Taphole mud with added boric acid and boron carbide and preparation method thereof

By using soybean oil derivatives and styrene modified soybean oil as liquid adhesives, combining boric acid and boron carbide, the problem of insufficient adhesion and high-temperature performance of the cannon mud is solved, and the fire resistance and stability of the cannon mud is significantly improved , ensuring its safety and effectiveness in high temperatures.

CN118754689BActive Publication Date: 2024-11-19JINGYEYUAN NEW MATERIALS HEBEI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411248711.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-19
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

During the use of existing gun mud, there are problems such as high pollution, short shelf life, poor adhesion and insufficient fire resistance. Especially when tar and resin are used as liquid bonding agents, the interface effect is not strong, and the carbon residual rate is low after high temperature, which affects safety. sex.

Method used

Soybean oil derivatives (LDH modified soybean oil, styrene modified soybean oil) are used as liquid binders to assist in high-temperature modified asphalt to form binders, and boron carbide is introduced to pass chelating intercalation and metals. Oxide formation improves bonding strength and high temperature performance, combines cyanite and molybdenum metal elements to promote the formation of three-dimensional whisker networks, and improves corrosion resistance and mechanical strength.

Benefits of technology

It significantly improves the plasticity, bonding strength, lubricity and high-temperature properties of the gun mud, enhances the flexural strength, corrosion resistance and oxidation resistance, improves the sintering performance and breathability, and ensures the stability and safety of the gun mud.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of refractory materials, specifically to a cannon clay added with boric acid and boron carbide and a preparation method thereof. The method comprises the following steps: Step I: weighing powder, high-temperature modified asphalt, liquid binder, boron carbide, and boric acid as raw materials for standby use; Step II: modifying boron carbide with a silane coupling agent; Step III: adding high-temperature modified asphalt to 130-140°C; adding a liquid binder, shearing at 3000-4000rpm for 10-15 minutes, cooling to 90-100°C to obtain a binder; dry-mixing powder, boric acid, and modified boron carbide for 10-15 minutes; adding a binder, mixing and grinding to obtain cannon clay. In the scheme, soybean oil-derived materials are used as liquid binders to coordinate with asphalt to effectively improve the plasticity and adhesion of the cannon clay; at the same time, boric acid and boron carbide are introduced to effectively enhance the high-temperature flexural strength, erosion resistance and other high-temperature properties of the cannon clay.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory materials, in particular to taphole clay added with boric acid and boron carbide and a preparation method thereof. Background Art

[0002] In the metallurgical industry, taphole clay is a plugging material mainly used for the taphole of a blast furnace, and its function is to ensure the normal production and safe operation of the blast furnace. Among them, taphole clay generally needs to have good refractory, slag resistance, oxidation resistance, air permeability and other high-temperature properties, so that it can quickly solidify to form a plugging layer when tapping iron, and can be easily opened when needed.

[0003] In the prior art, conventional taphole clay basically uses tar or resin as a liquid binder, but tar is highly polluting during production or use, and resin has a short shelf life. New plant oils are environmentally friendly renewable resources, which have the potential to be used as liquid binders. However, the interface effect between them and taphole clay powder is not high, and the adhesion needs to be further improved; and the residual carbon rate after high-temperature carbonization is not high, resulting in high linear shrinkage after burning and low high-temperature flexural strength, which affects safety.

[0004] In summary, it is of great significance to solve the above problems and prepare a taphole clay with added boric acid and boron carbide. Summary of the invention

[0005] The object of the present invention is to provide a taphole mud with added boric acid and boron carbide and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing taphole mud with added boric acid and boron carbide comprises the following steps:

[0008] Step I: weigh powder, high temperature modified asphalt, liquid binder, boron carbide and boric acid as raw materials and set aside;

[0009] Step II: dopamine and 5-ethynylpyridine formaldehyde are sequentially added to ethanol, stirred at 50-60°C for 3-5 hours under a nitrogen atmosphere, and purified to obtain alkynylpyridine dopamine; alkynylpyridine dopamine, 3-mercaptopropyltriethoxysilane, and an initiator are sequentially added to a solvent, and reacted under ultraviolet light for 2-2.5 hours to obtain a modified coupling agent; the modified coupling agent and boron carbide are sequentially added to an ethanol aqueous solution, the pH is adjusted to 4.5±0.2, stirred at 60-70°C for 3-4 hours, washed, and dried to obtain modified boron carbide;

[0010] Step III: Add high-temperature modified asphalt to 130~140℃; add liquid binder, shear at 3000~4000rpm for 10~15 minutes, cool to 90~100℃ to obtain a binder; dry mix the powder, boric acid, and modified boron carbide for 10~15 minutes; add the binder, mix and grind at 50~60℃ for 40~60 minutes to obtain cannon mud.

