Long-time ablation-resistant zirconium carbonitride ultra-high-temperature ceramic-based composite material as well as preparation method and application thereof

The chopped carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic material prepared by wet ball milling and discharge plasma sintering technology solves the problems of low fracture toughness and insufficient ablation resistance of existing ceramic materials in hypersonic aircraft, and achieves Efficient high temperature anti-ablation protection.

CN118754691AActive Publication Date: 2024-10-11NAT UNIV OF DEFENSE TECH

Patent Information

Application Number
CN202410839085.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing ultra-high temperature ceramic materials have problems with low fracture toughness and insufficient ablation resistance in hypersonic aircraft, which limits their wide application in harsh environments.

Method used

Metal zirconium powder, carbon powder, zirconium nitride, carbon nitride powder and chopped carbon fiber are used to prepare toughened chopped carbon fiber with high density and uniform C/N content through wet ball milling, ultrasonic stirring and discharge plasma sintering technology. Zirconium carbonitride ultra-high temperature ceramic composites.

Benefits of technology

It significantly improves the oxidation resistance, ablation resistance and mechanical properties of the material, enhances the flexural strength and fracture toughness of the ceramic, and is suitable for high temperature anti-ablation protection at 2500°C and above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754691A_ABST
    Figure CN118754691A_ABST
Patent Text Reader

Abstract

The invention discloses a long-time ablation-resistant zirconium carbonitride ultrahigh-temperature ceramic-based composite material as well as a preparation method and application thereof, and belongs to the technical field of preparation of composite materials for aerospace. According to the invention, the short carbon fiber toughened ZrCxNy ceramic-based composite material with the density of greater than or equal to 92% is prepared by a wet ball milling, ultrasonic heating and stirring and spark plasma sintering process for the first time. The nitrogen-containing carbide ultrahigh-temperature ceramic-based composite material designed and prepared by the invention is suitable for ultrahigh-temperature ablation-resistant protection at 2500 DEG C or above. Verification shows that after long-time (200s) ablation, the ceramic still keeps a state close to zero ablation rate and a continuous and stable anti-oxidation protection structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite materials for aerospace, and specifically relates to a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material and a preparation method and application thereof, and also relates to a short-cut carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic composite material and a preparation method and application thereof. Background Art

[0002] Ultra-high temperature ceramics (UHTCs) have excellent hardness, high-temperature ablation resistance and thermal shock resistance. They usually include high-melting point transition metal compounds such as borides, carbides and nitrides. They have become the most promising space structural materials. As the flight Mach number of the new generation of hypersonic aircraft continues to increase, more stringent requirements are placed on the thermal protection materials on the aircraft. They need to withstand higher temperatures (≥2500℃), have a longer service life, have higher thermal protection efficiency, and have a lightweight and reliable structure. Therefore, although the existing ultra-high temperature ceramics have many advantages, there are still some urgent problems to be solved before they can be applied to the key hot end components of hypersonic aircraft.

[0003] Carbon fiber has physical properties such as high strength, high modulus, high temperature resistance, corrosion resistance and low thermal expansion coefficient, and is an ideal material for ceramic toughening. Short-cut carbon fiber toughened ceramic matrix composites improve the inherent brittleness of pure ceramic materials, while combining the advantages of ceramic materials such as high temperature resistance, corrosion resistance, ablation resistance and high strength.

[0004] Studies have shown that the N element improves the oxidation resistance and ablation resistance of carbide ceramics, which is a new type of thermal protection material with great application prospects. Among them, zirconium carbonitride ceramics have the advantages of low cost, high melting point, and good ablation resistance. However, the shortcomings of ceramic materials such as brittleness, poor reliability and difficult processing seriously restrict their widespread application in harsh environments. These shortcomings of ceramic materials are determined by the type of bonding between their own atoms. Ceramic materials are usually composed of strong covalent bonds and ionic bonds, and have fewer slip systems. Therefore, ceramic materials are extremely difficult to undergo plastic deformation, and are prone to brittle fracture failure when the external load is too large.

