Digital ink composition, ceramic tile with mold effect and preparation method thereof
By using specific digital ink and water-based glaze slurry to repel the problem of unnatural transition between the three-dimensional texture effect of ceramic tile and the surrounding area, the high simulation, low cost and easy-to-preparation mold effect of ceramic tile is achieved.
Patent Information
- Application Number
- CN202411149683.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-21
AI Technical Summary
When existing ceramic tiles achieve three-dimensional concave and convex texture effect, the depressions and protrusions on the surface are difficult to naturally transition with the surrounding area. The color and gloss of the pattern after firing are inconsistent with the surrounding area, making it difficult to obtain high-simulation digital with low cost and easy to control production. Mold effect.
Two specific digital inks (first ink and second ink) are used to print the mold texture, and use their repulsion with the aqueous glaze slurry to form a more three-dimensional, profound and clear mold effect, which can form dots and lines. The texture is made of concave and convex texture, matching different color patterns, and there is no need to convert press-shaped molds, which is low cost and simple in preparation process.
The recesses and protrusions on the surface of the ceramic tile are naturally transitioned to the surrounding area, and the pattern color and gloss are consistent with the surrounding area. The mold effect is more realistic, with good texture, low cost and high preparation efficiency, which is suitable for modern automation and intelligent manufacturing.
Smart Images

Figure CN118755310B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building ceramic tiles, and in particular relates to a digital ink composition, a ceramic tile with a mold effect and a preparation method thereof. Background Art
[0002] The popular decorative rock slab products on the market generally use glaze changes to achieve decorative purposes. The following processes are usually used to form a concave and convex texture effect:
[0003] 1. Use a pressing mold to press a concave-convex texture effect on the surface of the tile blank. This method has the following shortcomings: (1) Each concave-convex texture requires a physical mold, which is not flexible enough; (2) The mold will exert pressure on the tile blank, and it is difficult to use this method to achieve a concave-convex texture on the surface of the ceramic slab and rock slab products that have been popular in the past two years; (3) The mold cannot press a very fine texture, which easily leads to loss of details; (4) The concave-convex texture on the surface of the tile blank will change with the physical wear of the mold, making it difficult to ensure batch stability.
[0004] 2. Applying a binder to adhere the frit dry particles on the surface of the brick to achieve a concave-convex texture effect. This method applies a binder and adheres the frit particles at specific positions on the brick, blows away the unbonded frit particles on the surface of the brick, and obtains a ceramic tile with a concave-convex texture on the surface after firing. This method has the following shortcomings: (1) In order to ensure the normal flow of the dry particles, the size of the dry particles is generally large, so it is impossible to obtain very narrow raised lines; (2) After firing, the glaze composition at the raised part and the glaze composition at the flat part are quite different, resulting in a large change in the color of the ink and the gloss of the glaze surface at the raised part and the surrounding flat part. The color and gloss transition of the pattern texture is abrupt, and the texture is reduced, and it is impossible to achieve a realistic imitation of stone, wood, cloth, leather and other surface effects.
[0005] 3. Use sinking and fine carving ink to etch a concave and convex texture effect on the surface of the tile. This method has the following shortcomings: (1) The sunken line texture formed by this method is completely formed by the melting, volatilization and corrosion of low-temperature materials at high temperatures, so the texture formed collapses and is not three-dimensional and sharp enough; (2) Because the corrosive agents used in sinking and fine carving inks are mostly vanadium compounds, when the corrosive agent content is high, there is often yellow residue on the lines after firing, which affects the color of the pattern texture; (3) Because the glaze composition of the sunken strips is greatly different from that of the surrounding areas, the color and gloss of the lines after firing are difficult to keep consistent with the surrounding areas, the color and gloss transition of the pattern texture is abrupt, the texture is reduced, and it is impossible to achieve realistic imitation stone, wood, cloth, leather and other effects.
[0006] 4. Use oily molds, fine carving, and deep effect inks to glaze the surface of the tile to form a concave and convex texture effect. The technical features disclosed in Publication No. CN109574711A are that the texture effect is formed on the surface of the tile by the repulsion of oily ceramic ink and water-based glaze slurry. This method has the following improvements: (1) When a wider line texture is required, if the performance of the oily effect ink is not properly matched, glaze beads will often appear in the grooves, affecting the beauty of the lines; (2) Where the glaze mold ink is sprayed, the concave effect formed by the glaze on the upper layer being pushed away causes a significant difference in the glaze composition here and the surrounding area. The color and gloss of the pattern after firing are difficult to keep consistent with the surrounding area, resulting in a large difference in the color and gloss of the pattern in the same area. The texture is reduced and it is impossible to achieve realistic imitation of stone, wood grain, fabric, leather and other materials.
[0007] To sum up, when existing ceramic tiles achieve a three-dimensional concave-convex texture effect, the depressions and protrusions on the surface are difficult to transition naturally with the surrounding areas, and the color and glossiness of the pattern after firing cannot be consistent with the surrounding area. Based on the existing technology, it is still difficult to obtain high-simulation digital mold effect ceramic tiles with good effects, low costs, and easy production control. Summary of the invention
[0008] In view of the problems existing in the prior art, the present invention aims to provide a digital ink composition, a ceramic tile with a mold effect and a preparation method thereof, so as to make the depressions and protrusions on the surface of the ceramic tile transition naturally with the surrounding area, the color and glossiness of the pattern can be consistent with the surrounding area, the mold effect is more three-dimensional, deep, clear, realistic and textured, the concave and convex layered mold effect is more varied, there is no need to open the mold and convert the special-shaped mold of the press, the cost is low, the preparation process is simple, the efficiency is high and the range of use is wide.
[0009] Based on the above purpose, the technical solution adopted by the present invention is as follows:
[0010] In a first aspect, the present invention provides a digital ink composition, comprising a first ink and a second ink,
[0011] The first ink comprises the following components in weight percentage: 20%-30% of the first barium frit, 3%-10% of the bright frit, 4%-10% of zinc vanadate, 55%-70% of the organic solvent, and 3%-8% of the dispersant, wherein the first barium frit comprises the following components in weight percentage: SiO2 42%-47%, Al2O3 14%-18%, CaO 3%-5%, Na2O 2%-4%, K2O 4%-7%, and BaO 14%-18%, and the bright frit comprises the following components in weight percentage: SiO2 58%-63%, Al2O3 15%-22%, CaO 2%-4%, Na2O 2%-6%, K2O 2%-4%, and Bi2O3 4%-9%;
[0012] The second ink contains the following components in weight percentage: 30%-45% of a second barium frit, 2%-10% of a matte frit, 1%-6% of zinc vanadate, 50%-60% of an organic solvent, and 2%-5% of a dispersant, wherein the second barium frit contains the following components in weight percentage: SiO2 40%~45%, Al2O3 16%~20%, CaO 1%~3%, Na2O 3%~7%, K2O 0.5%~3%, and BaO 16%~20%, and the matte frit contains the following components in weight percentage: SiO2 45%~55%, Al2O3 20%~23%, CaO 15%~25%, Na2O 3%~5%, K2O 2%~5%, and ZnO 5%~8%.
[0013] The first ink and the second ink are oily, and there is a repulsive effect between them and the water-based glaze slurry, so that a concave-convex texture can be formed. When the two inks are used to print the mold texture at the same time, the two inks will synergistically repel the water-based glaze slurry, making the mold effect formed more three-dimensional, profound, clear, realistic and textured, and can not only form dot-shaped concave-convex textures, but also linear concave-convex textures, with a stronger ability to match different color patterns, and without the need to convert the press special-shaped mold, ceramic tiles with concave-convex effects of various styles can be produced, and even different concave-convex textures can be achieved, and the concave-convex layered mold effect changes are richer, so that the natural effect of simulated stone can be achieved well; at the same time, there is no need to open the mold and convert the press special-shaped mold, the cost is lower, the preparation process is simple, the efficiency is high, and the scope of use is wide, which is in line with the development direction of modern automated intelligent manufacturing.
[0014] Preferably, the organic solvent in the first ink is isooctyl laurate, and the organic solvent in the second ink is methyl laurate. Preferably, the dispersants in the first ink and the second ink are independently polyester dispersants. More preferably, the dispersant in the first ink is Huihong HP1064; and the dispersant in the second ink is Lamberti FLUIJET628.
[0015] Preferably, the first ink is the digital ink N00520 of Tao Lixi Company; the second ink is the white digital ink S015 of Shuntong New Materials Company. When these two inks are used at the same time, the three-dimensionality and clarity of the mold effect are better.
[0016] In a second aspect, the present invention provides a ceramic tile with a mold effect, which includes a body, a bottom glaze layer, a surface glaze layer, a pattern layer and a protective glaze layer from top to bottom. The surface of the ceramic tile has a concave-convex texture, and the concave-convex texture is formed using the digital ink composition.
[0017] The ceramic tile utilizes a first ink and a second ink of a specific formula to print a mold texture. Because the first ink and the second ink will synergistically repel the aqueous glaze slurry, the mold effect formed is more three-dimensional, profound, clear, realistic, and textured. Not only can it form a dot-like concave-convex texture, but it can also form a linear concave-convex texture, and its ability to match different color patterns is stronger.
[0018] The ceramic tile has a better digital engraving effect than a real mold effect, and has a finer texture. Moreover, there is no need to convert the special-shaped mold of the press, so that ceramic tiles with various styles of concave and convex effects can be produced, and even the concave and convex textures of each piece can be different. The concave and convex layered mold effect is more varied, so that the natural effect of simulated stone can be well achieved. At the same time, there is no need to open the mold and convert the special-shaped mold of the press, and the mold texture and fineness can be adjusted at any time, the cost is lower, the preparation process is simple, the efficiency is high, and the scope of use is wide, which is in line with the development direction of modern automated intelligent manufacturing.