[0011] More optimally, the raw materials of the cannon mud include the following components: in parts by weight, 15-25 parts of 80 aggregate, 17-37 parts of ferrosilicon nitride, 12-27 parts of silicon carbide, 5-15 parts of kyanite, 5-12 parts of Guangxi white mud, 5-13 parts of high-temperature alumina powder, 2-15 parts of first-grade coke, 1-10 parts of silica ash, 2-12 parts of high-temperature modified asphalt, 5-20 parts of liquid binder, 0.1-0.6 parts of boron carbide, and 0.1-2 parts of boric acid.

[0012] More optimally, the ferrosilicon nitride comprises the following materials by weight: 15-25 parts of 200 mesh ferrosilicon nitride and 2-12 parts of 0-1 mm ferrosilicon nitride; the silicon carbide comprises the following materials by weight: 10-25 parts of 325F silicon carbide and 2-15 parts of 0-1 mm silicon carbide;

[0013] The 80 aggregate includes a first aggregate with a particle size of 1mm<≤3mm and a second aggregate with a particle size of 0mm<≤1mm, and the mass ratio of the two is 1:1~3; the primary coke includes a first coke with a particle size of 1mm<≤3mm and a second coke with a particle size of 0mm<≤1mm, and the mass ratio of the two is 1.5~4:1; the particle size of the boron carbide is 2~3μm.

[0014] More optimally, in the alkynylpyridine dopamine, the mass ratio of dopamine to 5-ethynylpyridinecarboxaldehyde is 1.5:1.3~1.5; the mass ratio of the alkynylpyridine dopamine to 3-mercaptopropyltriethoxysilane is 2.5:2.3~2.5.

[0015] More optimally, the liquid binder includes LDH-modified soybean oil and styrene-modified soybean oil in a mass ratio of 1.5-2:3-3.5.

[0016] More optimally, the preparation method of the LDH-modified soybean oil is as follows: nickel nitrate, ferric nitrate, and sodium molybdate are added to deionized water, and the pH is adjusted to 9±0.2 to obtain a metal salt solution; the metal salt solution is added dropwise to an alkynylpyridinium dopamine-deionized water solution, and stirred evenly to obtain a mixed solution; the solution is subjected to a hydrothermal reaction at 120-130° C. for 24 hours to obtain an alkynyl LDH; the alkynyl LDH, mercaptoethylamine, and an initiator are sequentially added to a solvent, and the solution is subjected to ultraviolet light reaction for 2-2.5 hours to obtain an amino-modified LDH; the epoxidized soybean oil, the amino-modified LDH, 4-(2-aminoethyl)phenylboronic acid pinacol ester, and zinc perchlorate are sequentially added to an ethanol-DMF mixed solvent, and the pH is adjusted to 8±0.2 using triethylamine; the mixture is stirred and reacted at 80-85° C. for 24 hours under a nitrogen atmosphere, and the mixture is cooled and post-treated to obtain an LDH-modified soybean oil.

[0017] More optimally, the LDH-modified soybean oil includes the following raw materials in parts by weight: 10 parts of epoxidized soybean oil, 2-2.5 parts of amino-modified LDH, 1-1.5 parts of 4-(2-aminoethyl)phenylboronic acid pinacol ester, and 0.5-0.8 parts of zinc perchlorate.

[0018] More optimally, the preparation method of the styrene-modified soybean oil is: epoxy soybean oil acrylate, styrene, maleic anhydride, alkynylpyridinium dopamine, and an initiator are sequentially added to a solvent, stirred and reacted at 80-85° C. for 3-4 hours under a nitrogen atmosphere, and the solvent is evaporated to obtain styrene-modified soybean oil.

