Temperature-sensitive intelligent control slurry, temperature-sensitive intelligent control coating and preparation method

Thermal intelligent control slurries and coatings are prepared by using molybdenum and tungsten-doped vanadium oxide thermal phase change materials, which solves the problem of limited temperature adjustment function of existing thermal phase change materials and achieves significant phase change conversion effects and high-temperature infrared reflection. It is suitable for use on a variety of material surfaces and has good adhesion and weather resistance.

CN118755299AInactive Publication Date: 2024-10-11SHANGHAI HUZHENG IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411244944.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing thermal phase change materials have limited temperature-regulating effects when hot and cold changes, and there is still room for improvement in application fields and performance, especially in terms of phase change range and sensitivity.

Method used

Molybdenum and tungsten doped vanadium oxide thermal phase change materials are used to prepare heat-sensitive intelligent control nanoparticles and combined with polyethylene glycol and other ingredients to prepare heat-sensitive intelligent control slurries and coatings, which are coated on glass, plastics, and metals. and other material surfaces to achieve intelligent temperature control functions.

Benefits of technology

It significantly improves the phase change conversion effect, has high temperature infrared reflectivity and good adhesion, and has strong weather resistance. It is suitable for automobiles, construction and other fields, and achieves stable thermal intelligent control effects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a thermosensitive intelligent control slurry, a thermosensitive intelligent control coating and a preparation method of the thermosensitive intelligent control slurry, and the thermosensitive intelligent control slurry is formed in a medium by preparing thermosensitive intelligent control nano particles and grinding and dispersing the thermosensitive intelligent control nano particles. The thermosensitive intelligent control slurry is further used for preparing a thermosensitive intelligent control coating. The prepared coating has the characteristics of thermal-sensitive intelligent control, namely infrared light transmission at low temperature and infrared reflection at high temperature, and has good application prospects in the aspects of roofs, outer wall coatings, containers, oil storage tank coatings, coatings of vehicles such as automobiles and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of slurries and coatings, and specifically to a thermal-sensitive intelligent-control slurry, a thermal-sensitive intelligent-control coating and a preparation method thereof. Background Art

[0002] As climate change becomes increasingly drastic, people have higher requirements for stable temperature perception. At the same time, in some areas, due to the influence of factors such as climate and environment, the changes in temperature are strong, causing people to feel uncomfortable. The development of thermal phase change materials helps to solve these problems. By controlling the phase change temperature, it can play a role in temperature regulation when the temperature changes. Thermal phase change materials are applied to functional coatings and can have a very wide range of application prospects, such as car and aircraft paint, building roofs, exterior walls, glass coatings for windows, and coatings for oil storage tanks and containers, etc., to achieve intelligent temperature control effects. Chinese patent CN114775296A discloses a high-light reflective phase change thermal storage coating for textiles. The phase change enthalpy value is increased by modifying the phase change microcapsule coating, achieving near-infrared reflection, and alleviating the problem of textiles being cold in winter and hot in summer. Chinese patent CN114621668B discloses a heat-insulating phase change coating, which uses polyethylene glycol-based polyurethane and tungsten-doped vanadium dioxide to form an emulsion, which is sprayed on the surface of the substrate to achieve heat insulation and heat preservation functions. There is still a lot of room for improvement in the performance of functional materials, such as the phase change range and sensitivity, the functional changes before and after the phase change, etc. There is also a lot of room for expansion in its application areas. In summary, a solution needs to be given to solve the problem. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a thermal-sensitive intelligent control slurry which is sensitive to phase change and has obvious phase change conversion effect, and on this basis, proposes a thermal-sensitive intelligent control coating which can be used on the surface of materials such as plastic, glass, and metal, and has outstanding thermal-sensitive intelligent control performance.