[0019] Preferably, the surface glaze layer comprises the following components in weight percentage: SiO2 49%~54%, TiO2 0.08%~0.25%, Al2O3 18%~23%, Fe2O3 0.1%~0.3%, Mn3O4 0.01%~0.02%, MgO 0.2~1.5%, CaO 0.8%~2.5%, Na2O 3.5%~5.5%, K2O 2.5%~4.5%, V2O5 0.01%~0.02%, ZrO2 4%~7%, HfO2 0.1%~0.2%, BaO 2.5%~4%, P2O5 0.1%~0.3%, SrO 0.1%~0.5%, ZnO 0.5%~2%, SO3 0.01%~0.05%, ignition loss 4.5%~7%;
[0020] The protective glaze layer comprises the following components in weight percentage: SiO2 48%~52%, TiO2 0.03%~0.15%, Al2O3 14%~18%, Fe2O3 0.1%~0.2%, MgO 1~2.5%, CaO 4.5%~6.5%, Na2O 2%~4%, K2O 2.5%~4.5%, V2O5 0.03%~0.08%, ZrO2 0.2%~0.8%, HfO2 0.01%~0.02%, BaO 5.5%~8%, P2O5 0.1%~0.2%, SrO 3.5%~5.5%, ZnO 3.5%~6%, SO3 0.01%~0.05%, and ignition loss 2.5%~4.5%.
[0021] The use of the above-mentioned specific glaze formula makes the digital ink and the glaze more matched and the combination effect better, thereby making the mold effect better; the use of the above-mentioned protective glaze with a specific chemical composition makes the hand feel more delicate and the eye protection effect is better; at the same time, the use of the above-mentioned specific glaze formula and protective glaze also ensures that the ceramic tiles have a good sintering effect, the surface depressions and protrusions have a natural transition with the surrounding areas, the pattern color and glossiness can be consistent with the surrounding area, the mold effect is more realistic, not irritating, and the stain resistance, anti-slip, wear resistance, color development, flexural strength and other properties are also better.
[0022] Preferably, the raw materials of the surface glaze layer include the following components in parts by weight: 9-11 parts of aluminum oxide, 2.5-4.5 parts of barium carbonate, 28-32 parts of potassium feldspar, 28-32 parts of sodium feldspar, 0-2 parts of dolomite, 8-12 parts of nepheline, 12.5-16.5 parts of quartz, and 0.5-2 parts of zinc oxide. In some embodiments, when preparing the surface glaze layer, water, a suspending agent, and a water reducing agent are also added. Based on the total weight of the raw materials of the surface glaze layer, the weight of water is 35%-40%, the weight of the suspending agent is 0.1%-0.2%, and the weight of the water reducing agent is 0.2%-0.3%. Exemplarily, the suspending agent is sodium methylcellulose; the water reducing agent is sodium tripolyphosphate.
[0023] Preferably, the raw materials of the protective glaze layer include the following components in parts by weight: 9-11 parts of aluminum oxide, 2.5-4.5 parts of barium carbonate, 28-32 parts of potassium feldspar, 28-32 parts of sodium feldspar, 0-2 parts of dolomite, 8-12 parts of nepheline, 12.5-16.5 parts of quartz, and 0.5-2 parts of zinc oxide. In some embodiments, when preparing the protective glaze layer, water, a suspending agent, and a water reducing agent are also added. Based on the total weight of the raw materials for the protective glaze layer, the weight of water is 35%-45%, the weight of the suspending agent is 0.1%-0.2%, and the weight of the water reducing agent is 0.2%-0.4%. Exemplarily, the suspending agent is sodium methylcellulose; the water reducing agent is sodium tripolyphosphate.
[0024] Preferably, the green body contains the following chemical components in weight percentage: SiO2 64.5%~68.5%, Al2O3 16.4%~20.4%, K2O 2.12%~4.12%, Na2O 1.28%~3.28%, CaO 0.82%~2.82%, MgO 0.1%~2.1%, Fe2O3 1.0%~2.0%, TiO2 0.1%~0.5%, and the rest are loss on ignition and impurities.
[0025] Preferably, the base glaze layer contains the following chemical components in weight percentage: SiO2 60%~62%, TiO2 0.05%~0.15%, Al2O3 18%~22%, Fe2O3 0.1%~0.2%, Mn3O4 0.01%~0.02%, MgO 2.5%~3.5%, CaO 2%~3%, Na2O2.5%~4.5%, K2O 0.5%~1.5%, V2O5 0.01%~0.02%, NiO 0.01%~0.02%, ZrO2 5%~7%, HfO2 0.1%~0.2%, BaO 0.01%~0.02%, P2O5 0.1%~0.3%, and ignition loss 1.0%~3.5%. When the base glaze layer contains the above-mentioned specific content of chemical components, it not only has a higher initial melting temperature and a wider firing range, but also has a good expansion coefficient matching with the body, the top glaze and the transparent glaze, and has a higher whiteness and a stronger covering ability. It can better cover the defects on the body, improve the surface flatness of the product, and make the pattern display clearer and the details more perfect. More preferably, the raw materials of the base glaze layer include the following components in parts by weight: 6 to 14 parts of air knife clay, 12 to 18 parts of calcined kaolin, 17 to 23 parts of potassium feldspar, 24 to 32 parts of sodium feldspar, 4 to 8 parts of burned talc, 3 to 5 parts of wollastonite, 6 to 10 parts of quartz, and 8 to 13 parts of zirconium silicate. Among them, the weight proportion of sodium feldspar in the base glaze raw materials is preferably 24% to 32%. In some embodiments, water, a suspending agent and a water reducing agent are added when preparing the base glaze layer. Based on the total weight of the base glaze layer raw materials, the weight of water is 35%-45%, the weight of the suspending agent is 0.1%-0.2%, and the weight of the water reducing agent is 0.2%-0.4%. Exemplarily, the suspending agent is sodium methylcellulose; the water reducing agent is sodium tripolyphosphate.
[0026] In this application, the raw materials of the base glaze, the top glaze and the protective glaze refer to the minerals or rocks used to make the corresponding glazes, excluding the processing aids used.
[0027] In a third aspect, the present invention provides a method for preparing the ceramic tile with a mold effect, comprising the following steps:
[0028] The green body is prepared by using green body raw materials, and then the base glaze is applied, the first ink and the second ink are simultaneously sprayed according to the mold pattern, dried, sprayed with the surface glaze, printed with the color pattern, dried, sprayed with the protective glaze, fired, polished, and edged to obtain a ceramic tile with a mold effect.
[0029] When the first ink is printed, the grayscale is set to 0.8%~46%;
[0030] When printing the second ink, the grayscale is set to 1%~15%.
[0031] The grayscale when printing the first ink and the second ink will affect the ink discharge stability, the naturalness of the mold contour, etc. By controlling the grayscale when printing the first ink and the second ink within the above-mentioned specific range, the ink discharge stability is ensured, the local mold texture is avoided to be too dark or too shallow, and the mold contour is natural.
[0032] Compared with printing mold ink after spraying the surface glaze, printing mold ink before spraying the surface glaze has a deeper mold effect. In addition to being able to form dot-shaped concave-convex textures, it can also form linear concave-convex textures. This is because the interaction between mold ink and surface glaze slurry is stronger than the interaction between mold ink and protective glaze slurry.
[0033] Preferably, the polishing step includes: using 8 groups of 600-mesh corundum resin half-section elastic modules for rough polishing for 30s-60s, 6 groups of 800-mesh corundum resin half-section elastic modules for rough polishing for 35s-50s, 8 groups of 240-mesh fiber modules for fine polishing for 30s-55s, and 5 groups of 240-mesh plastic silicon carbide grinding brushes for fine polishing for 25s-40s at 1.0MPa-3.0MPa. The above-mentioned specific polishing process can make the mold glaze effect more smooth and natural.
[0034] Preferably, the step of preparing the green body using the green body raw material comprises: ball milling the green body slurry, spray drying, screening, grading, pressing and molding, and drying to obtain the green body.
[0035] Preferably, the fineness of the slurry after ball milling satisfies 250-mesh sieve residue of 0.8 wt.% to 1.2 wt.%.
[0036] Preferably, the gradation satisfies: calculated based on the total weight of the graded raw materials, 330 mesh is 1% to 4%, 40 mesh is 25% to 32%, 60 mesh is 65% to 72%, and 100 mesh is 2% to 4%.
[0037] Preferably, when applying the base glaze, the base glaze slurry used meets the following requirements: 325 mesh residue is 0.6wt.%-0.8wt.%, specific gravity is 1.88-1.92g / mL, and flow rate is 33-38s / 100mL.
[0038] Preferably, the base glaze application amount is 350g / m 2 -450g / m 2 .
[0039] Preferably, the first ink and the second ink are each independently ejected in an amount of 2 to 50 g / m 2 .
[0040] Preferably, the temperature of the first drying is 60-120° C., and the time of the first drying is 1-3 minutes. After spraying the mold ink, the first drying can avoid the mold ink and the glaze slurry from being too repellent, which may cause glaze shrinkage. However, after the first drying, the organic solvent in the mold ink is not completely removed.
[0041] Preferably, when spraying the glaze, the glaze slurry used meets the following requirements: the residue on a 325-mesh sieve is 0.4wt.%-0.7wt.%, the specific gravity is 1.45-1.47g / mL, and the flow rate is 32-42s / 100mL.
[0042] Preferably, the glaze spraying amount is 500-850 g / m 2 .
[0043] Preferably, the temperature of the second drying is 60-120° C., and the time of the second drying is 1-3 min.