[0019] More optimally, the styrene-modified soybean oil includes the following raw materials in parts by weight: 30 parts of epoxy soybean oil acrylate, 5-7 parts of styrene, 2-3 parts of maleic anhydride, and 2-3 parts of alkynylpyridinium dopamine.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] In the scheme, soybean oil derivatives (LDH-modified soybean oil, styrene-modified soybean oil) are used as liquid adhesives to assist high-temperature modified asphalt in forming a binder, which can effectively bond the refractory aggregates in the cannon mud together, so that the cannon mud has good plasticity and bonding strength, and can improve the necessary lubricity during the cannon mud mixing process, making it easier for the cannon mud to squeeze into the iron mouth through the cannon mud to form a stable sealing material.

[0022] In general, directly using soybean oil or epoxidized soybean oil as a liquid adhesive has two problems. First, there are compatibility issues with asphalt, resulting in weak interfacial interaction and affecting adhesion. Second, the low residual carbon rate of soybean oil after high-temperature pyrolysis will lead to poor high-temperature folding resistance of the cannon mud. Therefore, the scheme uses a combination of LDH-modified soybean oil and styrene-modified soybean oil as a liquid adhesive. Among them, LDH-modified soybean oil styrene is an LDH of three metals: nickel, iron, and molybdenum. At the same time, nitrogen-containing rings and benzene-containing alkynylpyridine dopamine are introduced, and chelating intercalation is used on the LDH. Due to the introduction of alkynylpyridine dopamine, the residual carbon rate is enhanced, and a reinforcing agent can be formed after sintering to fill in the gaps in the cannon mud and inhibit the sintering shrinkage rate. At the same time, metal ions can be pyrolyzed to form metal oxides, thereby effectively promoting carbonization and graphitization, and further improving the high-temperature folding resistance and corrosion resistance. It should be noted that the amount of LDH introduced needs to be controlled. Excessive introduction will produce too much metal oxide, which will cause internal stress at high temperature due to different thermal expansion coefficients, resulting in structural destruction after sintering and affecting the mechanical strength; and it will cause the cannon mud to partially generate low-melting-point substances, reducing the strength, refractoriness and corrosion resistance of the cannon mud.

[0023] Among them, styrene-modified soybean oil is obtained by copolymerization of epoxy soybean oil acrylate, styrene, maleic anhydride, and alkynylpyridinium dopamine, which has similar compatibility with LDH-modified soybean oil; at the same time, the styrene and maleic anhydride it contains have good compatibility with asphalt; it can be used as a compatibilizer to effectively enhance the interface between binders and improve the fluidity of the binder. On the other hand, copolymerization grafting effectively improves the carbonization performance after sintering and improves the high-temperature performance of the taphole mud.

[0024] In addition, the liquid binder will decompose and release volatile components, leaving gaps after escape, further improving the permeability of the cannon mud.

[0025] In the scheme, boric acid containing boron is further introduced as a low-temperature sintering agent, so that the binder is carbonized to form a carbon bond, combined with high-temperature resistant white mud, and the sintering performance is improved. However, excessive introduction of boric acid will introduce too much bound water, resulting in densification and reduced mechanical strength. Therefore, in the scheme, the amount of boric acid introduced is limited, and boric ester segments are introduced into LDH-modified soybean oil to partially replace the introduction of boron elements.

[0026] In the scheme, the further introduction of boron carbide can significantly improve the anti-erosion and anti-scouring properties of the taphole mud, as well as the anti-slag and anti-oxidation properties. The addition of boron carbide is intended to improve the high-temperature performance of the taphole mud, increase air permeability, inhibit carbon oxidation, improve the fluidity of the taphole mud, and increase the taphole mud's improved wear resistance, strength and stability. At the same time, in order to enhance its dispersibility in the taphole mud, a silane coupling agent with a similar chain segment to the liquid binder is used for modification to improve its dispersibility in the taphole mud.

[0027] In the scheme, kyanite and molybdenum metal elements were introduced to effectively promote the growth of kyanite whiskers in needle-shaped mullite, forming a three-dimensional whisker network, reducing sintering shrinkage, and improving mechanical strength and corrosion resistance.