[0004] A method for preparing a thermosensitive intelligent control slurry and a thermosensitive intelligent control coating is as follows: (1) Preparation of thermosensitive intelligent control nanoparticles: According to the mass ratio, 1-3 parts of butyl titanate are added to 30-80 parts of ethanol and stirred to form solution A; 0.02-0.0.05 parts of ammonium molybdate are added to 10-20 parts of ethanol and stirred to form solution B. The two solutions are mixed evenly, and a hydrochloric acid / acetic acid solution with a concentration of 0.1-0.3 mol / L is added, heated to 40-50°C and stirred for 1-3 hours to form reactant C; 10-20 parts of ammonium vanadate, 0 .1-0.5 parts of ammonium tungstate and 0.01-0.05 parts of ammonium molybdate are added to 1000-2000 parts of ethanol in sequence and stirred evenly, 0.1-0.5 parts of polyethylene glycol (molecular weight 1000-3000g / mol) are added, reactant C is added, a pH regulator is added, and the mixture is heated to 45-55°C and stirred for 24-36 hours; the mixture is centrifuged, washed and dried, and calcined at 400-450°C with oxygen for 3-5 hours to obtain thermosensitive intelligent control nanoparticles; (2) Preparation of thermosensitive intelligent control slurry: According to the mass ratio, 1-5 parts of thermosensitive intelligent control nanoparticles are added to 10-20 parts of 1-2 mol / L hydrochloric acid for 1-2 hours, and then centrifuged and washed. Then, 0.05-0.1 parts of polyvinyl pyrrolidone (molecular weight 5000-20000 g / mol), 0.05-0.1 parts of polypropylene glycol (molecular weight 400-1000 g / mol), 0.02-0.05 parts of wetting agent and 50-80 parts of grinding medium are wet-milled for 1-3 hours to obtain thermosensitive intelligent control slurry.

[0005] Preferably, in step (1) of the method for preparing the thermosensitive intelligent control slurry, the mass ratio of hydrochloric acid to acetic acid in the hydrochloric acid / acetic acid solution is (2-4):1, and the hydrochloric acid / acetic acid solution is added through a microinjection pump at a rate of 1-3 ml / min; the pH adjuster is triethylamine, and the pH is adjusted to 8.5-10.

[0006] Preferably, in step (2) of the method for preparing the thermosensitive intelligent control slurry, the grinding medium is selected from one or more of ethanol, isopropanol, ethyl acetate, butyl acetate, toluene, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and ethylene glycol butyl ether acetate; and the wetting agent is selected from BYK164, BYK163, and BYK165.

[0007] Specifically, the present invention further provides a thermal-sensitive intelligent control coating, which is composed of the following components in percentage by mass: 30-50% of the thermosensitive intelligent control slurry prepared by the above preparation method; Film-forming resin 20-40%; Leveling agent 0.1-1%; Coupling agent 0.1-1%; The balance is solvent.

[0008] Among them, the film-forming resin is selected from acrylic resin, polyurethane resin, epoxy resin, the leveling agent is polyether polyester modified silicone, the coupling agent is silane coupling agent, and the solvent is consistent with the grinding medium of the thermal sensitive intelligent control slurry.

[0009] According to the embodiment, the thermosensitive intelligent control coating is prepared by the following method: weigh the components in the aforementioned mass percentages, mix the leveling agent, coupling agent, film-forming resin and solvent evenly to form a solution, gradually add the thermosensitive intelligent control slurry into the solution, stir at 1000-1500r / min for 1-2h, pass through a 200-mesh sieve, and obtain the thermosensitive intelligent control coating.

[0010] Compared with the prior art, the technical effect of the present invention is as follows: the present invention prepares a thermal-sensitive intelligent control slurry and applies it to a thermal-sensitive intelligent control coating. When the coating is applied to glass, plastic, metal and other substrates, the functional effect of intelligent temperature control can be achieved. Specifically, when the ambient temperature is lower than the phase change temperature of the material, the infrared light is in the transmission stage, and there is basically no effect when it is irradiated through the coating surface; when the ambient temperature is higher than the phase change temperature of the material, the crystal structure of the material changes, and the infrared light is in the reflection stage. When it is irradiated through the coating surface, it is reflected to achieve the temperature control function. This is mainly due to the performance of the molybdenum-tungsten-doped vanadium oxide thermal phase change material. At the same time, the molybdenum-doped titanium oxide material effectively supplements the ultraviolet blocking and infrared reflection properties, thereby enhancing the thermal-sensitive intelligent control functional effect of the coating. The coating formulated by the present invention can have a stable and durable thermal-sensitive intelligent control effect, and also has good adhesion to the substrate.

[0011] The thermal-sensitive intelligent control coating prepared by the present invention has the following advantages: significant phase change conversion effect, high infrared reflectivity at high temperature, good adhesion, and strong weather resistance. The thermal-sensitive intelligent control coating has high application value in the fields of automobiles, buildings, containers, oil storage tanks, etc. DETAILED DESCRIPTION

[0012] The present invention will be further described below in conjunction with specific embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the scope of protection of the present invention. After reading the content of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent changes and modifications also fall within the scope defined by the claims of the present invention.

[0013] The other raw materials used in the following examples are all commercially available products unless otherwise specified.

