A modified gold tailings micropowder and its preparation method and application

Modified gold tailings micro powder is prepared through dilute sulfuric acid slurry adjustment, surface activation and coating technology, which solves the problem of low mechanical performance of existing modified stone coal vanadium extraction tailings powder in polypropylene composite materials, significantly improving the modification The mechanical properties of gold tailings micro powder and PVC/PP composites achieve higher impact, tensile and bending strengths.

CN118755281BActive Publication Date: 2024-11-22ZHAOYUAN ZHONGHUAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411254450.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing modified stone coal vanadium-extracting tailings powder has low mechanical properties in polypropylene composite materials, and insufficient tensile strength and impact resistance, which limits its application in plastic composite materials.

Method used

Modified gold tailings micro powder is prepared by dilute sulfuric acid slurry, surface activation and coating technology. By adding raw materials such as methyl methacrylate polymer and tributyl phosphate, the compatibility and plasticization properties of the micro powder are improved, and the modification is formed. and compound it with PVC/PP to improve mechanical properties.

Benefits of technology

The mechanical properties of modified gold tailings micro powder and PVC/PP composite materials have been significantly improved, and the impact strength, tensile strength and bending strength have been significantly improved, achieving excellent mechanical performance indicators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a modified gold tailings micropowder and a preparation method and application thereof, and belongs to the technical field of gold tailings micropowder. A method for preparing a modified gold tailings micropowder comprises the following steps: slurry adjustment: adding the gold tailings micropowder to dilute sulfuric acid, stirring, and preparing a suspension with a concentration of 30-50wt%; surface activation: adding a surfactant to the suspension, heating to 60-70°C, stirring for 0.5-2h, adding sodium hexametaphosphate, stirring, obtaining a modified gold tailings micropowder slurry, filtering, and vacuum drying at 70-85°C to obtain an activated gold tailings micropowder dry powder; surface coating: adding a coating agent and a gold tailings micropowder dry powder to a powder surface coating machine, performing high-speed mixing and coating, controlling the temperature at 110-120°C during coating, cooling and crushing after the coating is completed, and obtaining a modified gold tailings micropowder. The modified gold tailings micropowder prepared by the present invention is used in plastics and has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gold tailings micropowder, and in particular to modified gold tailings micropowder and a preparation method and application thereof. Background Art

[0002] Gold tailings powder refers to the powder obtained after drying the overflow mud obtained after separating the coarse sand from the gold tailings. It is the main solid waste discharged after the gold tailings are reduced and recycled. Gold tailings powder mainly contains silicon dioxide, aluminum oxide, potassium oxide and sodium oxide, etc., which can be used to make cement, ceramics and various building materials. Gold tailings powder is used as a raw material to replace clay to produce cement clinker, manufacture sintered bricks, hollow bricks, sintered or non-sintered ceramsite, and pave roads.

[0003] Gold tailings powder contains a large amount of relatively stable silicon dioxide, aluminum oxide and other components. Because its fineness can reach more than 400 mesh, its application scope and application effect in the field of building materials are limited. In practice, the powder can be used as a filler for PVC and PP plastics.

[0004] The Chinese invention patent with publication number CN106867028A discloses a modified stone coal vanadium tailing powder used as a plastic filler and a preparation method thereof. The patent provides a preparation method for a modified stone coal vanadium tailing powder used as a plastic filler. The modified stone coal vanadium tailing powder used as a plastic filler prepared by the method has high hydrophobicity, low oil absorption value and good dispersibility. When used, it can effectively improve the mechanical properties of plastic composite materials and reduce the production cost of plastic composite materials. However, the tensile strength and impact strength of the modified stone coal vanadium tailing powder / polypropylene composite material prepared by the method are only 41.31-51.87MPa and 30.33-44.18KJ / m 2 , the mechanical properties are relatively low. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modified gold tailings powder and a preparation method and application thereof.

[0006] To achieve the above object, the present invention is implemented through the following technical solutions:

[0007] A method for preparing modified gold tailings powder comprises the following steps:

[0008] (1) Slurry preparation: Add gold tailings powder into dilute sulfuric acid and stir to prepare a suspension with a concentration of 30-50wt%;

[0009] (2) Surface activation: add a surfactant to the suspension, heat it to 60-70°C, stir it for 0.5-2h, then add sodium hexametaphosphate and stir it to obtain a modified gold tailings micropowder slurry, filter it, and vacuum dry it at 70-85°C to obtain an activated gold tailings micropowder dry powder;

[0010] (3) Surface coating: Add the coating agent and the dry powder of gold tailings micropowder into the powder surface coating machine for high-speed mixing and coating. The temperature is controlled at 110-120°C during coating. After coating, cool and crush to obtain modified gold tailings micropowder.

