A high temperature and saturated salt resistant lubricant for drilling fluid and preparation method thereof

Through the synergistic effect of modified fatty acid esters and modified alumina, a high-efficiency lubricant is formed, which solves the problem of decreased lubrication performance of traditional drilling fluid lubricants in high temperature and high salinity environments, and achieves high-efficiency lubrication and improved safety under high temperature and high salinity conditions.

CN118755454BActive Publication Date: 2024-11-19CHENGDU XIYOUHUAWEI SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411247651.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-19
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Traditional drilling fluid lubricants undergo thermal decomposition, salt corrosion, and volatilization in high-temperature and high-salt environments, leading to a sharp decline in lubrication performance and increasing drill string wear and the risk of stuck pipe.

Method used

By employing the synergistic effect of modified fatty acid esters and modified alumina, a highly efficient lubricant is formed through a unique preparation process. The modified fatty acid esters form a multi-layer adsorption film on the metal surface, while the nano-alumina modification improves dispersion performance and wear resistance, and reduces frictional resistance.

Benefits of technology

Under high temperature and high salinity conditions, it significantly reduces the frictional resistance between the drill string and the well wall, extends the life of the drill string, and improves drilling safety and efficiency. Moreover, the preparation method is simple and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of drilling fluid, and in particular to a high temperature and saturated salt resistant lubricant for drilling fluid and a preparation method thereof, which are used to solve the problem that traditional drilling fluid lubricants often suffer from thermal decomposition, salt corrosion and volatilization when facing high temperature and high salt, resulting in damage to the lubricating film structure and a sharp decrease in lubrication performance. The high temperature and saturated salt resistant lubricant for drilling fluid of the invention realizes efficient lubrication under high temperature and high saturated salinity conditions through unique formula design and preparation process under the synergistic effect of modified fatty acid ester and modified alumina, and can form a strong adsorption film under high temperature and saturated salt environment, which not only significantly reduces the friction resistance and torque between the drill tool and the well wall and mud cake, reduces the wear of the drill tool and the risk of stuck drill, prolongs the service life of the drill tool, but also improves the safety and efficiency of drilling operations, and the preparation method is simple, low cost, and easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of drilling fluid, and in particular to a high temperature and saturated salt resistant lubricant for drilling fluid and a preparation method thereof. Background Art

[0002] In the drilling process, drilling fluid is a key component. It not only carries cuttings, cools and lubricates the drill bit, but also has a direct impact on drilling efficiency and safety. Among the various functions of drilling fluid, lubrication performance is particularly important because it is directly related to the service life of the drill bit and the energy consumption during drilling. However, with the increase in exploration depth, drilling operations have to face more severe geological conditions, such as high temperature environment and formation water with high saturation salinity. When facing high temperature and high salt, traditional drilling fluid lubricants often experience thermal decomposition, salt corrosion, and volatilization, which leads to the destruction of the lubricating film structure and a sharp decline in lubrication performance, resulting in increased friction resistance between the drill bit and the well wall and mud cake, which not only aggravates the wear of the drill bit, but also increases the risk of stuck drill. Therefore, the development of a lubricant that can maintain high-efficiency lubrication performance under high temperature and high saturation salinity has important innovative significance and application value. Summary of the invention

[0003] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a high temperature and anti-saturated salt lubricant for drilling fluid and a preparation method thereof, which solves the problem that traditional drilling fluid lubricants often suffer from thermal decomposition, salt corrosion, and volatilization when facing high temperature and high salt, resulting in the destruction of the lubricating film structure and a sharp decline in lubrication performance.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following components in parts by weight:

[0006] 62.5-82.5 parts of modified fatty acid ester, 1.5-5.5 parts of modified alumina, 0.5-0.7 parts of emulsifier and 0.1-0.3 parts of defoamer;

[0007] Wherein, the modified fatty acid ester is prepared by the following steps:

[0008] Step A1: oleic acid, trimethylolpropane, p-toluenesulfonic acid and anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 20-25° C. and a stirring rate of 300-400 r / min for 20-30 min, and then the temperature is raised to 60-65° C. and stirred for reaction for 6-8 h. After the reaction is completed, the reaction product is cooled to room temperature and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution for 2-3 times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate 1;