[0014] The preparation method of the thermosensitive intelligent control slurry in Example 1 is as follows: (1) Preparation of thermosensitive intelligent control nanoparticles: 10g of butyl titanate was added to 800ml of ethanol and stirred to form solution A; 0.2g of ammonium molybdate was added to 150ml of ethanol and stirred to form solution B. The two solutions were mixed evenly, and a 0.2mol / L hydrochloric acid / acetic acid solution was added thereto at a rate of 2ml / min using a microinjection pump. The ratio of hydrochloric acid / acetic acid was 3:1, and the solution was heated to 45°C and stirred for 1h to form reactant C; 100g of ammonium vanadate, 1.5g of ammonium tungstate, and 0.2g of ammonium molybdate were added to 2000ml of ethanol in sequence and stirred evenly, and 4g of polyethylene glycol (molecular weight 2000g / mol) was added, and reactant C was added. Triethylamine was added to adjust the pH to 8.5, and the solution was heated to 55°C and stirred for 24h; the solution was washed by centrifugation and dried, and calcined at 450°C in an oxygen-free environment for 5h to obtain thermosensitive intelligent control nanoparticles; (2) Preparation of thermosensitive intelligent control slurry: 20 g of thermosensitive intelligent control nanoparticles were soaked in 120 ml of 1 mol / L hydrochloric acid for 2 h and then centrifuged and washed. They were then wet-milled for 2 h with 0.5 g of polyvinyl pyrrolidone (molecular weight 20,000 g / mol), 0.5 g of polypropylene glycol (molecular weight 1,000 g / mol), 0.3 g of BYK164, 100 ml of isopropanol, 200 ml of methyl isobutyl ketone, and 400 ml of ethylene glycol dimethyl ether to obtain thermosensitive intelligent control slurry.

[0015] The obtained thermal intelligent control slurry is used for the preparation of thermal intelligent control coatings. Weigh according to the mass percentage of each component: 35% thermal intelligent control slurry, 30% acrylic resin, 0.3% leveling agent polyether polyester copolymer modified polysiloxane, 0.5% coupling agent KH-570, and the remainder is solvent (the volume ratio of isopropyl alcohol: methyl isobutyl ketone: ethylene glycol dimethyl ether is 1:2:4). Mix the leveling agent, coupling agent, film-forming resin and solvent evenly to form a solution, and then gradually add the thermal intelligent control slurry to the solution, stir at 1200r / min for 2h, and pass through a 200-mesh sieve to obtain a thermal intelligent control coating.

[0016] The preparation method of the thermosensitive intelligent control slurry in Example 2 is as follows: (1) Preparation of thermosensitive intelligent control nanoparticles. 10g of butyl titanate was added to 800ml of ethanol and stirred to form solution A; 0.2g of ammonium molybdate was added to 120ml of ethanol and stirred to form solution B. The two solutions were mixed evenly, and a 0.2mol / L hydrochloric acid / acetic acid solution was added thereto at a rate of 1.5ml / min using a microinjection pump. The ratio of hydrochloric acid / acetic acid was 3:1, and the mixture was heated to 50°C and stirred for 1h to form reactant C; 100g of ammonium vanadate, 1.8g of ammonium tungstate, and 0.2g of ammonium molybdate were added to 2000ml of ethanol in sequence and stirred evenly, 5g of polyethylene glycol (molecular weight 1000g / mol) was added, reactant C was added, triethylamine was added to adjust the pH to 9, and the mixture was heated to 50°C and stirred for 36h; the mixture was centrifuged, washed, and dried, and calcined at 450°C in an oxygen-free environment for 5h to obtain thermosensitive intelligent control nanoparticles; (2) Preparation of thermosensitive intelligent control slurry: 20 g of thermosensitive intelligent control nanoparticles were soaked in 150 ml of 1 mol / L hydrochloric acid for 2 h and then centrifuged and washed. They were then wet-milled with 0.6 g of polyvinyl pyrrolidone (molecular weight 20,000 g / mol), 0.6 g of polypropylene glycol (molecular weight 1,000 g / mol), 0.3 g of BYK163, 100 ml of isopropanol, 300 ml of butyl acetate, and 300 ml of diethylene glycol dimethyl ether for 2 h to obtain thermosensitive intelligent control slurry.

[0017] The obtained thermal intelligent control slurry is used for the preparation of thermal intelligent control coatings. Weigh according to the mass percentage of each component: 36% thermal intelligent control slurry, 28% polyurethane resin, 0.2% leveling agent polyether polyester copolymer modified polysiloxane, 0.5% coupling agent KH-550, and the remainder is solvent (the volume ratio of isopropyl alcohol: butyl acetate: diethylene glycol dimethyl ether is 1:3:3). The leveling agent, coupling agent, film-forming resin and solvent are evenly mixed to form a solution, and then the thermal intelligent control slurry is gradually added to the solution, stirred at 1000r / min for 2h, and passed through a 200-mesh sieve to obtain a thermal intelligent control coating.