[0028] In summary, the present invention provides a cannon clay with added boric acid and boron carbide; soybean oil-derived materials are used as liquid adhesives to synergize with asphalt to effectively improve and ensure that the cannon clay has high plasticity and adhesion; at the same time, boric acid is introduced as a low-temperature sintering agent, boron carbide is used as an auxiliary reinforcing agent, and kyanite is introduced into conventional powders to effectively enhance the high-temperature properties of the cannon clay, such as high-temperature flexural strength. DETAILED DESCRIPTION

[0029] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0030] It should be noted that the following parts are parts by mass; the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions and exemplarily include: the brand of epoxidized soybean oil is Youpeng; the brand of epoxidized soybean oil acrylate is Chengfeng; the CAS number of 4-(2-aminoethyl)phenylboronic acid pinacol ester is 138500-90-0; the CAS number of dopamine is 51-61-6; the CAS number of 5-acetylenepyridinecarboxaldehyde is 940911-03-5; the relevant raw materials in the following examples are all commercially available.

[0031] Preparation of alkynylpyridine dopamine: 1.5 parts of dopamine and 1.35 parts of 5-ethynylpyridine carboxaldehyde are added to 20 parts of ethanol in sequence, stirred at 60° C. for 4 hours under a nitrogen atmosphere, and purified to obtain alkynylpyridine dopamine;

[0032] Preparation of the modified coupling agent: 2.5 parts of alkynylpyridinium dopamine, 2.4 parts of 3-mercaptopropyltriethoxysilane, and 0.1 parts of AIBN initiator were sequentially added to tetrahydrofuran, and reacted under ultraviolet light for 2 hours to obtain a modified coupling agent;

[0033] Preparation of LDH-modified soybean oil: (1) Add 3.2 parts of nickel nitrate, 2.1 parts of ferric nitrate, and 0.8 parts of sodium molybdate to 100 parts of deionized water, adjust the pH to 9.1, and obtain a metal salt solution; add the metal salt solution dropwise to a 10 wt% alkynylpyridinium dopamine-deionized water solution, stir evenly, and obtain a mixed solution; subject it to a hydrothermal reaction at 130 ° C for 24 hours to obtain alkynyl LDH; (2) Add 5 parts of alkynyl LDH, 10 parts of mercaptoethylamine, and 0.1 parts of AIBN initiator; Add them into the solvent in sequence, and react under ultraviolet light for 2 hours to obtain amino-modified LDH; (3) Add 10 parts of epoxidized soybean oil, 2.4 parts of amino-modified LDH, 1.3 parts of 4-(2-aminoethyl)phenylboronic acid pinacol ester, and 0.6 parts of zinc perchlorate in sequence to 50 parts of a 50wt% ethanol-DMF mixed solvent, and use triethylamine to adjust the pH to 8.2; under a nitrogen atmosphere, stir and react at 85°C for 24 hours, cool, and post-treat to obtain LDH-modified soybean oil.

[0034] Preparation of styrene-modified soybean oil: 30 parts of epoxy soybean oil acrylate, 6 parts of styrene, 3 parts of maleic anhydride, 2 parts of alkynylpyridinium dopamine, and BPO initiator were added to toluene in sequence, stirred and reacted at 85°C for 4 hours under a nitrogen atmosphere, and the solvent was evaporated to obtain styrene-modified soybean oil.

[0035] Embodiment 1: A method for preparing taphole mud with addition of boric acid and boron carbide, comprising the following steps:

[0036] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0037] (2) Weigh 8 parts of high temperature modified asphalt, 10 parts of liquid binder (LDH modified soybean oil, styrene modified soybean oil at a ratio of 1.8:3.2), 0.5 parts of 2-3 μm boron carbide, and 1.5 parts of boric acid as raw materials;

[0038] Step II: adding the modified coupling agent and boron carbide to a 70 wt% ethanol aqueous solution in sequence, adjusting the pH to 4.5, stirring at 65° C. for 4 hours, washing, and drying to obtain modified boron carbide;

[0039] Step III: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) Dry mix the powder, boric acid, and modified boron carbide for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain cannon mud.