[0009] Step A2: Add intermediate 1 and formic acid to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of 10-15°C and a stirring rate of 300-400r / min, then add hydrogen peroxide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, continue to stir and react for 10-15 hours. After the reaction is completed, add the reaction product to ethyl acetate, then stand and stratify, wash the organic phase with saturated sodium bicarbonate solution and saturated sodium chloride solution 2-3 times in sequence, then dry with anhydrous sodium sulfate, and then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain intermediate 2;

[0010] Step A3: 2,6-di-tert-butylphenol, paraformaldehyde, potassium tert-butoxide and tert-butanol are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and argon is introduced for protection. The mixture is stirred for reaction at a temperature of 20-25° C. and a stirring rate of 300-400 r / min for 20-30 min, and then the temperature is raised to reflux and stirred for reaction for 6-7 h. After the reaction is completed, the reaction product is cooled to room temperature, and then subjected to silica gel column chromatography using a mixed solvent to obtain intermediate 3;

[0011] Step A4: Add intermediate 2, intermediate 3, perfluorohexylethyl alcohol, aluminum phosphotungstate and anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 20-25°C and a stirring rate of 300-400r / min for 20-30min, then heat the temperature to 90-95°C and stir the reaction for 10-15h. After the reaction is completed, the reaction product is cooled to room temperature, then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with saturated sodium bicarbonate solution and saturated sodium chloride solution 2-3 times in sequence, then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain a modified fatty acid ester.

[0012] As a further solution of the present invention: the usage ratio of the oleic acid, trimethylolpropane, p-toluenesulfonic acid and anhydrous toluene in step A1 is 33-36 mmol: 10 mmol: 0.2-0.4 g: 40-50 mL.

[0013] As a further solution of the present invention: the usage ratio of the intermediate 1, formic acid and hydrogen peroxide solution in step A2 is 10 mmol:40-50 mmol:30-35 mL.

[0014] As a further solution of the present invention: the mass fraction of the hydrogen peroxide solution in step A2 is 25-30%.

[0015] As a further scheme of the present invention: the usage ratio of the 2,6-di-tert-butylphenol, paraformaldehyde, potassium tert-butoxide and tert-butanol in step A3 is 4 g: 2.5-3.5 g: 8-10 mmol: 40-50 mL.

[0016] As a further solution of the present invention: the mixed solvent in step A3 is a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:7-9.

[0017] As a further scheme of the present invention: the usage ratio of the intermediate 2, intermediate 3, perfluorohexylethyl alcohol, aluminum phosphotungstate and anhydrous toluene in step A4 is 10 mmol: 15-20 mmol: 15-20 mmol: 0.3-0.5 g: 80-100 mL.

[0018] As a further solution of the present invention: the modified alumina is prepared by the following steps:

[0019] Hexafluorobutyl acrylate and silane coupling agent KH-570 are added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen is introduced for protection. The reaction is stirred for 3-5 minutes at a temperature of 20-25°C and a stirring rate of 300-400r / min. Then, azobisisobutyronitrile solution is added dropwise while stirring, and the dropping rate is controlled to be 1-2 drops / s. After the addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 4-6 hours. Then, the temperature is lowered to 60-65°C and the pH is adjusted to 5-6 with hydrochloric acid solution. Then, nano-alumina is added and the stirring reaction is continued for 20-30 hours. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed with tetrahydrofuran 2-3 times, and then placed in a vacuum drying oven and dried at a temperature of 70-75°C for 3-5 hours to obtain modified alumina.

[0020] As a further solution of the present invention: the usage ratio of hexafluorobutyl acrylate, silane coupling agent KH-570, azobisisobutyronitrile solution and nano-alumina is 0.1-2.1g: 0.8-3.2g: 40-50mL: 1g.

[0021] As a further solution of the present invention: the azobisisobutyronitrile solution is a solution formed by dissolving azobisisobutyronitrile in anhydrous ethanol at a ratio of 0.05-0.07 g:20 mL.

[0022] As a further solution of the present invention: the mass fraction of the hydrochloric acid solution is 8-12%.

[0023] As a further solution of the present invention: the nano-alumina is nano-alumina with a particle size of 70 nm and α crystal form.