[0044] Herein, the definition of "first time" in "first drying" and the definition of "second time" in "second drying" are only used to distinguish between the two dryings.
[0045] Preferably, when spraying the protective glaze, the protective glaze slurry satisfies: the residue on a 325-mesh sieve is 0.4wt.%-0.8wt.%, the specific gravity is 1.45-1.55 g / mL, and the flow rate is 28-35s / 100mL.
[0046] Preferably, the amount of protective glaze sprayed is 200-400 g / m 2 .
[0047] Preferably, the maximum sintering temperature is 1180-1210°C.
[0048] In a second aspect, the present invention also provides a ceramic tile with a mold effect obtained by the preparation method.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] (1) The present invention uses two specific inks to print mold textures, so as to utilize the synergistic effect of the two inks to repel the water-based glaze slurry, so that the mold effect formed is more three-dimensional, profound, clear, realistic and textured. It can not only form dot-shaped concave-convex textures, but also line-shaped concave-convex textures, and has a stronger ability to match different color patterns.
[0051] (2) The present invention can produce ceramic tiles with various styles of concave-convex effects without the need to convert the special-shaped molds of the press, and can even achieve different concave-convex textures on each piece, and the concave-convex layered mold effects are more varied, thereby achieving a good natural effect of simulated stone; at the same time, there is no need to open molds and convert special-shaped molds of the press, the cost is lower, the preparation process is simple, the efficiency is high, and the application range is wide, which is in line with the development direction of modern automated intelligent manufacturing.
[0052] (3) The present invention adopts a glaze with a specific chemical composition to make the digital ink and the glaze more matched and the combination effect better, thereby making the mold effect better; the protective glaze with a specific chemical composition is adopted to make the hand feel more delicate and the eye protection effect better; the use of the above-mentioned specific glaze and protective glaze at the same time also ensures that the ceramic tiles have a good sintering effect, the surface depressions and protrusions have a natural transition with the surrounding areas, the pattern color and glossiness can be consistent with the surrounding area, the mold effect is more realistic, not irritating, and the stain resistance, anti-slip, wear resistance, color development, flexural strength and other properties are also better. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 This is a photo of the ceramic tile after spraying glaze during the preparation process of Example 1;
[0054] Figure 2 This is a photo of the ceramic tile after spraying protective glaze during the preparation process of Example 1;
[0055] Figure 3 This is a photo of the ceramic tile product of Example 1;
[0056] Figure 4 This is a photo of the ceramic tile product of Comparative Example 1;
[0057] Figure 5 This is a photo of the ceramic tile product of Comparative Example 2;
[0058] Figure 6 This is a photo of the ceramic tile product of Comparative Example 3;
[0059] Figure 7 This is a photo of the ceramic tile product of Comparative Example 4;
[0060] Figure 8 This is a photo of the ceramic tile product of Comparative Example 5;
[0061] Fig. 9 This is a photo of the ceramic tile product of Comparative Example 6;
[0062] Fig.10 This is a photo of the ceramic tile product of Comparative Example 7;
[0063] Fig.11 This is a photo of the ceramic tile product of Comparative Example 8;
[0064] Fig.12This is a photo of the ceramic tile product of Comparative Example 9;
[0065] Fig.13 This is a photo of the ceramic tile product of Comparative Example 15. DETAILED DESCRIPTION
[0066] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0067] Unless otherwise specified, the experimental methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.
[0068] Tao Lisi's digital ink N00520 contains the following components in weight percentage: first barium frit 20%-30%, bright frit 3%-10%, zinc vanadate 4%-10%, isooctyl laurate 55%-70%, polyester dispersant 3%-8%, wherein the first barium frit contains the following components in weight percentage: SiO2 42%~47%, Al2O3 14%~18%, CaO 3%~5%, Na2O 2%~4%, K2O 4%~7%, BaO 14%~18%, bright frit contains the following components in weight percentage: SiO2 58%~63%, Al2O3 15%~22%, CaO 2%~4%, Na2O 2%~6%, K2O 2%~4%, Bi2O3 4%~9%.
[0069] The white digital ink S015 of Shuntong New Materials Company contains the following components in weight percentage: second barium frit 30%-45%, matte frit 2%-10%, zinc vanadate 1%-6%, methyl laurate 50%-60%, polyester dispersant 2%-5%, wherein the second barium frit contains the following components in weight percentage: SiO2 40%~45%, Al2O3 16%~20%, CaO 1%~3%, Na2O 3%~7%, K2O 0.5%~3%, BaO 16%~20%, the matte frit contains the following components in weight percentage: SiO2 45%~55%, Al2O3 20%~23%, CaO 15%~25%, Na2O 3%~5%, K2O 2%~5%, ZnO 5%~8%.
[0070] Example 1
[0071] This embodiment provides a ceramic tile with a mold effect, and the preparation method thereof comprises the following steps:
[0072] (1) The raw materials for the green body were weighed and mixed according to the following weight formula: 17 parts of sand paste, 7 parts of bentonite, 20.2 parts of mixed mud, 14 parts of sodium stone powder, 40 parts of diopside, 3.2 parts of magnesia clay, 15 parts of environmentally friendly mud, 1.5 parts of waste brick particles, 13 parts of potassium sodium stone powder, 17 parts of sodium stone powder, 4 parts of antique mud, 0.367 parts of J028 debonding agent (Foshan Sanshui Taiyang New Materials Co., Ltd.), ball milled to a slurry fineness of 1.0 wt.% on a 250 mesh sieve, and spray dried to obtain a powder with the following chemical composition by weight percentage: SiO2 66.5%, Al2O3 18.4%, K2O 3.12%, Na2O 2.28%, CaO 1.82%, MgO 1.1%, Fe2O31.75%, TiO20.4%, and the rest are reduced and impurities, and then sieved and graded according to the following weight proportions: 30 mesh 2%, 40 mesh 28%, 60 mesh 68%, 100 mesh 2%, and then pressed and dried to obtain a first ceramic flat body;
[0073] (2) Weigh and mix the base glaze raw materials according to the following weight formula: 10 parts of air knife clay, 15 parts of calcined kaolin, 20 parts of potassium feldspar, 28 parts of sodium feldspar, 6 parts of burned talc, 3 parts of wollastonite, 8 parts of quartz, 10 parts of zirconium silicate, and add 40% of water, 0.15% of sodium methyl cellulose and 0.3% of sodium tripolyphosphate based on the total weight of the base glaze raw materials. Ball mill the slurry until the residue on a 325-mesh sieve is 0.9 wt.%, the specific gravity is 1.89 g / mL, the flow rate is 36 s / 100 mL, and the base glaze is applied on the obtained first ceramic flat body. The glaze amount is 400 g / m 2 , obtaining a second ceramic flat body, wherein the obtained base glaze comprises the following chemical components in weight percentage: SiO2 60.11%, TiO2 0.09%, Al2O3 21.80%, Fe2O3 0.16%, Mn3O4 0.01%, MgO 2.8%, CaO 2.0%, Na2O 3.95%, K2O 1.4%, V2O5 0.01%, NiO 0.01%, ZrO2 5.55%, HfO2 0.14%, BaO 0.01%, P2O5 0.15%, and ignition loss 1.81%;
[0074] (3) Designing the mold pattern through computer Photoshop software to form a mold effect texture inkjet file, and loading the file onto a ceramic inkjet machine, and loading the first ink and the second ink into the machine, wherein the first ink is the digital ink N00520 of Tao Lixi Company, and the second ink is the white digital ink S015 of Shuntong New Materials Company;
[0075] (4) The obtained second ceramic flat body is calibrated by a brick centering machine to ensure that the position of the brick is not offset during transportation, so as to achieve accurate alignment between the mold design pattern and the flat body. Then, the above-mentioned ceramic inkjet machine is used to print the mold effect ink according to the mold pattern. The grayscale of the first ink is controlled to be 30%, and the grayscale of the second ink is controlled to be 10%. Then, the third ceramic body is obtained by drying at 100°C for 2 minutes. The inkjet amount is 30g / m 2 , the viscosity of the ink is 25 ;
[0076] (5) Weigh and mix the glaze raw materials according to the following weight formula: 10 parts of aluminum oxide, 3.5 parts of barium carbonate, 30 parts of potassium feldspar, 30 parts of sodium feldspar, 1 part of dolomite, 10 parts of nepheline, 14.5 parts of quartz, and 1 part of zinc oxide. Add 36% of water, 0.13% of sodium methyl cellulose, and 0.25% of sodium tripolyphosphate based on the total weight of the glaze raw materials. Ball mill the slurry until the residue on a 325-mesh sieve is 0.7 wt.%, the specific gravity is 1.46 g / mL, the flow rate is 36 s / 100 mL, and spray the glaze on the obtained third ceramic body. The glaze amount is 700 g / m 2 , obtaining a fourth ceramic body, wherein the obtained glaze comprises the following chemical components in weight percentage: SiO2 51.67%, TiO2 0.14%, Al2O3 21.29%, Fe2O3 0.27%, Mn3O4 0.01%, MgO 0.83%, CaO 1.55%, Na2O 4.61%, K2O 3.55%, V2O5 0.02%, ZrO2 5.4%, HfO2 0.11%, BaO 3.16%, P2O5 0.2%, SrO 0.22%, ZnO 1.06%, SO3 0.03%, and loss on ignition 5.88%;
[0077] (6) calibrating the fourth ceramic body obtained by a brick centering machine to ensure that the position of the brick is not offset during transportation, and printing a color pattern to obtain a fifth ceramic body;
[0078] (7) Weigh and mix the protective glaze raw materials according to the following weight formula: 4 parts of aluminum oxide, 6.5 parts of barium carbonate, 35 parts of potassium feldspar, 35 parts of sodium feldspar, 5.5 parts of calcite, 2 parts of talc, 3 parts of quartz, 4.5 parts of zinc oxide, 4 parts of strontium carbonate, and 0.5 parts of zirconium silicate. Add 38% of water, 0.15% of sodium methyl cellulose, and 0.28% of sodium tripolyphosphate based on the total weight of the protective glaze raw materials, and ball mill until the slurry has a 325-mesh sieve residue of 0.65 wt.%, a specific gravity of 1.46 g / mL, and a flow rate of 30 s / 100 mL. Spray the protective glaze on the obtained fifth ceramic body at a glaze amount of 300 g / m 2, obtaining a sixth ceramic body, wherein the protective glaze comprises the following chemical components in weight percentage: SiO2 50.27%, TiO2 0.06%, Al2O3 16.84%, Fe2O3 0.16%, MgO 1.9%, CaO 5.4%, Na2O 2.70%, K2O 3.28%, V2O5 0.05%, ZrO2 0.43%, HfO2 0.01%, BaO 6.54%, P2O5 0.11%, SrO 4.12%, ZnO 4.69%, SO3 0.02%, and ignition loss 3.42%;
[0079] (8) The sixth ceramic body is sent to a roller kiln with a maximum firing temperature of 1210°C for firing. The fired ceramic tile semi-finished product is firstly rough-polished for 50 seconds using 8 groups of 600-mesh corundum resin half-elastic modules and 40 seconds using 6 groups of 800-mesh corundum resin half-elastic modules under a pressure of 1.5 MPa, and then fine-polished for 50 seconds using 8 groups of 240-mesh fiber modules and 30 seconds using 5 groups of 240-mesh plastic silicon carbide grinding brushes, and then edge-polished to obtain a ceramic tile with a mold effect.