[0011] The coating agent is composed of the following raw materials in parts by weight: 10-15 parts of tributyl phosphate and 10-15 parts of methyl methacrylate polymer.

[0012] The methyl methacrylate polymer is prepared by the following method:

[0013] S1: Deionized water, hexamethylenetetramine, tromethamine and glacial acetic acid are added to the reaction kettle in sequence, stirred and dissolved, heated to 65-75°C, reacted for 3-4 hours, cooled to room temperature, separated, and washed with deionized water for 3 times to obtain a first-generation polymer; the reaction equation is as follows:

[0014] S2: Add N,N-dimethylformamide, first-generation polymer, methyl methacrylate, C-94, and 1-butyl-3-methylimidazolium methane sulfonate ionic liquid to the reactor in sequence, protect with nitrogen, heat to 90-100°C, react for 3-5h, cool to room temperature, add deionized water and stir evenly, centrifuge, wash with anhydrous ethanol and deionized water, and dry under vacuum at 70-80°C to obtain methyl methacrylate polymer. The reaction equation is as follows:

[0015]

[0016] Among them, m=n+o+p+q.

[0017] In step S1, the mass ratio of deionized water, hexamethylenetetramine, tromethamine and glacial acetic acid is 100:12:(30-40):(10-15).

[0018] In step S2, the feed mass ratio of N,N-dimethylformamide, first-generation polymer, methyl methacrylate, C-94, and 1-butyl-3-methylimidazolium methane sulfonate ionic liquid is 100:20:(30-40):(0.8-1.2):(1-2).

[0019] After the surfactant and sodium hexametaphosphate are added in step (2), the concentration of the surfactant in the system is 2-3wt%, and the concentration of the sodium hexametaphosphate in the system is 0.2-0.8wt%.

[0020] The surfactant is composed of the following raw materials in parts by weight: 30-50 parts of hexadecyltrimethylammonium bromide and 15-20 parts of sodium petroleum sulfonate.

[0021] In the step (3), the mass ratio of the coating agent to the gold tailings micropowder is 1:(200-300).

[0022] The present invention also provides: modified gold tailings fine powder prepared by adopting the preparation method of the modified gold tailings fine powder.

[0023] The present invention also provides: application of the modified gold tailings powder in plastics.

[0024] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:

[0025] 1. The present invention prepares a novel methyl methacrylate polymer as a coating agent for modifying gold tailings micropowder. The methyl methacrylate polymer contains a large amount of methyl methacrylate groups and has good compatibility with PVC / PP. The methyl methacrylate polymer is coated on the surface of the micropowder, which increases the compatibility of the micropowder and PVC / PP and avoids the problem of agglomeration of the gold tailings micropowder during use. At the same time, the coating agent contains tributyl phosphate, which can be used as a plasticizer for PVC / PP.

[0026] 2. The modified gold tailings powder prepared by the method of the present invention is added to PVC / PP to significantly improve the mechanical properties of the plastic. DETAILED DESCRIPTION

[0027] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.

[0028] Example 1 Preparation of methyl methacrylate polymer:

[0029] S1: 1000g of deionized water, 120g of urotropine, 300g of tromethamine and 100g of glacial acetic acid were added to a reactor in sequence, stirred and dissolved, heated to 65°C, reacted for 3h, cooled to room temperature to separate the layers, separated the water layer, and washed with deionized water for 3 times (using 180g of deionized water each time) to obtain a first-generation polymer;

[0030] S2: 1000g N,N-dimethylformamide, 200g first-generation polymer, 300g methyl methacrylate, 8g C-94, and 10g 1-butyl-3-methylimidazolium methane sulfonate ionic liquid were added to the reactor in sequence, protected by nitrogen, heated to 90°C, reacted for 5h, cooled to room temperature, added with 1000g deionized water and stirred evenly, centrifuged, washed once with 200g anhydrous ethanol, and then washed with 250g deionized water, and vacuum dried at 70°C for 12h to obtain methyl methacrylate polymer.