[0024] As a further solution of the present invention: a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid comprises the following steps:

[0025] Step 1: Weigh 62.5-82.5 parts of modified fatty acid ester, 1.5-5.5 parts of modified alumina, 0.5-0.7 parts of emulsifier and 0.1-0.3 parts of defoamer according to weight parts, and set aside;

[0026] Step 2: Add modified fatty acid ester, modified alumina, emulsifier and defoamer into a mixer, stir and mix for 0.5-1.5h at a temperature of 40-60°C and a stirring rate of 300-400r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0027] As a further solution of the present invention: the emulsifier is one of sorbitan monooleate and polysorbate 80.

[0028] As a further solution of the present invention: the defoaming agent is DF-103 defoaming agent.

[0029] Beneficial effects of the present invention:

[0030] The invention discloses a high temperature and saturated salt resistant lubricant for drilling fluid and a preparation method thereof. The high temperature and saturated salt resistant lubricant for drilling fluid is obtained by adding modified fatty acid ester, modified alumina, emulsifier and defoamer into a mixer and stirring and mixing. The high temperature and saturated salt resistant lubricant for drilling fluid of the invention realizes efficient lubrication under high temperature and high saturated salinity conditions under the synergistic effect of modified fatty acid ester and modified alumina through unique formula design and preparation process, and can form a strong adsorption film under high temperature and saturated salt environment, which not only significantly reduces the friction resistance and torque between the drill tool and the well wall and mud cake, reduces the wear of the drill tool and the risk of stuck drill, prolongs the service life of the drill tool, but also improves the safety and efficiency of drilling operations. Moreover, the preparation method thereof is simple, low in cost and easy to industrialize.

[0031] In the process of preparing the high temperature and saturated salt resistant lubricant for drilling fluid, a modified fatty acid ester is first prepared. First, oleic acid and trimethylolpropane are reacted, and the carboxyl group on the oleic acid reacts with the three hydroxyl groups on the trimethylolpropane to form an intermediate 1 containing three ester groups. Then, the intermediate 1, formic acid and a hydrogen peroxide solution are reacted, and the intermediate 1 is oxidized with hydrogen peroxide as an oxidant, so that the olefin group on the intermediate 1 is converted into an epoxy group to obtain an intermediate 2. Then, 2,6-di-tert-butylphenol and polyformaldehyde are reacted to introduce a hydroxymethyl group on the benzene ring of 2,6-di-tert-butylphenol to obtain an intermediate 3. Then, the intermediate 2, the intermediate 3 and perfluorohexylethyl alcohol are reacted, and the epoxy group on the intermediate 2 is reacted with The hydroxyl groups on the intermediate 3 and perfluorohexylethyl alcohol react to introduce a hindered phenol structure and a large number of CF bonds to obtain a modified fatty acid ester; the modified fatty acid ester has a large number of ester groups and can form a multilayer adsorption film on the metal surface, thereby increasing the thickness and stability of the lubricating film. At the same time, the introduction of the fluorine element enhances the high temperature stability and chemical stability of the lubricant, thereby greatly improving the high temperature resistance and saturated salt resistance of the lubricant. The introduced hindered phenol structure gives it excellent antioxidant properties, thereby further improving its high temperature stability and chemical stability. The introduction of a large number of CF bonds enables the lubricant to have a very small friction coefficient, exhibiting good lubricity, thereby further improving the lubrication performance of the lubricant.

[0032] In the process of preparing the high temperature and saturated salt resistant lubricant for the drilling fluid, a modified alumina is also prepared. Hexafluorobutyl acrylate and silane coupling agent KH-570 are used as modifiers to modify the nano alumina. First, hexafluorobutyl acrylate and silane coupling agent KH-570 are polymerized using olefin groups to improve the degree of crosslinking and improve the mechanical properties. Then, the siloxane groups on the polymer are hydrolyzed to form silanols and then grafted to the particle surface of the nano alumina, so that the dispersion performance of the nano alumina is greatly improved, so that it can be evenly dispersed in the lubricant. The nano alumina has high hardness and high wear resistance. After fluorine-silicon modification, its surface energy is reduced. After adding it to the lubricant, it can convert the sliding friction part into rolling friction, play the role of "micro ball" in the friction process, and generate a chemical film on the surface of the friction pair to reduce friction, so that the stability and wear resistance of the lubricant are greatly improved. After being modified with hexafluorobutyl acrylate, a large number of CF bonds are introduced, so that the lubrication performance is further improved. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Embodiment 1:

[0035] This embodiment is a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following steps:

[0036] Step S1: 33 mmol oleic acid, 10 mmol trimethylolpropane, 0.2 g p-toluenesulfonic acid and 40 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 20° C. and a stirring rate of 300 r / min for 20 min, and then the mixture is stirred for reaction for 6 h at a temperature of 60° C. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed twice with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate 1;

[0037] Step S2: 10 mmol of intermediate 1 and 40 mmol of formic acid are added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 10° C. and a stirring rate of 300 r / min for 20 min, and then 30 mL of a 25% by mass hydrogen peroxide solution is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the stirring reaction is continued for 10 h. After the reaction is completed, the reaction product is added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed twice with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 2;

[0038] Step S3: 4 g of 2,6-di-tert-butylphenol, 2.5 g of paraformaldehyde, 8 mmol of potassium tert-butoxide and 40 mL of tert-butanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and argon was introduced for protection. The mixture was stirred at 20° C. and a stirring rate of 300 r / min for 20 min, and then the temperature was raised to reflux and stirred for 6 h. After the reaction was completed, the reaction product was cooled to room temperature, and then subjected to silica gel column chromatography using a mixed solvent of ethyl acetate and petroleum ether in a volume ratio of 1:7 to obtain intermediate 3;

[0039] Step S4: 10 mmol of intermediate 2, 15 mmol of intermediate 3, 15 mmol of perfluorohexylethyl alcohol, 0.3 g of aluminum phosphotungstate and 80 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 20° C. and a stirring rate of 300 r / min for 20 min, and then the mixture is stirred for reaction for 10 h at a temperature of 90° C. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed twice with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain a modified fatty acid ester;

[0040] Step S5: 0.1 g of hexafluorobutyl acrylate and 0.8 g of silane coupling agent KH-570 were added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen was introduced for protection. The reaction was stirred for 3 min at a temperature of 20° C. and a stirring rate of 300 r / min, and then 40 mL of azobisisobutyronitrile was added dropwise while stirring. The azobisisobutyronitrile solution formed by dissolving 0.05 g:20 mL in anhydrous ethanol was , the drop rate was controlled to be 1 drop / s, after the drop addition was completed, the temperature was raised to reflux and the reaction was continued with stirring for 4 hours, then the temperature was lowered to 60°C and the pH was adjusted to 5 with a hydrochloric acid solution with a mass fraction of 8%, then 1g of nano-alumina with a particle size of 70nm and α-crystal was added and the reaction was continued with stirring for 20 hours, after the reaction was completed, the reaction product was centrifuged, the precipitate was washed twice with tetrahydrofuran, and then placed in a vacuum drying oven and dried at a temperature of 70°C for 3 hours to obtain modified alumina;

[0041] Step S6: weighing 62.5 parts of modified fatty acid ester, 1.5 parts of modified alumina, 0.5 parts of emulsifier and 0.1 parts of defoamer according to weight for later use; the emulsifier is sorbitan monooleate; the defoamer is DF-103 defoamer;

[0042] Step S7: Add modified fatty acid ester, modified alumina, emulsifier and defoamer into a mixer, stir and mix for 0.5 h at a temperature of 40° C. and a stirring rate of 300 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0043] Embodiment 2:

[0044] This embodiment is a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following steps:

[0045] Step S1: 35 mmol oleic acid, 10 mmol trimethylolpropane, 0.3 g p-toluenesulfonic acid and 45 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 22° C. and a stirring rate of 350 r / min for 25 min, and then the mixture is stirred for reaction for 7 h at a temperature of 62° C. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed twice with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate 1;

[0046] Step S2: 10 mmol of intermediate 1 and 45 mmol of formic acid were added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen was introduced for protection. The reaction was stirred for 25 min at a temperature of 12 ° C and a stirring rate of 350 r / min, and then 32 mL of a 28% hydrogen peroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the dropwise addition was completed, the stirring reaction was continued for 12 h. After the reaction was completed, the reaction product was added to ethyl acetate, and then allowed to stand for stratification. The organic phase was washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 2;

[0047] Step S3: 4 g of 2,6-di-tert-butylphenol, 3.0 g of paraformaldehyde, 9 mmol of potassium tert-butoxide and 45 mL of tert-butanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and argon was introduced for protection. The mixture was stirred at 22° C. and a stirring rate of 350 r / min for 25 min, and then the mixture was stirred at reflux for 6.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then subjected to silica gel column chromatography using a mixed solvent of ethyl acetate and petroleum ether in a volume ratio of 1:8 to obtain intermediate 3;