[0018] The preparation method of the thermosensitive intelligent control slurry in Example 3 is as follows: (1) Preparation of thermosensitive intelligent control nanoparticles: 10g of butyl titanate was added to 800ml of ethanol and stirred to form solution A; 0.3g of ammonium molybdate was added to 150ml of ethanol and stirred to form solution B. The two solutions were mixed evenly, and a 0.2mol / L hydrochloric acid / acetic acid solution was added thereto at a rate of 3ml / min using a microinjection pump. The ratio of hydrochloric acid / acetic acid was 4:1, and the solution was heated to 50°C and stirred for 2h to form reactant C; 100g of ammonium vanadate, 1.8g of ammonium tungstate, and 0.1g of ammonium molybdate were added to 2000ml of ethanol in sequence and stirred evenly, and 5g of polyethylene glycol (molecular weight 2000g / mol) was added, and reactant C was added. Triethylamine was added to adjust the pH to 9, and the solution was heated to 55°C and stirred for 24h; the solution was washed by centrifugation and dried, and calcined at 450°C in an oxygen-free environment for 5h to obtain thermosensitive intelligent control nanoparticles; (2) Preparation of thermosensitive intelligent control slurry: 20 g of thermosensitive intelligent control nanoparticles were immersed in 150 ml of 1 mol / L hydrochloric acid for 2 h and then centrifuged and washed. They were then wet-milled for 2 h with 0.5 g of polyvinyl pyrrolidone (molecular weight 20,000 g / mol), 0.7 g of polypropylene glycol (molecular weight 1,000 g / mol), 0.3 g of BYK165, 100 ml of ethanol, 300 ml of diisobutyl ketone, and 400 ml of diethylene glycol dimethyl ether to obtain thermosensitive intelligent control slurry.

[0019] The obtained thermal intelligent control slurry is used for the preparation of thermal intelligent control coatings. Weigh according to the mass percentage of each component: 35% thermal intelligent control slurry, 28% epoxy resin, 0.5% leveling agent polyether polyester copolymer modified polysiloxane, 0.5% coupling agent KH-560, and the remainder is solvent (ethanol: diisobutyl ketone: diethylene glycol dimethyl ether volume ratio is 1:3:4). Mix the leveling agent, coupling agent, film-forming resin and solvent evenly to form a solution, and then gradually add the thermal intelligent control slurry to the solution, stir at 1500r / min for 2h, pass through a 200-mesh sieve, and obtain a thermal intelligent control coating.

[0020] Test Example The thermosensitive intelligent control coating prepared in each embodiment was coated on the surface of a transparent PET film substrate, and after drying at 80°C for about 100 minutes, the coating performance was tested. The adhesion was tested by the Baige method, the hardness was tested by the GB / T6739-2006 standard method, the aging resistance was tested for 2000 hours in a rapid UV aging box, and the clarity was measured by a haze meter. The blocking and transmission of visible light, ultraviolet light and infrared light (1400nm) were tested by the solar film tester LS182. In the infrared blocking rate test, the test environment temperature was controlled to be constant at 25°C and 45°C for 1 hour, and its changes were tested.

[0021] The test results are shown in Table 1. The tests show that the coatings of each embodiment show a high performance level, with adhesion reaching level 0 and hardness reaching 2H. The coating shows high aging resistance. After 2000h of rapid UV aging, the appearance and performance have not changed, and the surface has outstanding weather resistance. The haze test results show that the clarity of the coating has reached a very high level of clarity, and the haze is less than 1%. In addition, the coating samples have a high UV blocking rate and good visible light transmittance. With the change of ambient temperature, the infrared blocking rate can change from 82% at 25°C to 93% at 45°C, indicating its outstanding thermal intelligent control and heat insulation function. The above tests show that the coatings prepared by each embodiment have outstanding performance and have good application prospects in the field of intelligent environmental protection and energy saving.

[0022] Example 1 Example 2 Example 3 Adhesion Level 0 Level 0 Level 0 hardness 2H 2H 2H QUV2000h No change No change No change Haze 0.8% 0.8% 0.9% UV blocking rate 99% 99% 99% Visible light transmittance 72% 74% 72% Infrared blocking rate (25℃) 82% 83% 81% Infrared blocking rate (45℃) 93% 92% 90% The above content is a detailed description of the present invention in combination with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art of the present invention, without departing from the concept of the present invention, several simple deductions or substitutions can be made, which should be regarded as falling within the scope of protection of the present invention.