[0005] At present, the toughening method of structural ceramic materials has changed from improving the sintering density of ceramic materials and reducing defects to adding a second phase into the ceramic material that is insensitive to defects and can improve the damage tolerance of the material. Summary of the invention

[0006] In view of the problems of low fracture toughness and insufficient ablation resistance of ultra-high temperature ceramics in the prior art, the present invention provides a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material and its preparation method and application. It is a short-cut carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic composite material and its preparation method and application. For the first time, metal zirconium powder, carbon powder, zirconium nitride, carbon nitride powder, and short-cut carbon fiber are used to prepare a short-cut carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic composite material with a density of ≥92% and a uniform C / N content distribution through wet ball milling + ultrasonic stirring + spark plasma sintering.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material comprises the following steps:

[0009] 1) According to the molar ratio of Zr:C:ZrN:g-C3N4=(1-6):(3-10):(1-3):(0.2-2), metal zirconium powder, carbon powder and zirconium nitride powder are prepared, wherein the powder is a nano-sized powder or a micro-sized powder, and the prepared powder is uniformly mixed by wet ball milling to obtain a mixed powder, and the mixed powder is dried at 50-150° C. for 8-12 h under a vacuum atmosphere, and then passed through a 200-mesh sieve, and the sieved material is used as a spare material for plasma sintering;

[0010] The wet ball milling adopts organic ball milling medium, controls the ball milling speed to be 200-400r / min, the ball milling time to be 12-24h, and the ball to material ratio to be (3-10):1;

[0011] 2) Weighing carbon fiber with a volume fraction of (1-50) vol.% equivalent to the reserve material obtained in step 1), the length of the carbon fiber is 0.5-5 mm, and preparing an ethanol solution in which the carbon fiber is dispersed according to the mass ratio of carbon fiber: anhydrous ethanol = (0.5-2): 200;

[0012] 3) adding the prepared material obtained in step 1) to the carbon fiber-ethanol solution prepared in step 2), stirring and mixing evenly; placing the obtained mixed solution in an oven, drying at 50-100° C. for 24-30 hours, to obtain a mixed powder;

[0013] 4) The mixed powder obtained in step 3) is subjected to spark plasma sintering. The conditions of spark plasma sintering are: the temperature in the sintering furnace is 1600-2500°C, the heat preservation is 5-40min, the heating rate is 25-150°C / min, the cooling rate is 25-150°C / min, the pressure is 10-80Mpa, and the vacuum degree is less than 5pa, so as to obtain a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material. The density of the composite material is ≥92%, and the mass ablation rate is 1×10- -3 g / s-3×10 -3 g / s, the linear ablation rate is 5×10 -3 mm / s-1×10 -2 mm / s.

[0014] In the present invention:

[0015] Furthermore, in step 1), the particle size of the powder is less than 10 μm, and further, the particle size of the powder is less than 3 μm; and the purity of the powder is ≥99.9%.

[0016] Furthermore, in step 1), the ball milling medium is an organic matter, preferably ethanol; the sieve material is used as a spare material for plasma sintering. When used in industry, the spare material is sealed and stored in an airtight condition.

[0017] Furthermore, in step 2), carbon fibers having a volume fraction of (5-40) vol.% equivalent to the reserve material obtained in step 1) are weighed; the purity of the carbon fibers is ≥99.9%.

[0018] Furthermore, in step 4), the conditions of spark plasma sintering are: the temperature in the sintering furnace is 1700-2200°C, the insulation time is 10-30min, the heating rate is 100-150°C / min, the cooling rate is 100-150°C / min, the pressure is 20-60Mpa, and the vacuum degree is <5pa.