[0048] Step S4: 10 mmol of intermediate 2, 18 mmol of intermediate 3, 18 mmol of perfluorohexylethyl alcohol, 0.4 g of aluminum phosphotungstate and 90 mL of anhydrous toluene were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 25 min at a temperature of 22 ° C and a stirring rate of 350 r / min, and then the temperature was raised to 92 ° C and the reaction was stirred for 13 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase was washed twice with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a modified fatty acid ester;

[0049] Step S5: 1.1 g of hexafluorobutyl acrylate and 2.0 g of silane coupling agent KH-570 were added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen was introduced for protection. The reaction was stirred for 4 min at a temperature of 22 ° C and a stirring rate of 350 r / min. Then, 45 mL of azobisisobutyronitrile was added dropwise while stirring. The azobisisobutyronitrile solution formed by dissolving 0.06 g:20 mL of azobisisobutyronitrile in anhydrous ethanol was controlled. The droplet acceleration rate is 1 drop / s. After the droplet addition is completed, the temperature is raised to reflux and the reaction is continued with stirring for 5 hours. Then, the temperature is lowered to 62°C and the pH is adjusted to 5.5 with a 10% hydrochloric acid solution by mass. Then, 1 g of nano-alumina with a particle size of 70 nm and α-crystal is added and the reaction is continued with stirring for 25 hours. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed twice with tetrahydrofuran, and then placed in a vacuum drying oven and dried at a temperature of 72°C for 4 hours to obtain modified alumina.

[0050] Step S6: weighing 72.5 parts of modified fatty acid ester, 3.5 parts of modified alumina, 0.6 parts of emulsifier and 0.2 parts of defoamer according to weight for later use; the emulsifier is sorbitan monooleate; the defoamer is DF-103 defoamer;

[0051] Step S7: Add modified fatty acid ester, modified alumina, emulsifier and defoamer into a mixer, stir and mix for 1.0 h at a temperature of 50° C. and a stirring rate of 350 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0052] Embodiment 3:

[0053] This embodiment is a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following steps:

[0054] Step S1: 36 mmol oleic acid, 10 mmol trimethylolpropane, 0.4 g p-toluenesulfonic acid and 50 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 30 min, and then the mixture is stirred for reaction at a temperature of 65° C. for 8 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed three times with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate 1;

[0055] Step S2: 10 mmol of intermediate 1 and 50 mmol of formic acid are added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 15 ° C and a stirring rate of 400 r / min. Then, 35 mL of a 30% hydrogen peroxide solution by mass is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 15 h. After the reaction is completed, the reaction product is added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 2;

[0056] Step S3: 4 g of 2,6-di-tert-butylphenol, 3.5 g of paraformaldehyde, 10 mmol of potassium tert-butoxide and 50 mL of tert-butanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and argon was introduced for protection. The mixture was stirred for reaction at 25° C. and a stirring rate of 400 r / min for 30 min, and then the temperature was raised to reflux and stirred for reaction for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then subjected to silica gel column chromatography using a mixed solvent of ethyl acetate and petroleum ether in a volume ratio of 1:9 to obtain intermediate 3;

[0057] Step S4: 10 mmol of intermediate 2, 20 mmol of intermediate 3, 20 mmol of perfluorohexylethyl alcohol, 0.5 g of aluminum phosphotungstate and 100 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 25 ° C and a stirring rate of 400 r / min, and then the temperature is raised to 95 ° C and the reaction is stirred for 15 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a modified fatty acid ester;

[0058] Step S5: 2.1 g of hexafluorobutyl acrylate and 3.2 g of silane coupling agent KH-570 were added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 5 min, and then 50 mL of azobisisobutyronitrile was added dropwise while stirring. The azobisisobutyronitrile solution formed by dissolving 0.07 g:20 mL of azobisisobutyronitrile in anhydrous ethanol was formed. The dropping rate was controlled to be 2 drops / s. After the dropping was completed, the temperature was raised to reflux and the reaction was continued with stirring for 6 hours. Then, the temperature was lowered to 65°C and the pH was adjusted to 6 with a 12% hydrochloric acid solution. Then, 1 g of nano-alumina with a particle size of 70 nm and α-crystal was added and the reaction was continued with stirring for 30 hours. After the reaction was completed, the reaction product was centrifuged, and the precipitate was washed with tetrahydrofuran for 3 times, and then placed in a vacuum drying oven and dried at 75°C for 5 hours to obtain modified alumina.