[0031] Example 2 Preparation of methyl methacrylate polymer:

[0032] S1: 1000g of deionized water, 120g of urotropine, 350g of tromethamine, and 125g of glacial acetic acid were added to a reactor in sequence, stirred and dissolved, heated to 70°C, reacted for 3.5h, cooled to room temperature, separated, and washed with deionized water for 3 times (180g of deionized water each time) to obtain a first-generation polymer;

[0033] S2: 1000g N,N-dimethylformamide, 200g first-generation polymer, 350g methyl methacrylate, 10g C-94, and 15g 1-butyl-3-methylimidazolium methane sulfonate ionic liquid were added to the reactor in sequence, and the temperature was raised to 95°C under nitrogen protection. The reaction was performed for 4h, and the temperature was lowered to room temperature. 1000g deionized water was added and stirred evenly. The mixture was centrifuged and washed once with 200g anhydrous ethanol and then washed once with 250g deionized water. The mixture was dried under vacuum at 75°C for 10h to obtain methyl methacrylate polymer.

[0034] Example 3 Preparation of methyl methacrylate polymer:

[0035] S1: 1000g of deionized water, 120g of urotropine, 400g of tromethamine, and 150g of glacial acetic acid were added to a reactor in sequence, stirred and dissolved, heated to 75°C, reacted for 3h, cooled to room temperature, separated, and washed with deionized water for 3 times (180g of deionized water each time) to obtain a first-generation polymer;

[0036] S2: 1000g N,N-dimethylformamide, 200g first-generation polymer, 400g methyl methacrylate, 12g C-94, and 20g 1-butyl-3-methylimidazolium methane sulfonate ionic liquid were added to the reactor in sequence, and the temperature was raised to 100°C under nitrogen protection. The reaction was carried out for 3h, and the temperature was lowered to room temperature. 1000g deionized water was added and stirred evenly. The mixture was centrifuged and washed once with 200g anhydrous ethanol and then washed once with 250g deionized water. The mixture was dried under vacuum at 80°C for 8h to obtain methyl methacrylate polymer.

[0037] Example 4

[0038] A modified gold tailings powder is prepared by the following method:

[0039] (1) Slurry preparation: Add gold tailings powder into 10wt% dilute sulfuric acid and stir to prepare a 30wt% suspension;

[0040] (2) Surface activation: add a surfactant to the suspension to make the concentration of the surfactant in the system 2wt%, heat to 60°C, stir for 0.5h, then add sodium hexametaphosphate to make the concentration of sodium hexametaphosphate in the system 0.2wt%, stir for 0.5h to obtain a modified gold tailings micropowder slurry, filter, and vacuum dry at 70°C for 12h to obtain an activated gold tailings micropowder dry powder; the surfactant in this step is composed of the following raw materials in parts by weight: 30 parts of hexadecyltrimethylammonium bromide and 15 parts of sodium petroleum sulfonate;

[0041] Surface coating: Add the coating agent and the dry powder of gold tailings micropowder into a powder surface coating machine for high-speed mixing and coating. The temperature is controlled at 110°C during coating. After coating, the powder is cooled and crushed to obtain modified gold tailings micropowder. In this step, the coating agent is composed of the following raw materials in parts by weight: 10 parts of tributyl phosphate and 10 parts of methyl methacrylate polymer (prepared in Example 1). The mass ratio of the coating agent to the dry powder of gold tailings micropowder is 1:200.

[0042] Example 5

[0043] A modified gold tailings powder is prepared by the following method:

[0044] (1) Slurry preparation: Add gold tailings powder into 12wt% dilute sulfuric acid and stir to prepare a 40wt% suspension;

[0045] (2) Surface activation: add a surfactant to the suspension to make the concentration of the surfactant in the system 2.5wt%, heat to 65°C, stir for 1h, then add sodium hexametaphosphate to make the concentration of sodium hexametaphosphate in the system 0.5wt%, stir for 1h to obtain a modified gold tailings micropowder slurry, filter, and vacuum dry at 80°C for 10h to obtain an activated gold tailings micropowder dry powder; in this step, the surfactant is composed of the following raw materials in parts by weight: 40 parts of hexadecyltrimethylammonium bromide and 15 parts of sodium petroleum sulfonate;

[0046] (3) Surface coating: Add the coating agent and the dry powder of gold tailings micropowder into a powder surface coating machine for high-speed mixing and coating. The temperature is controlled at 115°C during coating. After coating, the powder is cooled and crushed to obtain modified gold tailings micropowder. In this step, the coating agent is composed of the following raw materials in parts by weight: 12 parts of tributyl phosphate and 15 parts of methyl methacrylate polymer (prepared in Example 2). The mass ratio of the coating agent to the dry powder of gold tailings micropowder is 1:250.