[0019] The present invention also relates to a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic matrix composite material, and also to a short carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic composite material, the density of the composite material is ≥92%, and the mass ablation rate is 1×10 after ablation for 200s in an oxyacetylene flame environment at 3000°C. -3 g / s-3×10 -3 g / s, the linear ablation rate is 5×10 -3 mm / s-1×10 -2 mm / s.

[0020] The present invention also relates to the application of the above-mentioned long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material, which is used for ultra-high temperature ablation protection of 2500°C and above.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1. In the preparation process of the long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material described in the present invention, metal zirconium powder, carbon powder, zirconium nitride, carbon nitride powder, and chopped carbon fiber are used for the first time through wet ball milling + ultrasonic stirring + spark plasma sintering to prepare a chopped carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic composite material with a density of ≥92% and uniform C / N content distribution. The preparation process is simple and easy, and the preparation cycle is short; the preparation raw materials have the advantage of low cost.

[0023] 2. The long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material described in the present invention is a new type of ultra-high melting point ceramic-based composite material designed and prepared, which overcomes the defects of existing ceramic-based composite materials such as poor oxidation resistance and weak comprehensive mechanical properties. By improving and optimizing the preparation method of ultra-high temperature ceramic-based composite materials, an ultra-high temperature ceramic-based composite material with good oxidation resistance and ablation resistance and strong comprehensive mechanical properties is prepared.

[0024] 3. The long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic matrix composite material described in the present invention improves the dispersibility of chopped carbon fibers by optimizing the process, and the chopped carbon fiber toughened zirconium carbonitride sample prepared by the present invention has a simple preparation process, a short cycle, and controllable costs; it has excellent antioxidant and ablation resistance, and has high application value in the field of aerospace materials. sf / ZrC x N y The carbon fibers are evenly distributed in the ultra-high temperature ceramic composite materials, without obvious agglomeration or breakage. The prepared material has excellent anti-ablation effect. By selecting appropriate proportions of powder and carbon fibers combined with spark plasma sintering, the obtained samples maintain a low ablation rate after being tested at 3000°C for 200s. The prepared material has good mechanical properties. After compounding an appropriate amount of carbon fiber with the mixed powder, the intrinsic defect of low fracture toughness of the monomer ceramic is improved, and the bending strength and fracture toughness of the ceramic are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 C prepared in Example 1 sf / ZrC 0.75 N 0.25 Macroscopic morphology of the sample surface;

[0026] Figure 2 C prepared in Example 1 sf / ZrC 0.75 N 0.25 Microscopic morphology of the sample surface;.

[0027] Figure 3 C prepared in Example 1 sf / ZrC 0.75 N 0.25 Microscopic morphology of the ablated surface of the sample after ablation in oxyacetylene flame at 3000℃ for 200s DETAILED DESCRIPTION

[0028] The present invention is further described in detail below by way of examples, but these examples should not be considered as limiting the present invention.

[0029] Embodiment 1:

[0030] A method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material comprises the following steps:

[0031] The raw materials were powdered according to the molar ratio of Zr:C:ZrN:g-C3N4=4:5:2:0.5, and ball-milled on a planetary ball mill for 10 hours. The powder particle size was 1-5um and the purity was greater than 99.9%. The ball-milling medium was an ethanol solution, the rotation speed was 300r / min, and the ball-to-material ratio was 4:1. The mixture was then placed in an oven at 70°C and dried for 24 hours. The mixed powder was sieved;

[0032] Weigh 30 vol.% carbon fiber with a length of 0.5 mm, and prepare a carbon fiber-ethanol solution according to the mass ratio of carbon fiber: anhydrous ethanol = 1:200; add the mixed powder to the carbon fiber-ethanol solution and stir to obtain a mixed powder solution; then place it in a 70°C oven to dry for 24 hours, and sieve to obtain a mixed powder;

[0033] The mixed powder was placed in a graphite mold for spark plasma sintering. The vacuum degree in the furnace was less than 5 Pa. The temperature was raised to 1700°C at a heating rate of 80°C / min, kept at that temperature for 15 minutes, and the pressure was 45MPa. Then, it was cooled to room temperature at a cooling rate of 100°C / min. C f / ZrC 0.75 N 0.25 Ceramic composite material (density 95.2%).