[0059] Step S6: weighing 82.5 parts of modified fatty acid ester, 5.5 parts of modified alumina, 0.7 parts of emulsifier and 0.3 parts of defoamer according to weight for later use; the emulsifier is polysorbate 80; the defoamer is DF-103 defoamer;

[0060] Step S7: Add modified fatty acid ester, modified alumina, emulsifier and defoamer into a mixer, stir and mix for 1.5 hours at a temperature of 60° C. and a stirring rate of 400 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0061] Comparative Example 1:

[0062] This comparative example is a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following steps:

[0063] Step S1: 82.5 parts of methyl oleate, 0.7 parts of emulsifier and 0.3 parts of defoamer are weighed according to weight and set aside; the emulsifier is polysorbate 80; the defoamer is DF-103 defoamer;

[0064] Step S7: adding methyl oleate, emulsifier and defoamer into a mixer, stirring and mixing for 1.5 hours at a temperature of 60° C. and a stirring rate of 400 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0065] Comparative Example 2:

[0066] This comparative example is a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following steps:

[0067] Step S1: 36 mmol oleic acid, 10 mmol trimethylolpropane, 0.4 g p-toluenesulfonic acid and 50 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 30 min, and then the mixture is stirred for reaction at a temperature of 65° C. for 8 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed three times with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate 1;

[0068] Step S2: 10 mmol of intermediate 1 and 50 mmol of formic acid are added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 15 ° C and a stirring rate of 400 r / min. Then, 35 mL of a 30% hydrogen peroxide solution by mass is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 15 h. After the reaction is completed, the reaction product is added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 2;

[0069] Step S3: 4 g of 2,6-di-tert-butylphenol, 3.5 g of paraformaldehyde, 10 mmol of potassium tert-butoxide and 50 mL of tert-butanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and argon was introduced for protection. The mixture was stirred for reaction at 25° C. and a stirring rate of 400 r / min for 30 min, and then the temperature was raised to reflux and stirred for reaction for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then subjected to silica gel column chromatography using a mixed solvent of ethyl acetate and petroleum ether in a volume ratio of 1:9 to obtain intermediate 3;

[0070] Step S4: 10 mmol of intermediate 2, 20 mmol of intermediate 3, 20 mmol of perfluorohexylethyl alcohol, 0.5 g of aluminum phosphotungstate and 100 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 25 ° C and a stirring rate of 400 r / min, and then the temperature is raised to 95 ° C and the reaction is stirred for 15 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a modified fatty acid ester;

[0071] Step S6: 82.5 parts of modified fatty acid ester, 0.7 parts of emulsifier and 0.3 parts of defoamer are weighed in parts by weight for later use; the emulsifier is polysorbate 80; the defoamer is DF-103 defoamer;

[0072] Step S7: adding the modified fatty acid ester, emulsifier and defoamer into a mixer, stirring and mixing for 1.5 hours at a temperature of 60° C. and a stirring rate of 400 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0073] Comparative Example 3:

[0074] This comparative example is a method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid, comprising the following steps:

[0075] Step S1: 36 mmol oleic acid, 10 mmol trimethylolpropane, 0.4 g p-toluenesulfonic acid and 50 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 400 r / min for 30 min, and then the mixture is stirred for reaction at a temperature of 65° C. for 8 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed three times with a saturated sodium bicarbonate solution and a saturated sodium chloride solution in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent to obtain an intermediate 1;

[0076] Step S2: 10 mmol of intermediate 1 and 50 mmol of formic acid are added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 15 ° C and a stirring rate of 400 r / min. Then, 35 mL of a 30% hydrogen peroxide solution by mass is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 15 h. After the reaction is completed, the reaction product is added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 2;

[0077] Step S3: 4 g of 2,6-di-tert-butylphenol, 3.5 g of paraformaldehyde, 10 mmol of potassium tert-butoxide and 50 mL of tert-butanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and argon was introduced for protection. The mixture was stirred for reaction at 25° C. and a stirring rate of 400 r / min for 30 min, and then the temperature was raised to reflux and stirred for reaction for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then subjected to silica gel column chromatography using a mixed solvent of ethyl acetate and petroleum ether in a volume ratio of 1:9 to obtain intermediate 3;