[0080] Example 2
[0081] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that when printing the mold effect ink, the grayscale value of the digital ink N00520 of Tao Lixi Company is controlled to be 1%.
[0082] Example 3
[0083] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that when printing the mold effect ink, the grayscale value of the digital ink N00520 of Tao Lixi Company is controlled to be 45%.
[0084] Example 4
[0085] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that when printing the mold effect ink, the gray value of the white digital ink S015 of Shuntong New Materials Company is controlled to be 1%.
[0086] Example 5
[0087] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that when printing the mold effect ink, the grayscale value of the white digital ink S015 of Shuntong New Materials Company is controlled to be 15%.
[0088] Example 6
[0089] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that when printing the mold effect ink, the grayscale value of Tao Lisi's digital ink N00520 is controlled to 10%, and the grayscale value of Shuntong New Materials' white digital ink S015 is controlled to 10%.
[0090] Example 7
[0091] This embodiment provides a ceramic tile with a mold effect, which is different from the embodiment 1 in that the base glaze raw material formula is different and the chemical composition of the base glaze obtained is different, as follows:
[0092] The base glaze raw materials are as follows by weight: 6 parts of air knife clay, 12 parts of calcined kaolin, 17 parts of potassium feldspar, 32 parts of sodium feldspar, 4 parts of burned talc, 3 parts of wollastonite, 6 parts of quartz, and 8 parts of zirconium silicate;
[0093] The obtained base glaze contains the following chemical components in weight percentage: SiO2 61.86%, TiO2 0.05%, Al2O3 19%, Fe2O3 0.1%, Mn3O4 0.02%, MgO 2.5%, CaO 2.7%, Na2O 4.2%, K2O 1.0%, V2O5 0.01%, NiO 0.02%, ZrO2 5.3%, HfO2 0.1%, BaO 0.01%, P2O5 0.1%, and loss on ignition 3.03%.
[0094] Example 8
[0095] This embodiment provides a ceramic tile with a mold effect, which is different from the embodiment 1 in that the base glaze raw material formula is different and the chemical composition of the base glaze obtained is different, as follows:
[0096] The base glaze raw materials are as follows by weight: 14 parts of air knife clay, 18 parts of calcined kaolin, 23 parts of potassium feldspar, 24 parts of sodium feldspar, 8 parts of burned talc, 5 parts of wollastonite, 10 parts of quartz, and 13 parts of zirconium silicate;
[0097] The obtained base glaze contains the following chemical components in weight percentage: SiO2 60.1%, TiO2 0.05%, Al2O3 22.0%, Fe2O3 0.2%, Mn3O4 0.01%, MgO 2.6%, CaO 2%, Na2O 3.16%, K2O 1.6%, V2O5 0.02%, NiO 0.02%, ZrO 27%, HfO2 0.1%, BaO 0.02%, P2O5 0.1%, and loss on ignition 1.02%.
[0098] Example 9
[0099] This embodiment provides a ceramic tile with a mold effect, which is different from the embodiment 1 in that the glaze raw material formula is different and the chemical composition of the obtained glaze is different, as follows:
[0100] The glaze raw materials are as follows by weight: 9 parts of aluminum oxide, 2.5 parts of barium carbonate, 28 parts of potassium feldspar, 30 parts of sodium feldspar, 0 parts of dolomite, 8 parts of nepheline, 12.5 parts of quartz, and 0.5 parts of zinc oxide;
[0101] The obtained glaze contains the following chemical components in weight percentage: SiO2 53.8%, TiO2 0.22%, Al2O3 18.5%, Fe2O3 0.2%, Mn3O4 0.02%, MgO 0.8%, CaO 1.5%, Na2 5.0%, K2O 3.4%, V2O5 0.01%, ZrO2 5.5%, HfO2 0.11%, BaO 3.0%, P2O5 0.12%, SrO 0.2%, ZnO 1.0%, SO3 0.02%, and loss on ignition 6.6%.
[0102] Example 10
[0103] This embodiment provides a ceramic tile with a mold effect, which is different from the embodiment 1 in that the glaze raw material formula is different and the chemical composition of the obtained glaze is different, as follows:
[0104] By weight, the glaze raw materials are as follows: 11 parts of aluminum oxide, 4.5 parts of barium carbonate, 32 parts of potassium feldspar, 28 parts of sodium feldspar, 2 parts of dolomite, 12 parts of nepheline, 16.5 parts of quartz, and 2 parts of zinc oxide;
[0105] The obtained glaze contains the following chemical components in weight percentage: SiO2 51.48%, TiO2 0.11%, Al2O3 23%, Fe2O3 0.1%, Mn3O4 0.02%, MgO 0.8%, CaO 1.0%, Na2O 4.3%, K2O 3.7%, V2O5 0.01%, ZrO 24%, HfO2 0.2%, BaO 3.8%, P2O5 0.2%, SrO 0.4%, ZnO 2%, SO3 0.02%, and loss on ignition 4.86%.
[0106] Embodiment 11
[0107] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that the protective glaze raw material formula is different and the chemical composition of the obtained protective glaze is different, as follows:
[0108] The protective glaze raw materials are as follows by weight: 3 parts of aluminum oxide, 5.5 parts of barium carbonate, 30 parts of potassium feldspar, 40 parts of sodium feldspar, 5 parts of calcite, 1 part of talc, 2 parts of quartz, 3.5 parts of zinc oxide, 3 parts of strontium carbonate, and 0.3 parts of zirconium silicate;
[0109] The obtained protective glaze contains the following chemical components in weight percentage: SiO2 52%, TiO2 0.11%, Al2O3 14.5%, Fe2O3 0.2%, MgO 1.2%, CaO 5.5%, Na2O 4.0%, K2O 3.0%, V2O5 0.04%, ZrO2 0.6%, HfO2 0.01%, BaO 6.0%, P2O5 0.2%, SrO 4.0%, ZnO 4.3%, SO3 0.01%, and loss on ignition 4.33%.
[0110] Example 12
[0111] This embodiment provides a ceramic tile with a mold effect, which is different from Embodiment 1 in that the protective glaze raw material formula is different and the chemical composition of the obtained protective glaze is different, as follows:
[0112] The protective glaze raw materials are as follows by weight: 5 parts of aluminum oxide, 7.5 parts of barium carbonate, 40 parts of potassium feldspar, 30 parts of sodium feldspar, 6 parts of calcite, 3 parts of talc, 4 parts of quartz, 5.5 parts of zinc oxide, 5 parts of strontium carbonate, and 1.5 parts of zirconium silicate;
[0113] The obtained protective glaze contains the following chemical components in weight percentage: SiO2 50%, TiO2 0.11%, Al2O3 17.5%, Fe2O3 0.1%, MgO 1.0%, CaO 6.0%, Na2O 2.5%, K2O 3.6%, V2O5 0.05%, ZrO2 0.3%, HfO2 0.01%, BaO 5.5%, P2O5 0.2%, SrO 5.0%, ZnO 5.0%, SO3 0.01%, and loss on ignition 3.12%.
[0114] Embodiment 13
[0115] This embodiment provides a ceramic tile with a mold effect, which is different from the embodiment 1 in that the green body raw material formula is different and the chemical composition of the green body obtained is different, as follows:
[0116] The raw materials of the green body are as follows by weight: 23.9 parts of DY107 potassium sodium sand, 4.1 parts of PS441 sodium sand, 4.1 parts of PS434 sodium sand, 18 parts of PS118 potassium sodium stone powder; 8.1 parts of DY139 potassium sand, 5.3 parts of DY340 wollastonite, 1.5 parts of DY339 bentonite, 0.5 parts of DY311 raw bauxite, 5 parts of DY203 black mud, 22.5 parts of DY214 mud paste, 3 parts of DY335 bentonite, 4.5 parts of DY302 talc, 5.5 parts of GF02 ordinary white mud powder, 5 parts of pressed mud, 0.37 parts of HF023 degumming agent, 0.98 parts of HF017 water glass, and 0.12 parts of HF035 deflocculating agent;
[0117] The obtained green body contains the following chemical components in weight percentage: SiO2 66.67%, Al2O3 18.67%, K2O 3.2%, Na2O 1.41%, CaO 1.98%, MgO 1.46%, Fe2O3 1.16%, TiO2 0.17%, and the rest are loss on ignition and impurities.
