.). It can also act as a flux to help lower the melting temperature, making the glass easier to melt and form, and improving the chemical stability and weather resistance of the glass.
[0034] P2O5 can increase the dispersion coefficient of glass, making the glass more transparent to ultraviolet rays, and making the glass more transparent to ultraviolet rays and having a higher transmittance.
[0035] The lead content of the present invention is tested in accordance with the standards and specifications of T / SCS-000001-2018 "Lead-free UV-transmitting glass lamp tube", and the lead content is tested in accordance with GB / T 21170-2007 "Determination of lead and cadmium dissolution from glass containers";
[0036] The iron content of the present invention is tested according to the standard and specification T / SCS-000001-2018 "Lead-free UV-transmitting glass lamp tube", and the iron content is tested according to GB / T 36985-2018 atomic absorption spectrometry.
[0037] The average transmittance of the present invention is tested according to the ISO9050 glass transmission spectrum measurement method in the visible light range;
[0038] The maximum ultraviolet transmittance of the present invention is tested according to the ISO 2003 glass transmission spectrometry method in the visible light and near infrared region;
[0039] The expansion coefficient of the present invention is tested according to the standard of GB / T 4545-1991 "Determination of the average linear thermal expansion coefficient of glass";
[0040] The softening point of the present invention is tested according to the glass softening point test method of GBT 28195-2011;
[0041] The water resistance grade of the present invention is tested according to the water resistance test method and classification of glass particles at 98° C. in GB / T 6582-2021.
[0042] Technical effects and advantages of the present invention:
[0043] The lead-free glass tube for ultraviolet lamp of the present invention does not contain lead, is harmless to human body and environment, has good environmental protection performance, has high transmittance in ultraviolet band, can effectively transmit ultraviolet light, thereby achieving better sterilization effect, adopts all-electric melting furnace for production and processing, makes lamp tube production and manufacturing simple, realizes green and environmental protection of the whole manufacturing process, is more energy-saving, has good workshop environment, does not produce harmful substances, protects the health of employees, the product has high light transmittance, has good sterilization effect, and has strong blue light characteristic, reasonable raw material ratio makes glass tube have good physical properties, has certain hardness and wear resistance, prolongs the service life of lamp tube, has high transmittance, good water resistance, lead-free component makes glass tube more environmentally friendly, reduces potential harm to environment and human body. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is the management index of the present invention. DETAILED DESCRIPTION
[0045] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the present invention. In addition, the forms of the various structures recorded in the following embodiments are only examples. The lead-free glass tube for ultraviolet lamp involved in the present invention is not limited to the various structures recorded in the following embodiments. All other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.
[0046] Example 1
[0047] The invention provides a lead-free glass tube for an ultraviolet-transmitting lamp. The chemical raw material components of the glass tube are as follows: Li2O is 0.6%, B2O3 is 1.2%, Na2O is 11%, MgO is 1.2%, Al2O3 is 3.6%, SiO2 is 66%, K2O is 3.73%, CaO is 0.9%, BaO is 9%, Co2O3 is 0.48%, NiO is 1.6%, Fe2O3 is 0.02%, ZrO2 is 0.4%, SrO is 0.6%, MnO is 0.05%, SO3 is 0.08%, ZnO is 0.05%, and P2O5 is 0.39%.
[0048] The purity of the chemical raw materials used in the glass tubes of lead-free UV lamps is 99.9%;
[0049] The chemical raw material components of the glass tube for lead-free ultraviolet lamp are weighed according to the mass percentage, put into a blender and stirred for about 5 minutes, and the crushed and cleaned broken glass is put into the blender and stirred together with the powder for 3 minutes, and then the mixture is taken out; the mixing ratio of the chemical raw materials and broken glass for lead-free ultraviolet lamp glass tube is 1:9;
[0050] The mixture of lead-free glass tubes for UV lamps is smelted in a fully electric furnace with a smelting temperature of 1440°C, a melting time of 8 hours, and a retention time in the smelting zone of 75 minutes to ensure that all raw materials are completely melted and mixed evenly to form a homogeneous glass liquid; the annealing temperature of lead-free glass tubes for UV lamps is 550°C, and the insulation time is 90 minutes.
[0051] Example 2
[0052] The invention provides a lead-free glass tube for an ultraviolet-transmitting lamp. The chemical raw material components of the glass tube are as follows: Li2O is 4%, B2O3 is 4%, Na2O is 14%, MgO is 3%, Al2O3 is 3%, SiO2 is 60%, K2O is 4.5%, CaO is 1.2%, BaO is 4%, Co2O3 is 0.3%, NiO is 1.3%, Fe2O3 is 0.02%, ZrO2 is 0.08%, SrO is 0.25%, MnO is 0.05%, SO3 is 0.08%, ZnO is 0.05%, and P2O5 is 0.17%.