[0040] Embodiment 2: A method for preparing taphole mud with added boric acid and boron carbide, comprising the following steps:

[0041] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0042] (2) Weigh 6 parts of high temperature modified asphalt, 8 parts of liquid binder (LDH modified soybean oil, styrene modified soybean oil in a ratio of 2:3), 0.5 parts of 2-3 μm boron carbide, and 2 parts of boric acid as raw materials and set aside;

[0043] Step II: adding the modified coupling agent and boron carbide to a 70 wt% ethanol aqueous solution in sequence, adjusting the pH to 4.5, stirring at 65° C. for 4 hours, washing, and drying to obtain modified boron carbide;

[0044] Step III: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) Dry mix the powder, boric acid, and modified boron carbide for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain cannon mud.

[0045] Embodiment 3: A method for preparing taphole mud with added boric acid and boron carbide, comprising the following steps:

[0046] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0047] (2) Weigh 10 parts of high temperature modified asphalt, 12 parts of liquid binder (LDH modified soybean oil, styrene modified soybean oil at a ratio of 1.5:3.5), 0.3 parts of 2-3 μm boron carbide, and 1 part of boric acid as raw materials and set aside;

[0048] Step II: adding the modified coupling agent and boron carbide to a 70 wt% ethanol aqueous solution in sequence, adjusting the pH to 4.5, stirring at 65° C. for 4 hours, washing, and drying to obtain modified boron carbide;

[0049] Step III: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) Dry mix the powder, boric acid, and modified boron carbide for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain cannon mud.

[0050] Comparative Example 1: Using styrene-modified soybean oil as the liquid binder alone; the rest is the same as Example 1; the details are as follows:

[0051] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0052] (2) Weigh 8 parts of high temperature modified asphalt, 10 parts of styrene modified soybean oil, 0.5 parts of 2-3 μm boron carbide, and 1.5 parts of boric acid as raw materials and set aside;

[0053] Step II: adding the modified coupling agent and boron carbide to a 70 wt% ethanol aqueous solution in sequence, adjusting the pH to 4.5, stirring at 65° C. for 4 hours, washing, and drying to obtain modified boron carbide;

[0054] Step III: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) Dry mix the powder, boric acid, and modified boron carbide for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain cannon mud.

[0055] Comparative Example 2: The amount of LDH-modified soybean oil used was increased; the rest was the same as Example 1; the details are as follows:

[0056] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0057] (2) Weigh 8 parts of high temperature modified asphalt, 10 parts of liquid binder (LDH modified soybean oil and styrene modified soybean oil at a ratio of 3.2:1.8), 0.5 parts of 2-3 μm boron carbide, and 1.5 parts of boric acid as raw materials and set aside;

[0058] Step II: adding the modified coupling agent and boron carbide to a 70 wt% ethanol aqueous solution in sequence, adjusting the pH to 4.5, stirring at 65° C. for 4 hours, washing, and drying to obtain modified boron carbide;

[0059] Step III: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) Dry mix the powder, boric acid, and modified boron carbide for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain cannon mud.

[0060] Comparative Example 3: Anthracene oil was used as the liquid binder; the rest was the same as Example 1; the details are as follows:

[0061] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0062] (2) Weigh 8 parts of high temperature modified asphalt, 10 parts of anthracene oil, 0.5 parts of 2-3 μm boron carbide, and 1.5 parts of boric acid as raw materials and set aside;

[0063] Step II: adding the modified coupling agent and boron carbide to a 70 wt% ethanol aqueous solution in sequence, adjusting the pH to 4.5, stirring at 65° C. for 4 hours, washing, and drying to obtain modified boron carbide;

[0064] Step III: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) Dry mix the powder, boric acid, and modified boron carbide for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain cannon mud.