[0118] Embodiment 14
[0119] This embodiment provides a ceramic tile with a mold effect, which is different from the embodiment 1 in that the green body raw material formula is different and the chemical composition of the green body obtained is different, as follows:
[0120] In parts by weight, the raw materials for the green body are as follows: 17 parts of sand paste, 7 parts of bentonite, 20 parts of mixed mud, 14.5 parts of sodium stone powder, 40 parts of diopside, 3.4 parts of magnesia clay, 15 parts of environmentally friendly mud, 1.5 parts of waste brick particles, 13 parts of potassium sodium stone powder, 16.5 parts of sodium stone powder, 5 parts of antique mud, and 0.367 parts of J028 degumming agent.
[0121] The obtained green body contains the following chemical components in weight percentage: SiO2 67.97%, Al2O3 18.46%, K2O 2.34%, Na2O 2.1%, CaO 0.85%, MgO 1.38%, Fe2O3 1.74, TiO2 0.27%, and the rest are loss on ignition and impurities.
[0122] Embodiment 15
[0123] The present embodiment provides a ceramic tile with a mold effect, which differs from Embodiment 1 in that the polishing treatment is different, specifically as follows: at 1.0 MPa, first use 8 groups of 600-mesh corundum resin half-elastic modules for rough polishing for 55 seconds and 6 groups of 800-mesh corundum resin half-elastic modules for rough polishing for 45 seconds, then use 8 groups of 240-mesh fiber modules for fine polishing for 50 seconds and 5 groups of 240-mesh plastic silicon carbide grinding brushes for fine polishing for 35 seconds.
[0124] Example 16
[0125] The present embodiment provides a ceramic tile with a mold effect, which differs from Embodiment 1 in that the polishing treatment is different, specifically as follows: at 3.0 MPa, first use 8 groups of 600-mesh corundum resin half-cut elastic modules for rough polishing for 35 seconds and 6 groups of 800-mesh corundum resin half-cut elastic modules for rough polishing for 40 seconds, then use 8 groups of 240-mesh fiber modules for fine polishing for 35 seconds and 5 groups of 240-mesh fiber grinding brushes for fine polishing for 30 seconds.
[0126] Comparative Example 1
[0127] This comparative example provides a ceramic tile with a mold effect, and the preparation method thereof is as follows:
[0128] (1) Adding water, a suspending agent and a thickener to the green body raw material, ball milling to a slurry fineness that satisfies a 250-mesh sieve residue of 0.9 wt.%, spray drying, and obtaining a powder having the following chemical composition by weight percentage: SiO2 66.5%, Al2O3 18.4%, K2O 3.12%, Na2O 2.28%, CaO 1.82%, MgO 1.1%, and the remainder being loss on ignition and impurities, and then sieving and grading according to the following weight percentages: 30 mesh 2%, 40 mesh 32%, 60 mesh 63%, 100 mesh 3%, and then pressing and molding, and drying to obtain a ceramic flat green body;
[0129] (2) Weigh and mix the base glaze raw materials according to the following weight formula: 29 parts of potassium feldspar, 19 parts of sodium feldspar, 10 parts of air knife clay, 8 parts of barium carbonate, 2 parts of calcined talc, 2 parts of wollastonite, 3 parts of calcite, 15 parts of calcined kaolin, 12 parts of zirconium silicate, and add 35% of the total weight of water, 0.1% of sodium methyl cellulose and 0.12% of sodium tripolyphosphate. Ball mill the slurry until the residue on a 325-mesh sieve is 0.7 wt.%, the specific gravity is 1.84 g / mL, the flow rate is 40 s / 100 mL, and the base glaze is applied on the obtained ceramic flat body at a glaze amount of 450 g / m 2 ;
[0130] (3) applying fine sand dry granular glaze on the surface of the base glaze layer to form a top glaze layer, wherein the fine sand dry granular glaze is composed of the following components by weight: 20 parts of fine sand dry granules, 75 parts of suspending agent, and 5 parts of protective glaze slurry;
[0131] The fine sand dry particles are composed of the following chemical components by weight percentage: SiO251.11%, Al2O319.19%, CaO9.06%, Na2O1.47%, K2O5.37%, ZrO20.03%, Fe2O30.05%, ZnO4.55%, P2O50.01%, BaO0.1%, SrO 6.56%, MgO 2.09%, TiO20.15%, CuO0.08%, HfO20.05%, ignition loss 0.13%, and the particle size of the fine sand dry particles is 320 mesh;
[0132] The protective glaze slurry is composed of the following chemical components by weight percentage: SiO2 55%, Al2O3 10%, CaO 5%, Na2O3%, K2O 3%, Fe2O3 0.12%, ZnO 4%, P2O5 0.1%, BaO 5.49%, SrO 2.5%, MgO 5.5%, TiO2 0.03%, HfO2 0.06%, SO3 0.3%, ignition loss 5.9%;
[0133] The suspending agent is 9022A, which includes the following components by weight: 12 parts of acrylate polymer, 8 parts of propylene glycol block copolymer, 3 parts of surfactant, 1 part of thickener, and 7 parts of ceramic dispersant;
[0134] The specific gravity of fine sand dry granular glaze is 1.4g / mL, the flow rate is 35s / 100mL, the 325 mesh sieve residue is 1.2wt.%, and the glaze amount is 300g / m²;
[0135] (4) Firing is performed to obtain a primary finished ceramic tile, wherein the firing temperature is 1200° C. and the firing time is 50 minutes.
[0136] (5) A 2000-mesh resin grinding disc is used for micro-brush polishing for 2 minutes to obtain a finished ceramic tile, wherein the pressure of the resin grinding disc on the finished ceramic tile is 0.6 MPa.
[0137] Comparative Example 2
[0138] This comparative example provides a ceramic tile with a mold effect, and the preparation method thereof is as follows:
[0139] Prepare a ceramic body layer, specifically the same as in Example 1;
[0140] Applying a bottom glaze on the surface of the ceramic body layer to form a bottom glaze layer, the details are the same as in Example 1;
[0141] The decorative layer is printed by inkjet printing on the surface of the base glaze layer, wherein the grayscale of Dow DSI-105C, Dow DSI-MA209, Tolisi CXN40118, and Yangzi NGY82012 are 15%, 5%, 10%, and 8%, respectively.
[0142] Applying candy dry granule glaze on the surface of the decorative layer to form a surface glaze layer, wherein the candy dry granule glaze is made by mixing transparent frit and printing oil in a mass ratio of 3:1, and the particle size of the transparent frit is 120 mesh;
[0143] The finished ceramic tile is fired at 1240°C for 50 minutes.
[0144] Among them, the transparent frit particles are made of the following raw materials by weight: 40 parts of potassium feldspar, 10 parts of sodium feldspar, 8 parts of kaolin, 10 parts of barium carbonate, 8 parts of wollastonite, 6 parts of zinc oxide, 5 parts of strontium carbonate, 9 parts of calcite, 2 parts of quartz powder and 3 parts of aluminum oxide. The above raw materials are mixed and melted at 1500°C to form frits, which are then crushed to obtain the required particle size.
[0145] Comparative Example 3
[0146] This comparative example provides a ceramic tile with a mold effect, and the specific steps are as follows:
[0147] Prepare a ceramic body layer, specifically the same as in Example 1;
[0148] Applying a bottom glaze on the surface of the ceramic body layer to form a bottom glaze layer, the details are the same as in Example 1;
[0149] The decorative layer is printed by inkjet printing on the surface of the base glaze layer, wherein the grayscale of Dow DSI-105C, the grayscale of Yangzi NGY82016, the grayscale of Tao Lixi CXN40118, and the grayscale of Yangzi NGY82012 are 20%, 10%, and 10%, respectively.
[0150] Apply semi-polished dry granular glaze on the surface of the decorative layer to form a surface glaze layer, wherein the semi-polished dry granular glaze is made by mixing semi-polished dry granules with printing oil in a mass ratio of 3:7, the particle size of the semi-polished dry granules is 200 mesh, and the glaze amount of the semi-polished dry granular glaze is 450 g / m²;
[0151] The product was fired at 1230°C for 50 minutes, and then semi-polished for 2 minutes using a semi-polishing device and a 2000-mesh semi-polishing grinding block to obtain a semi-polished dry-granular ceramic tile product.