[0053] The purity of the chemical raw materials used in the glass tubes of lead-free UV lamps is 99.9%;
[0054] The chemical raw material components of the glass tube for lead-free ultraviolet lamp are weighed according to the mass percentage, put into a blender and stirred for about 5 minutes, and the crushed and cleaned broken glass is put into the blender and stirred together with the powder for 3 minutes, and then the mixture is taken out; the mixing ratio of the chemical raw materials and broken glass for lead-free ultraviolet lamp glass tube is 1:9;
[0055] The mixture of lead-free glass tubes for UV lamps is smelted in a fully electric furnace with a smelting temperature of 1480°C, a melting time of 7 hours, and a retention time in the smelting zone of 70 minutes to ensure that all raw materials are completely melted and mixed evenly to form a homogeneous glass liquid; the annealing temperature of lead-free glass tubes for UV lamps is 550°C, and the insulation time is 70 minutes.
[0056] Example 3
[0057] The invention provides a lead-free glass tube for ultraviolet-transmitting lamps, wherein the chemical raw material components are as follows: Li2O is 0.7%, B2O3 is 1.3%, Na2O is 10.5%, MgO is 1.5%, Al2O3 is 4%, SiO2 is 67%, K2O is 4%, CaO is 2%, BaO is 6%, Co2O3 is 0.4%, NiO is 1.6%, Fe2O3 is 0.15%, ZrO2 is 0.1%, SrO is 0.35%, MnO is 0.05%, SO3 is 0.08%, ZnO is 0.05%, and P2O5 is 0.22%;
[0058] The purity of the chemical raw materials used in the glass tubes of lead-free UV lamps is 99.9%;
[0059] The chemical raw material components of the glass tube for lead-free ultraviolet lamp are weighed according to the mass percentage, put into a blender and stirred for about 5 minutes, and the crushed and cleaned broken glass is put into the blender and stirred together with the powder for 3 minutes, and then the mixture is taken out; the mixing ratio of the chemical raw materials and broken glass for lead-free ultraviolet lamp glass tube is 1:9;
[0060] The mixture of lead-free glass tubes for UV lamps is smelted in a fully electric furnace with a smelting temperature of 1480°C, a melting time of 10 hours, and a retention time in the smelting zone of 80 minutes to ensure that all raw materials are completely melted and mixed evenly to form a homogeneous glass liquid; the annealing temperature of the lead-free glass tubes for UV lamps is between 600°C and the insulation time is 60 minutes.
[0061] Example 4
[0062] The invention provides a lead-free glass tube for an ultraviolet-transmitting lamp. The chemical raw material components of the glass tube are as follows: Li2O is 0.7%, B2O3 is 1.3%, Na2O is 11%, MgO is 1.5%, Al2O3 is 4%, SiO2 is 67%, K2O is 3.93%, CaO is 1%, BaO is 6%, Co2O3 is 0.4%, NiO is 1.5%, Fe2O3 is 0.1%, ZrO2 is 0.4%, SrO is 0.6%, MnO is 0.05%, SO3 is 0.08%, ZnO is 0.05%, and P2O5 is 0.39%.
[0063] The purity of the chemical raw materials used in the glass tubes of lead-free UV lamps is 99.9%;
[0064] The chemical raw material components of the glass tube for lead-free ultraviolet lamp are weighed according to the mass percentage, put into a blender and stirred for about 5 minutes, and the crushed and cleaned broken glass is put into the blender and stirred together with the powder for 3 minutes, and then the mixture is taken out; the mixing ratio of the chemical raw materials and broken glass for lead-free ultraviolet lamp glass tube is 1:9;
[0065] The mixture of lead-free glass tubes for UV lamps is smelted in a fully electric furnace with a smelting temperature of 1480°C, a melting time of 7 hours, and a retention time in the smelting zone of 60 minutes to ensure that all raw materials are completely melted and mixed evenly to form a homogeneous glass liquid; the annealing temperature of lead-free glass tubes for UV lamps is between 500°C and the insulation time is 80 minutes.