[0034] The ablation test was carried out according to the ablation test equipment described in the national standard GJB323A-96. After ablation at 3000℃ for 200s, the mass ablation rate was 1×10 -3 g / s, the linear ablation rate is 2×10 -3 mm / s.

[0035] Embodiment 2:

[0036] A method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material comprises the following steps:

[0037] The raw materials were powdered according to the molar ratio of Zr:C:ZrN:g-C3N4=5:3:1:0.6, and ball-milled on a planetary ball mill for 10 hours. The powder particle size was 1-5um and the purity was greater than 99.9%. The ball-milling medium was an ethanol solution, the rotation speed was 300r / min, and the ball-to-material ratio was 4:1. The mixture was then placed in an oven at 60°C and dried for 24 hours. The mixed powder was sieved to obtain the mixed powder.

[0038] Weigh 20 vol.% carbon fiber with a length of 0.5 mm, and prepare a carbon fiber-ethanol solution according to the mass ratio of carbon fiber: anhydrous ethanol = 0.5:200; add the mixed powder to the carbon fiber-ethanol solution and stir to obtain a mixed powder solution; then place it in a 60°C oven to dry for 24 hours, and sieve to obtain a mixed powder;

[0039] The mixed powder was placed in a graphite mold for spark plasma sintering. The vacuum degree in the furnace was less than 5 Pa. The temperature was raised to 1800 °C at a heating rate of 150 °C / min, kept at that temperature for 30 min, and the pressure was 50 MPa. Then, it was cooled to room temperature at a cooling rate of 150 °C / min to obtain C f / ZrC 0.80 N 0.20 Ceramic composite material (density 92.5%).

[0040] The ablation test was carried out according to the ablation test equipment described in the national standard GJB323A-96. After ablation at 3000℃ for 200s, the mass ablation rate was 2×10 -3 g / s, the linear ablation rate is 2×10 -2 mm / s.

[0041] Embodiment 3:

[0042] A method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material comprises the following steps:

[0043] The raw materials were powdered according to the molar ratio of Zr:C:ZrN:g-C3N4=2:3:1:0.5, and ball-milled on a planetary ball mill for 10 hours. The powder particle size was 1-5um and the purity was greater than 99.9%. The ball-milling medium was ethanol solution, the rotation speed was 300r / min, and the ball-to-material ratio was 4:1. Then, it was placed in a 70°C oven for drying for 24 hours and sieved to obtain a mixed powder;

[0044] Weigh 10 vol.% carbon fiber with a length of 1 mm, and prepare a carbon fiber-ethanol solution according to the mass ratio of carbon fiber: anhydrous ethanol = 2:200; add the mixed powder to the carbon fiber-ethanol solution and stir to obtain a mixed powder solution; then place it in a 70°C oven to dry for 24 hours, and sieve to obtain a mixed powder;

[0045] The mixed powder was placed in a graphite mold for spark plasma sintering. The vacuum degree in the furnace was less than 5 Pa. The temperature was raised to 2200°C at a heating rate of 80°C / min, kept at that temperature for 20 minutes, and the pressure was 60 MPa. Then, the mixed powder was cooled to room temperature at a cooling rate of 100°C / min. C f / ZrC 0.65 N 0.35 Ceramic composite material (density 94.9%).

[0046] The ablation test was carried out according to the ablation test equipment described in the national standard GJB323A-96. After ablation at 3000℃ for 200s, the mass ablation rate was 3×10 -3 g / s, the linear ablation rate is 3×10 -2 mm / s.