[0152] Comparative Example 4
[0153] This comparative example provides a marble effect tile, and the specific preparation method is as follows:
[0154] (1) Preparation of bottom glaze particles:
[0155] Weigh the raw materials according to the following weight percentages: 9% calcite, 11% barium carbonate, 48% potassium feldspar, 8% zinc oxide, 11% kaolin, 3% calcium borate, 1% soda ash and 9% quartz sand, mix them, add them into a furnace, calcine and melt them at 1500℃, and then flow out of the furnace and quench them with water to form bottom glaze particles;
[0156] (2) Preparation of base glaze
[0157] Weigh the raw materials according to the following weight percentages: 82% of base glaze particles, 10% of zirconium silicate, 3% of calcined kaolin and 5% of air knife clay, and mix them to obtain a base glaze;
[0158] (3) Preparation of base glaze slurry:
[0159] The raw materials were weighed according to the following weight ratio: 100 parts of base glaze, 39 parts of water, 0.15 parts of methyl cellulose and 0.35 parts of sodium tripolyphosphate, mixed, ball-milled for 10 hours, passed through a 100-mesh sieve, and the residue was measured to be 0.3 wt.%, then passed through an 80-mesh sieve and aged for 24 hours to obtain base glaze slurry;
[0160] (4) Preparation of fine dry particles:
[0161] The raw materials are weighed according to the following weight percentages: calcite 10%, barium carbonate 10%, strontium carbonate 1.5%, potassium feldspar 50%, kaolin 12%, calcium borate 3.5%, soda ash 1%, quartz sand 10% and dolomite 2%, mixed, added into a furnace and calcined and melted at 1500°C, and then flowed out of the furnace and quenched with water to form fine dry particles; wherein the fine dry particles include the following components according to weight percentage: SiO2 56.2%, Al2O3 19.86%, MgO 1.77%, CaO 10.78%, Na2O 2.08%, K2O 4.43%, SrO2 0.02% and BaO 4.86%, and the particle size of the fine dry particles is 200 meshes;
[0162] (5) Preparation of marble glaze:
[0163] Weigh the raw materials according to the following weight percentages: 87% fine dry particles, 8% calcined zinc oxide and 5% air knife soil, mix them to obtain simulated marble glaze;
[0164] (6) Preparation of marble glaze slurry:
[0165] The raw materials were weighed according to the following weight percentages: 100 parts of simulated marble glaze, 39 parts of water, 0.15 parts of methyl cellulose and 0.35 parts of sodium tripolyphosphate, mixed, ball-milled for 10 hours, passed through a 100-mesh sieve, and the residue on the sieve was measured to be 0.3wt.%, then passed through an 80-mesh sieve and aged for 24 hours to obtain a simulated marble glaze slurry; wherein the simulated marble glaze slurry includes the following components according to weight percentage: SiO2 54.8%, Al2O3 18.92%, MgO 1.84%, CaO 9.65%, Na2O 3.86%, K2O 3.21%, SrO2 0.04%, BaO 4.23%, and ZnO 3.45%;
[0166] (7) Using conventional porcelain as the ceramic body;
[0167] (8) Apply base glaze slurry on the surface of the ceramic body, wherein the glaze specific gravity is 1.85g / m 3 , flow rate 35s / 100mL, glaze volume 350g / m 2 ;
[0168] (9) Use the same inkjet printer to print ink on the surface with the base glaze slurry and print the sinking fine carving ink, where the sinking uses the Idaga CIK-RC1151 with an inkjet volume of 25%; the fine carving uses the Tao Li Xi CZN-00078 with an inkjet volume of 75%;
[0169] (10) 47 parts by weight of marble glaze slurry, 8 parts by weight of fine dry particles and 45 parts by weight of ceramic printing ink are mixed and glazed on the surface after inkjet printing, wherein the glaze specific gravity is 1.55 g / m 3, flow rate 32s / 100mL, glaze volume 600g / m 2 ;
[0170] (11) firing, wherein the firing temperature is 1220° C. and the firing period is 60 minutes;
[0171] (12) Polishing: First, use a 300-mesh diamond module to roughly polish the fired body for 1 minute, and then use a 1500-mesh resin grinding wheel to fine-polish the body for 2 minutes to obtain marble-effect tiles.
[0172] Comparative Example 5
[0173] This comparative example provides a positioning wax effect tile, and the preparation method thereof is as follows:
[0174] (1) Dry-pressing the green body powder to obtain a brick; the green body powder includes, by weight percentage, 13.5% super white sand, 2% high alumina clay, 6.7% burned talc, 6.5% pyrophyllite, 12% Sichuan potassium sodium feldspar water-abrasive, 17% Guangxi potassium sodium feldspar water-abrasive, 4.9% high sodium feldspar, 11.5% ball clay, 12.2% kaolin, 8% diopside, 5% raw ore high plasticity mud, 0.5% ceramic waste, 0.1% sodium tripolyphosphate and 0.1% sodium methyl cellulose; drying the brick in a drying kiln to form a brick layer, and the moisture content of the brick after drying is controlled within 0.35wt%;
[0175] (2) Drying the green body at 155°C for 30 minutes;
[0176] (3) Clean the surface of the blank and spray water to moisten it;
[0177] (4) applying a bottom glaze, wherein the bottom glaze slurry is made of the following raw materials by weight: 20 parts of potassium feldspar, 28 parts of sodium feldspar, 5 parts of wollastonite, 15 parts of kaolin, 10 parts of calcined kaolin, 10 parts of air knife clay, 6 parts of alumina, 5 parts of wollastonite, 6 parts of quartz, 6 parts of alumina, 0.2 parts of methyl cellulose, 0.4 parts of sodium tripolyphosphate, and 34 parts of water. The above raw materials are added into a ball mill according to the number of parts, and ball milled for 6 hours until the fineness is 0.7wt.% on a 325-mesh sieve, and the specific gravity is 1.89 g / L. When discharging the slurry, iron is removed and the slurry is passed through a 140-mesh sieve;
[0178] (5) The printer inkjet prints patterns and glue inks, wherein the pattern ink Dow DSI-105C has a grayscale of 10%, the Yangzi NGY82016 has a grayscale of 4%, the Tao Lisi CXN40118 has a grayscale of 8%, the Yangzi NGY82012 has a grayscale of 8%, and the glue ink Tao Lisi CZN00045 has a grayscale of 70%;
[0179] (6) applying protective glaze, wherein the protective glaze slurry is made of the following raw materials by weight percentage: 25 parts of potassium feldspar, 20 parts of sodium feldspar, 10 parts of calcite, 5 parts of wollastonite, 12 parts of kaolin, 4 parts of dolomite, 3 parts of aluminum oxide, 5 parts of zinc oxide, 3 parts of strontium carbonate, 8 parts of barium carbonate, 5 parts of calcined talc, 0.2 parts of methyl cellulose, 0.4 parts of sodium tripolyphosphate, and 34 parts of water. The above raw materials are added into a ball mill according to the number of parts, and ball milled for 7 hours until the fineness is 0.6wt.% on a 325-mesh sieve, and the specific gravity is 1.90 g / L. When discharging the slurry, iron is removed and the slurry is passed through a 140-mesh sieve;
[0180] (7) The printing position of glue ink reserves a position for printing bonding ink. The grayscale content of bonding ink Tao Lixi CZN000455 is 70%;
[0181] (8) Screen printing dry granular powder at the location where the bonding ink is applied in step (7), wherein the chemical composition of the dry granular powder is as follows: SiO2 54.52%, Al2O3 17.34%, Fe2O3 0.03%, MgO 1.73%, CaO 7.94%, Na2O 2.03%, K2O 4.33%, V2O5 0.01%, BaO 4.37%, SO3 0.04%, ZnO 3.61%, SrO 3.92%, PbO 0.04%, ignition loss 0.09%, and the excess dry granular powder not bonded is recovered;
[0182] (9) Firing, the temperature is controlled at 1200°C and the time is 60 minutes;
[0183] (10) Brush polishing the surface of ceramic tiles, as follows: use a 1500 mesh resin grinding wheel to rough polish the body after rough polishing for 1 minute, and then use a 3000 mesh resin grinding wheel to fine polish the body after rough polishing for 2 minutes.
[0184] Comparative Example 6
[0185] This comparative example provides a ceramic tile with a mold effect, and its preparation method is different from that of Example 1 in that when printing the mold effect ink, only the digital ink N00520 of Tao Lisi Company is used, and the grayscale value is controlled at 40%; the white digital ink S015 of Shuntong New Materials Company is not used.
[0186] Comparative Example 7
[0187] This comparative example provides a ceramic tile with a mold effect, and its preparation method is different from that of Example 1 in that when printing the mold effect ink, the grayscale value of the digital ink N00520 of Tao Lixi Company is controlled at 65%.
[0188] Comparative Example 8
[0189] This comparative example provides a ceramic tile with a mold effect, and its preparation method is different from that of Example 1 in that when printing the mold effect ink, only the white digital ink S015 of Shuntong New Materials Company is used, and the grayscale value is controlled at 40%; the digital ink N00520 of Tao Lixi Company is not used.
[0190] Comparative Example 9
[0191] This comparative example provides a ceramic tile with a mold effect, and its preparation method is different from that of Example 1 in that when printing the mold effect ink, the grayscale value of the white digital ink S015 of Shuntong New Materials Company is controlled at 30%.
[0192] Comparative Example 10
[0193] The present comparative example provides a ceramic tile with a mold effect, and the preparation method thereof is different from that of Example 1 in that the raw material formula of the glaze in step (5) is different, specifically, by weight: 5 parts of aluminum oxide, 4 parts of barium carbonate, 35 parts of potassium feldspar, 42 parts of sodium feldspar, 2.5 parts of dolomite, 6 parts of zirconium silicate, 5 parts of quartz, and 2 parts of zinc oxide; the obtained glaze contains the following chemical components in weight percentage: SiO2 53.67%, TiO2 0.14%, Al2O3 17.29%, Fe2O3 0.27%, Mn3O4 0.01%, MgO 0.83%, CaO 2.05%, Na2O 4.86%, K2O 3.8%, V2O5 0.02%, ZrO2 5.4%, HfO2 0.11%, BaO 3.66%, P2O5 0.2%, SrO 0.22%, ZnO 1.56%, SO3 0.03%, ignition reduction 5.88%.