[0066] The Li2O of the present invention is used to improve the durability and chemical stability of glass, enhance the thermal shock resistance of glass, and make it less likely to break when the temperature changes;
[0067] B2O3 helps it form a grid structure of glass, improves the stability and durability of glass, and reduces the melting temperature of glass, thereby saving energy and reducing energy consumption in the production process, and increasing the service life and stability of UV lamps;
[0068] Na2O is a co-solvent that lowers the melting temperature of glass raw materials, reduces energy consumption in the production process, makes the glass production process more economical and efficient, changes the structure of the glass network, and thus affects a series of physical properties of the glass, such as thermal expansion coefficient, softening point, etc., helps to improve the stability of the glass, especially when ultraviolet rays pass through, it can keep the performance of the glass tube intact;
[0069] MgO is a network modifier that adjusts the glass network structure, thereby affecting the physical properties of the glass, such as thermal expansion coefficient, softening point, etc. This helps to improve the heat resistance and mechanical strength of the glass tube, and improve the stability of the glass, especially when ultraviolet rays pass through, to keep the performance of the glass tube undamaged, which is very important for ensuring the service life and stability of the UV lamp;
[0070] Al2O3 can form aluminum-oxygen tetrahedrons in the glass structure, which can be connected with silicon-oxygen tetrahedrons, thereby strengthening the network structure of the glass, improving its chemical resistance and wear resistance, and improving the hardness and thermal shock resistance of the glass, making the glass tube more durable;
[0071] SiO2 forms silicon-oxygen tetrahedrons in glass. These tetrahedrons are connected into a network through shared oxygen atoms at the vertices, forming the skeleton of the glass, which makes the glass have high chemical and thermal stability. SiO2 has good light transmittance, especially in the ultraviolet region, it can effectively transmit ultraviolet rays without too much absorption or loss. SiO2 has good mechanical strength and chemical resistance, and does not contain harmful substances such as lead. SiO2 has a high melting point, which helps to improve the heat resistance of glass, so that it can remain stable in high temperature environments and is not easily deformed or damaged.
[0072] K2O is a flux that can effectively reduce the melting temperature of glass raw materials, which helps reduce energy consumption in the production process, making the glass production process more economical and efficient. It can effectively improve other properties of glass, such as enhancing the light transmittance and chemical corrosion resistance of glass, and it is very important to increase the service life and stability of UV lamps.
[0073] CaO can improve the chemical stability of glass, making it more resistant to chemical corrosion. CaO can adjust the thermal expansion coefficient of glass, making it more stable when the temperature changes, reducing the stress and cracking risk caused by temperature changes. When CaO is used outdoors, it can improve its weather resistance and prevent damage to the glass caused by natural environments such as sun and rain. Since it does not contain heavy metals such as lead, the use of CaO helps protect the environment.
[0074] BaO makes the glass reach a higher UV transmittance, especially at a wavelength of 365nm, the transmittance can reach 85% or higher, ensuring that the glass can cut off the transmission of visible light, that is, the average transmittance in the wavelength range of 425nm to 675nm is less than 0.1%, which helps to concentrate the irradiation of ultraviolet rays and avoid the interference of visible light. BaO can replace traditional lead-containing glass, reduce environmental pollution, improve the chemical stability of glass, extend the service life, and improve the optical properties of glass;
[0075] Co2O3 is usually used as a colorant in glass tubes. This coloring effect is sometimes intentional and is used to filter specific wavelengths of visible light to optimize the transmission efficiency of ultraviolet rays. It can also improve the stability of the glass, keep the performance of the glass intact under high temperature and ultraviolet radiation, and increase the service life of the ultraviolet lamp;
[0076] NiO is used to enhance the chemical stability of glass and optimize the ultraviolet transmittance of glass, making it have a higher transmittance within a specific wavelength range, thereby improving the disinfection and lighting effects of lamps and extending the service life of glass tubes;
[0077] Fe2O3 requires extremely precise control to ensure the UV transmittance of the glass tube and avoid unnecessary coloration, thereby improving the disinfection effect and service life of the lamp;
[0078] ZrO2 can improve the wear resistance and impact resistance of glass, and can replace materials containing lead glass. It has good chemical stability and increases the service life of the product.
[0079] The presence of SrO helps to promote the formation of a specific glass network structure, thereby strengthening the network structure of the glass and increasing its characteristic temperature, which helps to ensure the efficiency and stability of the lamp in ultraviolet transmission, reduce harm to the human body and the environment, and at the same time helps to improve the optical properties of the glass tube, meeting environmental protection and safety requirements;
[0080] MnO acts as a colorant, affecting the color of glass and is used to improve the color and optical properties of glass;
[0081] SO3 removes bubbles and impurities in the glass melt during the glass clarification process, thereby improving the transparency and quality of the glass;
[0082] ZnO can enhance the resistance of glass to chemicals, making it more durable, and help improve the weather resistance of glass, that is, the ability to adapt to the external environment (such as ultraviolet rays, humidity, temperature changes, etc.). It can also act as a flux to help lower the melting temperature, making the glass easier to melt and form, and improving the chemical stability and weather resistance of the glass.
[0083] P2O5 can increase the dispersion coefficient of glass, making the glass more transparent to ultraviolet rays, and making the glass more transparent to ultraviolet rays and having a higher transmittance.
[0084] The lead content of the present invention is tested in accordance with the standards and specifications of T / SCS-000001-2018 "Lead-free UV-transmitting glass lamp tube", and the lead content is tested in accordance with GB / T 21170-2007 "Determination of lead and cadmium dissolution from glass containers";
[0085] The iron content of the present invention is tested according to the standard and specification T / SCS-000001-2018 "Lead-free UV-transmitting glass lamp tube", and the iron content is tested according to GB / T 36985-2018 atomic absorption spectrometry.