[0065] Comparative Example 4: Boric acid and boron carbide are not introduced, and the rest is the same as Example 1; the details are as follows:

[0066] Step I: (1) Weigh 21 parts of 80 aggregate (a first aggregate with a particle size of 1 mm < ≤ 3 mm and a second aggregate with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1:2), 20 parts of 200 mesh ferrosilicon nitride, 10 parts of 0-1 mm ferrosilicon nitride, 15 parts of 325F silicon carbide, 10 parts of 0-1 mm silicon carbide, 6 parts of kyanite, 6 parts of Guangxi white mud, 6 parts of high-temperature alumina powder, 10 parts of primary coke (a first coke with a particle size of 1 mm < ≤ 3 mm and a second coke with a particle size of 0 mm < ≤ 1 mm, the mass ratio of the two is 1.5:1), and 6 parts of silica fume to obtain powder;

[0067] (2) Weigh 8 parts of high temperature modified asphalt and 10 parts of liquid binder (LDH modified soybean oil and styrene modified soybean oil in a ratio of 1.8:3.2) as raw materials and set aside;

[0068] Step II: (1) Add high-temperature modified asphalt to 135°C; add liquid binder, shear at 3500rpm for 15 minutes, cool to 90°C to obtain a binder; (2) dry mix the powder for 15 minutes; add binder, mix and grind at 55°C for 60 minutes to obtain taphole mud.

[0069] Performance test: The prepared taphole mud was rolled into a cylindrical shape at 80KN; it was preheated at 450℃ for 5 hours, charcoal-buried heat treated at 1450℃ for 3 hours, and cooled to obtain a sample; its linear shrinkage was tested with reference to GB / T5988-2007; its apparent porosity was tested with reference to GB / T2997-2000; its high temperature flexural strength was tested with reference to GB / T3002-2004; the obtained data are shown in the following table:

[0070] sample Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Linear shrinkage% 0.59 0.60 0.63 0.73 0.56 0.69 0.56 Apparent porosity% 27.9 28.2 27.3 31.1 25.6 29.3 28.4 High temperature flexural strength MPa 14.3 14.0 13.6 11.3 12.7 11.7 12.3

[0071] Conclusion: From the data in the above table, it can be seen that: in this application, the high temperature performance of the cannon mud is effectively improved by using a specific proportion of styrene-modified soybean oil and LDH-modified soybean oil as liquid binders; from the data of Comparative Examples 1 to 4, it can be seen that: in Comparative Example 1, the single styrene-modified soybean oil, because it does not contain LDH, reduces the catalytic carbonization and graphitization, resulting in a decrease in performance; in Comparative Example 2, due to the excessive use of LDH-modified soybean oil, the internal stress of sintering in the cannon mud is increased, resulting in a decrease in performance; in Comparative Example 3, the existing anthracene oil is used as a comparison, and it can be found that the liquid binder in the present application has better high temperature performance; in Comparative Example 4, due to the lack of introduction of boric acid and boron carbide, the sintering performance is reduced, thereby reducing the high temperature performance of the cannon mud.

[0072] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing taphole mud with addition of boric acid and boron carbide, characterized in that: The following steps are involved: Step I: weigh powder, high temperature modified asphalt, liquid binder, boron carbide and boric acid as raw materials and set aside; Step II: dopamine and 5-ethynylpyridine formaldehyde are sequentially added to ethanol, stirred at 50-60°C for 3-5 hours under a nitrogen atmosphere, and purified to obtain alkynylpyridine dopamine; alkynylpyridine dopamine, 3-mercaptopropyltriethoxysilane, and an initiator are sequentially added to a solvent, and reacted under ultraviolet light for 2-2.5 hours to obtain a modified coupling agent; the modified coupling agent and boron carbide are sequentially added to an ethanol aqueous solution, the pH is adjusted to 4.5±0.2, stirred at 60-70°C for 3-4 hours, washed, and dried to obtain modified boron carbide; Step III: Add high-temperature modified asphalt to 130-140°C; add liquid binder, shear at 3000-4000rpm for 10-15 minutes, cool to 90-100°C to obtain binder; dry mix powder, boric acid and modified boron carbide for 10-15 minutes; add binder, mix and grind at 50-60°C for 40-60 minutes to obtain taphole mud; The liquid binder includes LDH-modified soybean oil and styrene-modified soybean oil in a mass ratio of 1.5-2:3-3.5; The preparation method of the LDH-modified soybean oil is as follows: nickel nitrate, ferric nitrate and sodium molybdate are added to deionized water, and the pH value is adjusted to 9±0.2 to obtain a metal salt solution; the metal salt solution is added dropwise to an alkynylpyridinium dopamine-deionized water solution, and stirred evenly to obtain a mixed solution; the mixed solution is subjected to a hydrothermal reaction at 120-130° C. for 24 hours to obtain an alkynyl LDH; the alkynyl LDH, mercaptoethylamine and an initiator are sequentially added to a solvent, and the mixture is subjected to ultraviolet light reaction for 2-2.5 hours to obtain an amino-modified LDH; the epoxidized soybean oil, the amino-modified LDH, 4-(2-aminoethyl)phenylboronic acid pinacol ester and zinc perchlorate are sequentially added to an ethanol-DMF mixed solvent, and the pH value is adjusted to 8±0.2 using triethylamine; the mixture is stirred and reacted at 80-85° C. for 24 hours under a nitrogen atmosphere, and the mixture is cooled and post-treated to obtain an LDH-modified soybean oil; The preparation method of the styrene-modified soybean oil is as follows: epoxy soybean oil acrylate, styrene, maleic anhydride, alkynylpyridinium dopamine and an initiator are sequentially added into a solvent, stirred and reacted at 80-85° C. for 3-4 hours under a nitrogen atmosphere, and the solvent is evaporated to obtain the styrene-modified soybean oil.