Claims

1. A method for preparing a thermosensitive intelligent control slurry, characterized in that: The method is as follows: (1) Preparation of thermosensitive intelligent control nanoparticles: According to the mass ratio, 1-3 parts of butyl titanate are added to 30-80 parts of ethanol and stirred to form solution A; 0.02-0.0.05 parts of ammonium molybdate are added to 10-20 parts of ethanol and stirred to form solution B. The two solutions are mixed evenly, and a hydrochloric acid / acetic acid solution with a concentration of 0.1-0.3 mol / L is added, and the mixture is heated to 40-50°C and stirred for 1-3 hours to form reactant C; 10-20 parts of ammonium vanadate, 0.1-0.5 parts of ammonium tungstate, and 0.01-0.05 parts of ammonium molybdate are sequentially added to 1000-2000 parts of ethanol and stirred evenly, 0.1-0.5 parts of polyethylene glycol with a molecular weight of 1000-3000 g / mol are added, reactant C is added, a pH regulator is added, and the mixture is heated to 45-55° C. and stirred for 24-36 hours; the mixture is centrifugally cleaned and dried, and oxygen-free calcined at 400-450° C. for 3-5 hours to obtain thermosensitive intelligent control nanoparticles; (2) Preparation of thermosensitive intelligent control slurry: According to the mass ratio, 1-5 parts of thermosensitive intelligent control nanoparticles are added to 10-20 parts of 1-2 mol / L hydrochloric acid for 1-2 hours and then centrifuged for washing. Then, 0.05-0.1 parts of polyvinyl pyrrolidone with a molecular weight of 5000-20000 g / mol, 0.05-0.1 parts of polypropylene glycol with a molecular weight of 400-1000 g / mol, 0.02-0.05 parts of wetting agent and 50-80 parts of grinding medium are wet-milled for 1-3 hours to obtain thermosensitive intelligent control slurry.

2. The method for preparing the thermosensitive intelligent control slurry according to claim 1, characterized in that: In step (1), the mass ratio of hydrochloric acid to acetic acid in the hydrochloric acid / acetic acid solution is (2-4):1, and the hydrochloric acid / acetic acid solution is added at a rate of 1-3 ml / min through a microinjection pump.

3. The method for preparing the thermosensitive intelligent control slurry according to claim 1, characterized in that: In step (1), the pH adjusting agent is triethylamine, and the pH is adjusted to 8.5-10.

4. The method for preparing the thermosensitive intelligent control slurry according to claim 1, characterized in that: In step (2), the grinding medium is selected from one or more of ethanol, isopropanol, ethyl acetate, butyl acetate, toluene, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and ethylene glycol butyl ether acetate.

5. The method for preparing the thermosensitive intelligent control slurry according to claim 1, characterized in that: In step (2), the wetting agent is selected from BYK164, BYK163, and BYK165.

6. A thermal-sensitive intelligent control coating, characterized in that: The following mass percentage content composition: 30-50% of the thermosensitive intelligent control slurry prepared by the preparation method according to any one of claims 1 to 5; Film-forming resin 20-40%; Leveling agent 0.1-1%; Coupling agent 0.1-1%; The balance is solvent; The film-forming resin is selected from one of acrylic resin, polyurethane resin and epoxy resin, the leveling agent is polyether polyester modified silicone, the coupling agent is a silane coupling agent, and the solvent is consistent with the grinding medium of the thermal sensitive intelligent control slurry.

7. The thermal-sensitive intelligent control coating according to claim 6, characterized in that: It is prepared by the following method: weigh the content described in claim 6, mix the leveling agent, coupling agent, film-forming resin and solvent evenly to form a solution, gradually add the thermal intelligent control slurry into the solution, stir at 1000-1500r / min for 1-2h, pass through a 200-mesh sieve, and obtain a thermal intelligent control coating.

Citation Information

Patent Citations

  • A thermally insulating polyethylene glycol-based polyurethane / tungsten-doped vanadium dioxide composite phase change coating, its preparation method, and its application.

    CN114621668B

  • High-light-reflection phase-change heat storage coating for textiles and preparation method of high-light-reflection phase-change heat storage coating

    CN114775296A

  • Method for preparing hypovanadic oxide doped powder material

    CN101481142A

  • Titanium dioxide and M-phase vanadium dioxide composite nanoparticle and preparation method thereof

    CN104045345A

  • Method for preparing molybdenum doped titanium dioxide film by virtue of sol-gel method