[0086] The average transmittance of the present invention is tested according to the ISO9050 glass transmission spectrum measurement method in the visible light range;
[0087] The maximum ultraviolet transmittance of the present invention is tested according to the ISO 2003 glass transmission spectrometry method in the visible light and near infrared region;
[0088] The expansion coefficient of the present invention is tested according to the standard of GB / T 4545-1991 "Determination of the average linear thermal expansion coefficient of glass";
[0089] The softening point of the present invention is tested according to the glass softening point test method of GBT 28195-2011;
[0090] The water resistance grade of the present invention is tested according to the water resistance test method and classification of glass particles at 98° C. in GB / T 6582-2021.
[0091] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A lead-free glass tube for ultraviolet light, comprising cullet and chemical raw materials, characterized in that: The mass percentages of its chemical raw material components are: Li2O is 0.5-5%, B2O3 is 0.1-5%, Na2O is 6-14%, MgO is 0.01-5%, Al2O3 is 1-6%, SiO2 is 60-70%, K2O is 1-6%, CaO is 0.01-5%, BaO is 0.01-9%, Co2O3 is 0.01-0.5%, NiO is 1.3%-1.9%, Fe2O3 is 0.1%-0.2%, ZrO2 is 0.01%-0.6%, SrO is 0.01%-0.7%, MnO is 0.01%-0.1%, SO3 is 0.01%-0.1%, ZnO is 0.01%-0.06%, and P2O5 is 0.01%-1%.
2. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 1, characterized in that: The mass percentages of its chemical raw material components are: Li2O is 0.5%-0.7%, B2O3 is 0.3%-1.3%, Na2O is 8%-11%, MgO is 0.8%-1.5%, Al2O3 is 2.5%-4.0%, SiO2 is 63-68, K2O is 2.0%-5.0%, CaO is 0.8%-2.5%, BaO is 6.0%-10.0%, Co2O3 is 0.4% - 0.8%, NiO is 1.3% - 1.9%, Fe2O3 is 0.1% - 0.2%, ZrO2 is 0.01% - 0.6%, SrO is 0.01% - 0.7%, MnO is 0.01% - 0.06%, SO3 is 0.01% - 0.1%, ZnO is 0.01% - 0.06%, and P2O5 is 0.01% - 0.5%.
3. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 1, characterized in that: The lead-free glass tube for ultraviolet lamp contains 0.6% Li2O, 1.2% B2O3, 11% Na2O, 1.2% MgO, 3.6% Al2O3, 66% SiO2, 3.73% K2O, 0.9% CaO, 9% BaO, 0.48% Co2O3, 1.6% NiO, 0.02% Fe2O3, 0.4% ZrO2, 0.6% SrO, 0.05% MnO, 0.08% SO3, 0.05% ZnO and 0.39% P2O5.
4. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 1, characterized in that: The purity of the chemical raw material components used in the lead-free ultraviolet-transmitting lamp glass tube is 99.9% or above.
5. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 1, characterized in that: The chemical raw material components of the lead-free ultraviolet lamp glass tube are weighed according to mass percentage, put into a mixer and stirred for about 5 to 7 minutes, and the crushed and cleaned broken glass is put into the mixer and stirred together with the powder for 2 to 3 minutes, and then the mixture is taken out.
6. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 1, characterized in that: The mixing ratio of the chemical raw materials and the broken glass in the lead-free ultraviolet-transmitting lamp glass tube is 1:
9.
7. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 5, characterized in that: The mixture of the lead-free glass tube for ultraviolet lamp is melted in a fully electric furnace at a melting temperature of 1400-1480°C, a melting time of 6-10 hours, and a retention time in the melting zone of 60-90 minutes, to ensure that all raw materials can be completely melted and mixed evenly to form a homogeneous glass liquid.
8. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 7, characterized in that: After the lead-free ultraviolet-transmitting glass tube for the ultraviolet-transmitting lamp is melted, the glass liquid is made into the lead-free ultraviolet-transmitting glass tube by a vertical or horizontal tube drawing method, and then an annealing treatment is performed.
9. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 8, characterized in that: The annealing temperature of the lead-free ultraviolet-transmitting lamp glass tube is between 500 and 600° C., and the heat preservation time is 60 to 120 minutes.
10. The lead-free glass tube for ultraviolet-transmitting lamp according to claim 1, characterized in that: The lead-free glass tube for ultraviolet lamp does not contain lead, has a maximum ultraviolet transmittance of >85%, an expansion coefficient of 85-105*10^-6 / °C, a softening point of (620±20°C), and a water resistance grade of HGB1.