2. The method for preparing taphole mud with addition of boric acid and boron carbide according to claim 1, characterized in that: The raw materials of the cannon mud include the following components: in parts by weight, 15-25 parts of 80 aggregate, 17-37 parts of ferrosilicon nitride, 12-27 parts of silicon carbide, 5-15 parts of kyanite, 5-12 parts of Guangxi white mud, 5-13 parts of high-temperature alumina powder, 2-15 parts of first-grade coke, 1-10 parts of silica ash, 2-12 parts of high-temperature modified asphalt, 5-20 parts of liquid binder, 0.1-0.6 parts of boron carbide, and 0.1-2 parts of boric acid.

3. The method for preparing taphole mud with addition of boric acid and boron carbide according to claim 2, characterized in that: The ferrosilicon nitride comprises the following materials in parts by weight: 15-25 parts of 200 mesh ferrosilicon nitride and 2-12 parts of 0-1 mm ferrosilicon nitride; the silicon carbide comprises the following materials in parts by weight: 10-25 parts of 325F silicon carbide and 2-15 parts of 0-1 mm silicon carbide; The 80 aggregate includes a first aggregate with a particle size of 1mm<≤3mm and a second aggregate with a particle size of 0mm<≤1mm, and the mass ratio of the two is 1:1~3; the primary coke includes a first coke with a particle size of 1mm<≤3mm and a second coke with a particle size of 0mm<≤1mm, and the mass ratio of the two is 1.5~4:1; the particle size of the boron carbide is 2~3μm.

4. The method for preparing taphole mud with addition of boric acid and boron carbide according to claim 1, characterized in that: In the alkynylpyridine dopamine, the mass ratio of dopamine to 5-ethynylpyridine carboxaldehyde is 1.5:1.3-1.5; the mass ratio of the alkynylpyridine dopamine to 3-mercaptopropyltriethoxysilane is 2.5:2.3-2.

5.

5. The method for preparing taphole mud with addition of boric acid and boron carbide according to claim 1, characterized in that: The LDH-modified soybean oil comprises the following raw materials in parts by weight: 10 parts of epoxidized soybean oil, 2-2.5 parts of amino-modified LDH, 1-1.5 parts of 4-(2-aminoethyl)phenylboronic acid pinacol ester, and 0.5-0.8 parts of zinc perchlorate.

6. The method for preparing taphole mud with addition of boric acid and boron carbide according to claim 1, characterized in that: The styrene-modified soybean oil comprises the following raw materials in parts by weight: 30 parts of epoxy soybean oil acrylate, 5-7 parts of styrene, 2-3 parts of maleic anhydride, and 2-3 parts of alkynylpyridinium dopamine.

7. Cannon clay prepared according to the method for preparing cannon clay with added boric acid and boron carbide according to any one of claims 1 to 6.