[0047] Example 6

[0048] A modified gold tailings powder is prepared by the following method:

[0049] (1) Slurry preparation: Add gold tailings powder into 15wt% dilute sulfuric acid and stir to prepare a 50wt% suspension;

[0050] (2) Surface activation: add a surfactant to the suspension to make the concentration of the surfactant in the system 3wt%, heat to 70°C, stir for 2h, then add sodium hexametaphosphate to make the concentration of sodium hexametaphosphate in the system 0.8wt%, stir for 2h to obtain a modified gold tailings micropowder slurry, filter, and vacuum dry at 85°C for 9h to obtain an activated gold tailings micropowder dry powder; in this step, the surfactant is composed of the following raw materials in parts by weight: 50 parts of hexadecyltrimethylammonium bromide and 20 parts of sodium petroleum sulfonate;

[0051] (3) Surface coating: Add the coating agent and the dry powder of gold tailings micropowder into a powder surface coating machine for high-speed mixing and coating. The temperature is controlled at 120°C during coating. After coating, the powder is cooled and crushed to obtain modified gold tailings micropowder. In this step, the coating agent is composed of the following raw materials in parts by weight: 15 parts of tributyl phosphate and 12 parts of methyl methacrylate polymer (prepared in Example 3). The mass ratio of the coating agent to the dry powder of gold tailings micropowder is 1:300.

[0052] Application Example 1

[0053] 300 g of modified gold tailings powder (prepared in Example 4), 100 g of PVC, 15 g of zinc stearate, 20 g of dioctyl phthalate, 10 g of antioxidant SP, and 5 g of accelerator ZBEC were mixed uniformly, put into an open mill, and mixed at 190° C. for 15 min. After mixing uniformly, vulcanized on a flat vulcanizer to obtain a PVC material.

[0054] Application Example 2

[0055] 300 g of modified gold tailings powder (prepared in Example 5), 100 g of PVC, 15 g of zinc stearate, 20 g of dioctyl phthalate, 10 g of antioxidant SP, and 5 g of accelerator ZBEC were mixed uniformly, put into an open mill, and mixed at 190° C. for 15 min. After mixing uniformly, vulcanized on a flat vulcanizer to obtain a PVC material.

[0056] Application Example 3

[0057] 300 g of modified gold tailings powder (prepared in Example 6), 100 g of PVC, 15 g of zinc stearate, 20 g of dioctyl phthalate, 10 g of antioxidant SP, and 5 g of accelerator ZBEC were mixed uniformly, put into an open mill, and mixed at 190° C. for 15 min. After mixing uniformly, vulcanized on a flat vulcanizer to obtain a PVC material.

[0058] Application Example 4

[0059] 300 g of modified gold tailings powder (prepared in Example 5), 100 g of PP, 15 g of zinc stearate, 20 g of dioctyl phthalate, 10 g of antioxidant SP, and 5 g of accelerator ZBEC were mixed uniformly, put into an open mill, and mixed at 190° C. for 15 min. After mixing uniformly, vulcanized on a flat vulcanizer to obtain a PVC material.

[0060] Comparative Example 1

[0061] The difference from Application Example 2 is that the modified gold tailings powder used is different. The preparation method of the modified gold tailings powder is basically the same as that of Example 5, except that no methyl methacrylate polymer is added to the coating agent in step (3).

[0062] Comparative Example 2

[0063] The difference from Application Example 4 is that the modified gold tailings powder used is different. The preparation method of the modified gold tailings powder is basically the same as that of Example 5, except that no methyl methacrylate polymer is added to the coating agent in step (3).

[0064] Comparative Example 3

[0065] The difference from Application Example 2 is that the modified gold tailings powder used is different. The preparation method of the modified gold tailings powder is basically the same as that of Example 5, the difference being that the coating agent in step (3) is replaced by an equal weight of KH-570 silane coupling agent.

[0066] Comparative Example 4

[0067] The difference from Application Example 2 is that the modified gold tailings powder is replaced by an equal weight of unmodified gold tailings powder.

[0068] The main components of the gold tailings powder used in the examples and comparative examples of the present application are silicon dioxide (60.18wt%), aluminum oxide (19.47wt%), calcium oxide (2.64wt%), and iron oxide (2.39 wt%); the brand of PP used is polypropylene T36F; and the brand of PVC used is S-700 from Qilu Petrochemical.

[0069] The composite materials prepared in Application Examples 1-4 and Comparative Examples 1-4 of the present application were tested for impact strength (GB / T 1043.2-2018), tensile strength (GB / T1040.2-2022) and flexural strength (GB / T 9341-2008). The test results are shown in Table 1.