[0194] Comparative Example 11
[0195] The present comparative example provides a ceramic tile with a mold effect, and the preparation method thereof is different from that of Example 1 in that the raw material formula of the glaze in step (5) is different, specifically, by weight: 8 parts of aluminum oxide, 2 parts of barium carbonate, 33 parts of potassium feldspar, 40 parts of sodium feldspar, 2 parts of dolomite, 7.5 parts of zirconium silicate, 4.5 parts of quartz, and 3 parts of zinc oxide; the obtained glaze contains the following chemical components in weight percentage: SiO2 50.17%, TiO2 0.14%, Al2O3 25.29%, Fe2O3 0.27%, Mn3O4 0.01%, MgO 0.83%, CaO 1.05%, Na2O 3.61%, K2O 3.05%, V2O5 0.02%, ZrO2 5.0%, HfO2 0.11%, BaO 3.06%, P2O5 0.2%, SrO 0.22%, ZnO 1.06%, SO3 0.03%, ignition reduction 5.88%.
[0196] Comparative Example 12
[0197] This comparative example provides a ceramic tile with a mold effect, and its preparation method is different from that of Example 1 in that:
[0198] The protective glaze raw materials are as follows by weight: 2.5 parts of aluminum oxide, 7.5 parts of barium carbonate, 36 parts of potassium feldspar, 32 parts of sodium feldspar, 5.0 parts of calcite, 2 parts of talc, 3.5 parts of quartz, 5.5 parts of zinc oxide, 4.5 parts of strontium carbonate, and 1.5 parts of zirconium silicate;
[0199] The obtained protective glaze contains the following chemical components in weight percentage: SiO2 53.27%, TiO2 0.03%, Al2O3 13.5%, Fe2O3 0.53%, MgO 1.0%, CaO 3.3%, Na2O 4.0%, K2O 3.5%, V2O5 0.04%, ZrO2 1.6%, HfO2 0.01%, BaO 5.8%, P2O5 0.1%, SrO 4.5%, ZnO 5.4%, SO3 0.02%, and loss on ignition 3.4%.
[0200] Comparative Example 13
[0201] This comparative example provides a ceramic tile with a mold effect, and its preparation method is different from that of Example 1 in that:
[0202] The protective glaze raw materials are as follows by weight: 6 parts of aluminum oxide, 5.6 parts of barium carbonate, 35.5 parts of potassium feldspar, 33.4 parts of sodium feldspar, 5.0 parts of calcite, 1.5 parts of talc, 2.5 parts of quartz, 5 parts of zinc oxide, 4 parts of strontium carbonate, and 1.5 parts of zirconium silicate;
[0203] The obtained protective glaze contains the following chemical components in weight percentage: SiO2 52.5%, TiO2 0.02%, Al2O3 18.95%, Fe2O3 0.05%, MgO 1.1%, CaO 3.4%, Na2O 4.0%, K2O 3.8%, V2O5 0.03%, ZrO2 2.0%, HfO2 0.01%, BaO 4.5%, P2O5 0.1%, SrO 3.0%, ZnO 5.0%, SO3 0.01%, and loss on ignition 1.53%.
[0204] Comparative Example 14
[0205] This comparative example provides a ceramic tile with a mold effect, which differs from Example 1 in that the polishing treatment is different, specifically as follows: at 3.0 MPa, first use 8 groups of 600-mesh corundum resin full-cut elastic modules for rough polishing for 30 seconds and 6 groups of 800-mesh corundum resin full-cut elastic modules for rough polishing for 35 seconds, then use 8 groups of 240-mesh fiber modules for fine polishing for 30 seconds and 5 groups of 240-mesh fiber grinding brushes for fine polishing for 25 seconds.
[0206] Comparative Example 15
[0207] This comparative example provides a ceramic tile with a mold effect, which differs from Example 1 in that steps (3) and (4) are adjusted between steps (6) and (7), that is, the first ink and the second ink are printed after printing the color pattern and before spraying the protective glaze.
[0208] The various properties of the ceramic tiles of the above embodiments and comparative examples were measured, wherein the test method of the static friction coefficient was carried out in accordance with GB / T 4100-2006;
[0209] The stain resistance test is carried out in accordance with GB / T3810.14-2006. Use light oil containing chrome green and oil pen to draw 3 times each. The higher the grade, the better the stain resistance.
[0210] The glossiness is measured in accordance with GB / T 13891-2006. When the glossiness is within the range of 9°~12°, the surface depressions and protrusions have a natural transition with the surrounding areas, otherwise the transition is unnatural.
[0211] The flexural strength is determined in accordance with GB / T 4100-2015.
[0212] The wear resistance is determined in accordance with GB / T 3810.2-2016.
[0213] Color development ability is determined by visual observation;
[0214] The glaze effect is judged by visual inspection and touch.
[0215] The test results are shown in Table 1.
[0216] Table 1
[0217]
[0218] From the above data, it can be seen that the glossiness of the ceramic tiles in each embodiment is in the range of 9°~12°, the depressions and protrusions on the surface have a natural transition with the surrounding areas; the stain resistance is level 5, the static friction coefficient is above 0.92, the wear resistance is above level 3, the color development ability is strong, the flexural strength is above 44MPa, and the mold effect is good.
[0219] Comparative Examples 1 to 5 use conventional methods to prepare ceramic tiles with mold effects. Among them, Comparative Example 1 uses fine sand dry granular glaze to produce a mold effect. Although there is a certain mold effect in the hand feel, the particle size of the fine sand dry granular glaze is too small, resulting in no mold effect visually, and the resulting ceramic tiles have poor wear resistance; Comparative Example 2 uses candy dry granular glaze to produce a mold effect. The mold effect is not three-dimensional enough, with many ups and downs and repetitiveness, and feels like sand grains. In addition, the candy dry granular glaze has a high gloss, resulting in a high gloss ceramic tile that is not eye-friendly, and the resulting ceramic tile has poor wear resistance; Comparative Example 3 uses semi-polished dry granular glaze and semi-polished to produce a mold effect. Although the visual mold effect is better than Comparative Example 2, but the mold effect is worse than that of Comparative Example 2 in terms of hand feel, and the mold has many repetitive ups and downs, is unnatural, hides dirt seriously and is not wear-resistant; Comparative Example 4 uses sunken fine carving ink and fine dry particles to produce a mold effect. The line stripes are obviously sunken due to the effect of the sunken fine carving ink, but the mold effect in other parts is not obvious. Even if the coating range of the sunken fine carving ink is increased, the concave and convex texture formed is still not three-dimensional enough, and it is easy to absorb and hide dirt. Problems; Comparative Example 5 forms a mold effect by applying an adhesive to adhere dry particles and dry powder. The mold effect is not obvious and natural, and is easily affected by the external environment, making the glaze surface orange peel-like. In addition, the color development ability is poor, and it hides dirt and is not anti-slip.
[0220] Comparative Example 6 only uses the first ink, and the applicable firing temperature range is very narrow. In the actual production process, the temperature of the roller kiln will be affected by the external environment and fluctuate. The above factors lead to poor reproducibility of the mold effect of this comparative example. The mold texture effect of some batches is obvious, and the mold texture effect of some batches is not obvious. At the same time, the color of the mold effect position is too bright, and the gloss transition with the surrounding area is unnatural; Comparative Example 8 only uses the second ink, the mold texture is not obvious, the contour is undulating unnaturally, and the color is too matte, and the gloss transition with the surrounding area is unnatural; each embodiment uses the first ink and the second ink at the same time, and the organic solvents of the two inks are used to synergistically repel the aqueous glaze slurry, so that the formed mold effect is three-dimensional, deep and clear, and the bright frit and the matte frit in the two inks are organically combined to make the calcium oxide content more suitable, and the firing temperature range is wider, the mold effect has good reproducibility, and at the same time, the zinc oxide content that improves brightness and hardness is more suitable, the mold effect position feels good, and the gloss transition with the surrounding area is natural.
[0221] In Comparative Example 7, the grayscale of the first ink is relatively high, and the mold effect is obvious, but the position of the mold effect is relatively bright, which makes the mold contour unnatural, and the local sharpness and dirt are hidden, the ink discharge is unstable, and the control operation range is narrow; in Comparative Example 9, the grayscale of the second ink is relatively high, and the mold effect is obvious, but the position of the mold effect is relatively dull, which makes the mold contour unnatural and whitish, and the local sharpness and dirt are hidden, the ink discharge is unstable, and the control operation range is narrow.
[0222] In Comparative Examples 10 and 12, due to the low aluminum content in the surface glaze or protective glaze, the sintering temperature is low, the wear resistance is poor, the flexural strength is poor, and the mold effect collapses unnaturally into a defective state. Even if the sintering temperature is increased, the surface hardness of the glaze will decrease due to the low aluminum content, and the glaze viscosity and the initial melting point will be reduced, and the surface tension will be reduced, resulting in poor wear resistance, the glaze gloss is shiny and not eye-protecting, and the mold effect is poor. In Comparative Examples 11 and 13, due to the high aluminum content in the surface glaze or protective glaze, the sintering temperature is high, the stain resistance is poor, the coloring ability is poor, and the glaze surface is prickly. Even if the sintering temperature is lowered, the aluminum oxide is high, which has a greater impact on the brittleness of the glaze, and the glaze surface loses its flexibility, so that the mold position cracks during the firing process. At the same time, it will increase the viscosity of the glaze and increase the initial melting point, affecting crystallization and phase separation, and the expansion coefficient will be low, resulting in poor glaze color and dirt absorption, and the mold effect is sharp and unnatural, and the glaze gloss will be greatly reduced.
[0223] Comparative Example 14 uses a fully cut elastic module for rough polishing, has a high glossiness, is not eye-friendly, and has a general mold effect, is not skid-resistant, and has poor wear resistance.
[0224] Comparative Example 15 uses the repulsion between the mold effect ink and the protective glaze slurry to form a concave-convex texture. The repulsion effect is weak, the mold effect is not good, it is not natural, not three-dimensional, not realistic, and it hides dirt seriously.