[0047] Embodiment 4:

[0048] A method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material comprises the following steps:

[0049] The raw materials were powdered according to the molar ratio of Zr:C:ZrN:g-C3N4=2:5:3:0.6, and ball-milled on a planetary ball mill for 10 hours. The powder particle size was 1-5um and the purity was greater than 99.9%. The ball-milling medium was an ethanol solution, the rotation speed was 300r / min, and the ball-to-material ratio was 4:1. The mixture was then placed in an oven at 60°C and dried for 24 hours. The mixed powder was sieved;

[0050] Weigh 30 vol.% carbon fiber with a length of 3 mm, and prepare a carbon fiber-ethanol solution according to the mass ratio of carbon fiber: anhydrous ethanol = 1.5:200; slowly add the mixed powder into the carbon fiber-ethanol solution, and stir it at the same time to obtain a mixed powder solution; then place it in a 60°C oven to dry for 24 hours, and sieve it to obtain a mixed powder;

[0051] The mixed powder was placed in a graphite mold for spark plasma sintering. The vacuum degree in the furnace was less than 5 Pa. The temperature was raised to 2100°C at a heating rate of 150°C / min, kept at that temperature for 30 minutes, and the pressure was 50 MPa. Then, the mixed powder was cooled to room temperature at a cooling rate of 100°C / min. C f / ZrC 0.82 N 0.18 Ceramic composite material (density 92.3%).

[0052] The ablation test was carried out according to the ablation test equipment described in the national standard GJB323A-96. After ablation at 3000℃ for 200s, the mass ablation rate was 4×10 -3 g / s, the linear ablation rate is 1×10 -2 mm / s.

[0053] Comparative Example:

[0054] The main difference between the comparative example and the embodiment is that no reinforcing and toughening carbon fiber component is added;

[0055] The raw materials were powdered according to the molar ratio of Zr:C:ZrN:g-C3N4=4:5:1:0.5 and ball-milled on a planetary ball mill for 10 hours. The powder particle size was 1-3um and the purity was greater than 99.9%. The ball-milling medium was ethanol solution. The rotation speed was 300r / min and the ball-to-material ratio was 5:1. The powder was then placed in an oven at 70°C and dried for 24 hours. The powder was sieved to obtain the powder.

[0056] The powder is placed in a graphite mold for spark plasma sintering. The vacuum degree in the furnace is less than 5Pa. The temperature is raised to 2100℃ at a heating rate of 80℃ / min, kept for 10 minutes, and the pressure is 30MPa. It is then cooled to room temperature at a cooling rate of 100℃ / min to obtain high-purity single-phase face-centered cubic structure ceramics (density of 96.8%).

[0057] According to the ablation test equipment described in the national standard GJB323A-96, an ablation test was conducted. After ablation for 200s at 3000°C in an oxyacetylene flame environment, there were obvious ablation pits and fractures. The ablation resistance was not as good as the short carbon fiber toughened zirconium carbonitride ultra-high temperature ceramic composite material in Example 3.

[0058] The results show that:

[0059] It can be seen from Examples 1-4 that the obtained long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material has excellent ablation resistance after 3000°C oxyacetylene flame test, and its ablation resistance is significantly improved over that of zirconium carbonitride ultra-high temperature ceramics.

[0060] Comparison of Examples 1-4 and the comparative example shows that adding appropriate chopped carbon fibers can significantly improve the thermal shock resistance and ablation resistance of ceramic materials.

[0061] The above are only preferred implementations of the present invention. The protection scope of the present invention is not limited to the above embodiments. Various process schemes that are not substantially different from the concept of the present invention are within the protection scope of the present invention.