[0070] Table 1

[0071]

[0072] It can be seen from Table 1 Application Examples 1-3 that the composite materials obtained by compounding the modified gold tailings powder prepared by the present invention with PVC have excellent mechanical properties, and the impact strength is greater than 125KJ / m 2 , tensile strength>50MPa, flexural strength>105MPa.

[0073] Application Example 4 is a composite material obtained by compounding the modified gold tailings powder prepared by the present invention with PP, which has excellent mechanical properties and an impact strength of 139KJ / m 2 , tensile strength is 62MPa and flexural strength is 121MPa.

[0074] Comparative Examples 1 and 3 are composite materials prepared by compounding modified gold tailings powder and PVC in different modification methods. It can be seen from the data in Table 1 that the impact strength is less than 90KJ / m 2 , tensile strength ≤50MPa, flexural strength <100MPa.

[0075] Comparative Example 2 is a composite material obtained by compounding modified gold tailings powder prepared by different modification methods with PP. From the data in Table 1, it can be seen that its impact strength is 61KJ / m 2 , tensile strength is 50MPa and flexural strength is 83MPa.

[0076] Comparative Example 4 is a composite material obtained by compounding unmodified gold tailings powder with PVC. From the data in Table 1, it can be seen that its impact strength is 41KJ / m 2 , tensile strength is 38MPa and flexural strength is 59MPa.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing modified gold tailings powder, characterized in that: The following steps are involved: (1) Slurry preparation: Add gold tailings powder into dilute sulfuric acid and stir to prepare a suspension with a concentration of 30-50wt%; (2) Surface activation: add a surfactant to the suspension, heat it to 60-70°C, stir it for 0.5-2h, then add sodium hexametaphosphate and stir it to obtain a modified gold tailings micropowder slurry, filter it, and vacuum dry it at 70-85°C to obtain an activated gold tailings micropowder dry powder; (3) Surface coating: Add the coating agent and the activated gold tailings micropowder into a powder surface coating machine for high-speed mixing and coating. The temperature is controlled at 110-120°C during coating. After coating, cool and crush to obtain modified gold tailings micropowder. The coating agent is composed of the following raw materials in parts by weight: 10-15 parts of tributyl phosphate and 10-15 parts of methyl methacrylate polymer; The methyl methacrylate polymer is prepared by the following method: S1: Deionized water, hexamethylenetetramine, tromethamine and glacial acetic acid were added to a reaction kettle in sequence, stirred and dissolved, heated to 65-75°C, reacted for 3-4 hours, cooled to room temperature and separated, the water layer was separated, and washed with deionized water for 3 times to obtain a first-generation polymer; S2: Add N,N-dimethylformamide, first-generation polymer, methyl methacrylate, C-94, and 1-butyl-3-methylimidazolium methane sulfonate ionic liquid to the reactor in sequence, protect with nitrogen, heat to 90-100°C, react for 3-5 hours, cool to room temperature, add deionized water and stir evenly, centrifuge, wash with anhydrous ethanol and deionized water, and vacuum dry at 70-80°C to obtain methyl methacrylate polymer.

2. The method for preparing modified gold tailings powder according to claim 1, characterized in that: In step S1, the mass ratio of deionized water, hexamethylenetetramine, tromethamine and glacial acetic acid is 100:12:(30-40):(10-15).

3. The method for preparing modified gold tailings powder according to claim 1, characterized in that: In step S2, the feed mass ratio of N,N-dimethylformamide, first-generation polymer, methyl methacrylate, C-94, and 1-butyl-3-methylimidazolium methane sulfonate ionic liquid is 100:20:(30-40):(0.8-1.2):(1-2).

4. The method for preparing modified gold tailings powder according to claim 1, characterized in that: After the surfactant and sodium hexametaphosphate are added in step (2), the concentration of the surfactant in the system is 2-3wt%, and the concentration of the sodium hexametaphosphate in the system is 0.2-0.8wt%.

5. The method for preparing modified gold tailings powder according to claim 1, characterized in that: The surfactant is composed of the following raw materials in parts by weight: 30-50 parts of hexadecyltrimethylammonium bromide and 15-20 parts of sodium petroleum sulfonate.

6. The method for preparing modified gold tailings powder according to claim 1, characterized in that: In the step (3), the mass ratio of the coating agent to the activated gold tailings micropowder is 1:(200-300).

7. A modified gold tailings fine powder prepared by the method for preparing modified gold tailings fine powder according to any one of claims 1 to 6.