[0225] Figures 1 to 3 This is a photo of the ceramic tile of Example 1. It can be seen that the mold effect is good, the concave and convex texture is obvious, and the depressions and protrusions on the surface have a natural transition with the surrounding areas.
[0226] Figure 4 This is a photo of the ceramic tile of Comparative Example 1, from which it can be seen that there is no mold effect;
[0227] Figure 5 This is a photo of the ceramic tile of Comparative Example 2, from which it can be seen that it has a concave-convex effect but the mold has many repetitive ups and downs;
[0228] Figure 6 This is a photo of the ceramic tile of Comparative Example 3, from which it can be seen that it has a concave-convex effect but the mold has many repetitive ups and downs;
[0229] Figure 7 This is a photo of the ceramic tile of Comparative Example 4, from which it can be seen that there is no mold effect;
[0230] Figure 8 This is a photo of the ceramic tile of Comparative Example 5. It can be seen from the picture that the mold effect is not obvious, unnatural, and the glaze surface is like orange peel;
[0231] Fig. 9 This is a photo of the ceramic tile of Comparative Example 6, from which it can be seen that the mold effect is not obvious;
[0232] Fig.10This is a photo of the ceramic tile of Comparative Example 7. It can be seen from the figure that the mold effect is obvious, but the local mold texture is too deep or too shallow, and the mold contour is unnatural;
[0233] Fig.11 This is a photo of the ceramic tile of Comparative Example 8, from which it can be seen that the mold effect is not obvious;
[0234] Fig.12 This is a photo of the ceramic tile of Comparative Example 9. It can be seen from the figure that the mold effect is obvious, but the local mold texture is too deep or too shallow, and the mold contour is unnatural.
[0235] Fig.13 This is a photo of the ceramic tile of comparative example 15. It can be seen from the picture that its mold effect is not good, it is not three-dimensional, and it is not realistic and natural.
[0236] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a ceramic tile with a mold effect, characterized in that: The following steps are involved: The green body is prepared by using green body raw materials, and then the base glaze is applied. The first ink and the second ink are sprayed at the same time according to the mold pattern. The first drying is performed, the surface glaze is sprayed, the color pattern is printed, the second drying is performed, the protective glaze is sprayed, the glaze is fired, the glaze is polished, and the edges are ground to obtain a ceramic tile with a mold effect. When the first ink is printed, the grayscale is set to 0.8%~46%; When printing the second ink, the grayscale is set to 1%~15%; The first ink comprises the following components in weight percentage: 20%-30% of the first barium frit, 3%-10% of the bright frit, 4%-10% of zinc vanadate, 55%-70% of the organic solvent, and 3%-8% of the dispersant, wherein the first barium frit comprises the following components in weight percentage: SiO2 42%-47%, Al2O3 14%-18%, CaO 3%-5%, Na2O 2%-4%, K2O 4%-7%, and BaO 14%-18%, and the bright frit comprises the following components in weight percentage: SiO2 58%-63%, Al2O3 15%-22%, CaO 2%-4%, Na2O 2%-6%, K2O 2%-4%, and Bi2O3 4%-9%; The second ink comprises the following components in weight percentage: 30%-45% of the second barium frit, 2%-10% of the matte frit, 1%-6% of zinc vanadate, 50%-60% of the organic solvent, and 2%-5% of the dispersant, wherein the second barium frit comprises the following components in weight percentage: SiO2 40%-45%, Al2O3 16%-20%, CaO 1%-3%, Na2O 3%-7%, K2O 0.5%-3%, and BaO 16%-20%, and the matte frit comprises the following components in weight percentage: SiO2 45%-55%, Al2O3 20%-23%, CaO 15%-25%, Na2O 3%-5%, K2O 2%-5%, and ZnO 5%-8%; The surface glaze layer comprises the following components in weight percentage: SiO2 49%~54%, TiO2 0.08%~0.25%, Al2O3 18%~23%, Fe2O3 0.1%~0.3%, Mn3O4 0.01%~0.02%, MgO 0.2~1.5%, CaO 0.8%~2.5%, Na2O 3.5%~5.5%, K2O 2.5%~4.5%, V2O5 0.01%~0.02%, ZrO2 4%~7%, HfO2 0.1%~0.2%, BaO 2.5%~4%, P2O5 0.1%~0.3%, SrO 0.1%~0.5%, ZnO 0.5%~2%, SO3 0.01%~0.05%, ignition loss 4.5%~7%; The raw materials of the surface glaze layer include the following components in parts by weight: 9-11 parts of aluminum oxide, 2.5-4.5 parts of barium carbonate, 28-32 parts of potassium feldspar, 28-32 parts of sodium feldspar, 0-2 parts of dolomite, 8-12 parts of nepheline, 12.5-16.5 parts of quartz, and 0.5-2 parts of zinc oxide; The protective glaze layer comprises the following components in percentage by weight: SiO2 48%-52%, TiO2 0.03%-0.15%, Al2O3 14%-18%, Fe2O3 0.1%-0.2%, MgO 1-2.5%, CaO 4.5%-6.5%, Na2O 2%-4%, K2O 2.5%-4.5%, V2O5 0.03%-0.08%, ZrO2 0.2%-0.8%, HfO2 0.01%-0.02%, BaO 5.5%-8%, P2O5 0.1%-0.2%, SrO 3.5%-5.5%, ZnO 3.5%-6%, SO3 0.01%-0.05%, ignition loss 2.5%-4.5%; The raw materials of the protective glaze layer include the following components in parts by weight: 9-11 parts of aluminum oxide, 2.5-4.5 parts of barium carbonate, 28-32 parts of potassium feldspar, 28-32 parts of sodium feldspar, 0-2 parts of dolomite, 8-12 parts of nepheline, 12.5-16.5 parts of quartz, and 0.5-2 parts of zinc oxide; The polishing step includes: using 8 groups of 600-mesh corundum resin half-cut elastic modules for rough polishing for 30s-60s, 6 groups of 800-mesh corundum resin half-cut elastic modules for rough polishing for 35s-50s, 8 groups of 240-mesh fiber modules for fine polishing for 30s-55s, and 5 groups of 240-mesh plastic silicon carbide grinding brushes for fine polishing for 25s-40s at 1.0MPa-3.0MPa.
2. The method for preparing a ceramic tile with a mold effect according to claim 1, characterized in that: The organic solvent in the first ink is isooctyl laurate, and the organic solvent in the second ink is methyl laurate; the dispersants in the first ink and the second ink are independently polyester dispersants.
3. The method for preparing a ceramic tile with a mold effect according to claim 1, characterized in that: The green body comprises the following chemical components in weight percentage: SiO2 64.5%-68.5%, Al2O3 16.4%-20.4%, K2O 2.12%-4.12%, Na2O 1.28%-3.28%, CaO 0.82%-2.82%, MgO 0.1%-2.1%, Fe2O3 1.0%-2.0%, TiO2 0.1%-0.5%, and the rest are loss on ignition and impurities.
4. The method for preparing a ceramic tile with a mold effect according to claim 1, characterized in that: The base glaze layer contains the following chemical components in weight percentage: SiO2 60%~62%, TiO2 0.05%~0.15%, Al2O3 18%~22%, Fe2O3 0.1%~0.2%, Mn3O4 0.01%~0.02%, MgO 2.5%~3.5%, CaO 2%~3%, Na2O 2.5%~4.5%, K2O 0.5%~1.5%, V2O5 0.01%~0.02%, NiO 0.01%~0.02%, ZrO2 5%~7%, HfO2 0.1%~0.2%, BaO 0.01%~0.02%, P2O5 0.1%~0.3%, and ignition loss 1.0%~3.5%.
5. The method for preparing a ceramic tile with a mold effect according to claim 1, characterized in that: At least one of the following conditions is met: S1, the step of preparing the green body using the green body raw material comprises: ball milling the green body slurry, spray drying, screening, grading, pressing and forming, and drying to obtain the green body, wherein the fineness of the slurry after ball milling satisfies the 250 mesh sieve residue of 0.8wt.%~1.2wt.%, and the grading satisfies: calculated based on the total weight of the graded raw materials, 30 mesh 1%~4%, 40 mesh 25%~32%, 60 mesh 65%~72%, 100 mesh 2%~4%; S2. When applying the bottom glaze, the bottom glaze slurry used meets the following requirements: the residue on a 325-mesh sieve is 0.6wt.%-0.8wt.%, the specific gravity is 1.88-1.92g / mL, and the flow rate is 33-38s / 100mL; S3, the base glaze application amount is 350g / m 2 -450g / m 2 ; S4: The inkjet amount of the first ink and the second ink is independently 2-50 g / m 2 ; S5, the first drying temperature is 60-120°C, and the first drying time is 1-3 minutes; S6. When spraying the glaze, the glaze slurry used meets the following requirements: the residue on a 325-mesh sieve is 0.4wt.%-0.7wt.%, the specific gravity is 1.45-1.47g / mL, and the flow rate is 32-42s / 100mL; S7, the glaze spraying amount is 500~850g / m 2 ; S8, the temperature of the second drying is 60-120°C, and the time of the second drying is 1-3 minutes; S9, when spraying the protective glaze, the protective glaze slurry meets the following requirements: the residue on a 325-mesh sieve is 0.4wt.%-0.8wt.%, the specific gravity is 1.45-1.55g / mL, and the flow rate is 28-35s / 100mL; S10: The spraying amount of the protective glaze is 200-400 g / m 2 ; S11. The maximum sintering temperature is 1180-1210°C.
6. A ceramic tile obtained by the method for preparing a ceramic tile with a mold effect as described in any one of claims 1 to 5.