Claims

1. A method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material, characterized in that: The following steps are involved: 1) According to the molar ratio of Zr:C:ZrN:g-C3N4=(1-6):(3-10):(1-3):(0.2-2), metal zirconium powder, carbon powder and zirconium nitride powder are prepared, wherein the powder is a nano-sized powder or a micro-sized powder, and the prepared powder is uniformly mixed by wet ball milling to obtain a mixed powder, and the mixed powder is dried at 50-150° C. for 8-12 h under a vacuum atmosphere, and then passed through a 200-mesh sieve, and the sieved material is used as a spare material for plasma sintering; The wet ball milling adopts organic ball milling medium, controls the ball milling speed to be 200-400r / min, the ball milling time to be 12-24h, and the ball to material ratio to be (3-10):1; 2) Weighing carbon fiber with a volume fraction of (1-50) vol.% equivalent to the reserve material obtained in step 1), the length of the carbon fiber is 0.5-5 mm, and preparing an ethanol solution in which the carbon fiber is dispersed according to the mass ratio of carbon fiber: anhydrous ethanol = (0.5-2): 200; 3) adding the prepared material obtained in step 1) to the carbon fiber-ethanol solution prepared in step 2), stirring and mixing evenly; placing the obtained mixed solution in an oven, drying at 50-100° C. for 24-30 hours, to obtain a mixed powder; 4) The mixed powder obtained in step 3) is subjected to spark plasma sintering. The conditions of spark plasma sintering are: the temperature in the sintering furnace is 1600-2500°C, the heat preservation is 5-40min, the heating rate is 25-150°C / min, the cooling rate is 25-150°C / min, the pressure is 10-80Mpa, and the vacuum degree is less than 5pa, so as to obtain a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material. The density of the composite material is ≥92%, and the mass ablation rate is 1×10- -3 g / s-3×10 -3 g / s, the linear ablation rate is 5×10 -3 mm / s-1×10 -2 mm / s.

2. The method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material according to claim 1, characterized in that: In step 1), the particle size of the powder is less than 10 μm; the purity of the powder is ≥99.9%.

3. The method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material according to claim 2, characterized in that: In step 1), the particle size of the powder is less than 3 μm.

4. The method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material according to claim 1, characterized in that: In step 1), the ball milling medium is ethanol.

5. The method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material according to claim 1, characterized in that: In step 2), carbon fibers having a volume fraction of (5-40) vol.% equivalent to the reserve material obtained in step 1) are weighed; the purity of the carbon fibers is ≥99.9%.

6. The method for preparing a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic-based composite material according to claim 1, characterized in that: In step 4), the conditions of spark plasma sintering are: the temperature in the sintering furnace is 1700-2200°C, the insulation time is 10-30min, the heating rate is 100-150°C / min, the cooling rate is 100-150°C / min, the pressure is 20-60Mpa, and the vacuum degree is <5pa.

7. A long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic matrix composite material, characterized in that: The method for preparing a long-time ablation-resistant zirconium carbonitride ultra-high temperature ceramic matrix composite material according to any one of claims 1 to 6 is used to obtain the composite material, wherein the density of the composite material is ≥92%, and the mass ablation rate is 1×10 -3 g / s-3×10 -3 g / s, the linear ablation rate is 5×10 -3 mm / s-1×10 -2 mm / s.

8. The use of a long-term ablation-resistant zirconium carbonitride ultra-high temperature ceramic matrix composite material as claimed in claim 7, characterized in that: The composite material is used for ultra-high temperature ablation protection at 2500°C and above.

Citation Information

Patent Citations

  • Preparation method for short carbon fiber / silicon carbide composites

    CN103204693A

  • Long-time ablation-resistant ultrahigh-melting-point nitrogen-containing carbide ultrahigh-temperature ceramic and application thereof

    CN110845238A

  • Long-time ablation-resistant ultrahigh-melting-point nitrogen-containing carbide ultrahigh-temperature ceramic and application thereof

    CN111072388A

  • Preparation method of chopped fiber reinforced ceramic matrix composite material

    CN113999012A

  • Chopped carbon fiber gradient toughened ultrahigh-melting-point ceramic-based composite material and preparation method thereof

    CN118063217A

Cited By

  • Preparation method of hafnium carbonitride material, thermal spraying powder and application of thermal spraying powder

    CN119569113A

  • Ablation-resistant connecting piece and preparation method thereof

    CN120906885A