[0078] Step S4: 10 mmol of intermediate 2, 20 mmol of intermediate 3, 20 mmol of perfluorohexylethyl alcohol, 0.5 g of aluminum phosphotungstate and 100 mL of anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 25 ° C and a stirring rate of 400 r / min, and then the temperature is raised to 95 ° C and the reaction is stirred for 15 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase is washed with a saturated sodium bicarbonate solution and a saturated sodium chloride solution three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a modified fatty acid ester;

[0079] Step S6: 82.5 parts of modified fatty acid ester, 5.5 parts of nano-alumina with a particle size of 70 nm and α-crystal form, 0.7 parts of emulsifier and 0.3 parts of defoamer are weighed according to weight parts for later use; the emulsifier is polysorbate 80; the defoamer is DF-103 defoamer;

[0080] Step S7: Add modified fatty acid ester, nano-alumina, emulsifier and defoamer into a mixer, stir and mix for 1.5 hours at a temperature of 60° C. and a stirring rate of 400 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

[0081] Performance Test:

[0082] Preparation of fresh water-based slurry: Add 400 mL of deionized water into the slurry cup, then add 0.7 g of anhydrous sodium carbonate and 20.0 g of sodium-based bentonite for testing, and stir for 20 min at a stirring rate of 10,000 r / min. Stop twice during the stirring process and use a glass rod to scrape off the bentonite adhering to the stirring cup. After stirring, seal and cure at room temperature for 24 h.

[0083] Preparation of 4% salt water slurry: Add 16g of sodium chloride to the fresh water base slurry and stir for 20min at a stirring rate of 10000r / min;

[0084] Preparation of saturated salt water slurry: Add 144 g of sodium chloride to the fresh water base slurry and stir for 20 min at a stirring rate of 10,000 r / min;

[0085] 4 g of the high temperature and saturated salt resistant lubricant for drilling fluid from Examples 1-3 and Comparative Examples 1-3 were added to 400 mL of fresh water base slurry, 4% brine slurry and saturated brine slurry, respectively, and stirred for 5 min at a stirring rate of 10000 r / min. The lubrication coefficient reduction rate before hot rolling aging was tested, and then rolling aging was carried out at a temperature of 220°C for 16 h, and then cooled to room temperature, and then stirred for 5 min, and the lubrication coefficient reduction rate after hot rolling aging was tested.

[0086] The test results are shown in the following table:

[0087]

[0088] Referring to the data in the above table, it can be known that the lubricating performance of the high temperature and saturated salt resistant lubricant for drilling fluid in the present invention is excellent, and the performance improvement effect of the high temperature and saturated salt resistant lubricant for drilling fluid prepared under the synergistic effect of modified fatty acid ester and nano-alumina is the best. The high temperature and saturated salt resistant lubricant for drilling fluid can significantly reduce the extreme pressure lubrication coefficient, has strong salt resistance, and can withstand temperatures up to 220°C. It is suitable for well types such as vertical wells, inclined wells and horizontal wells, fresh water, seawater and saturated salt water drilling fluid systems, and is especially suitable for high-density drilling fluid systems for deep wells and ultra-deep wells.

[0089] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0090] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A high temperature and saturated salt resistant lubricant for drilling fluid, characterized in that: It comprises the following components in parts by weight: 62.5-82.5 parts of modified fatty acid ester, 1.5-5.5 parts of modified alumina, 0.5-0.7 parts of emulsifier and 0.1-0.3 parts of defoaming agent; Wherein, the modified fatty acid ester is prepared by the following steps: Step A1: oleic acid, trimethylolpropane, p-toluenesulfonic acid, and anhydrous toluene are stirred and reacted. After the reaction, the reaction product is cooled and then added to ethyl acetate. The organic phase is allowed to stand for stratification, washed and dried, and then vacuum filtered. The filtrate is rotary evaporated to obtain intermediate 1. The ratio of oleic acid, trimethylolpropane, p-toluenesulfonic acid, and anhydrous toluene in step A1 is 33-36 mmol:10 mmol:0.2-0.4 g:40-50 mL. Step A2: Stirring the intermediate 1 and formic acid to react, then adding a hydrogen peroxide solution dropwise while stirring. After the addition is complete, stirring and reacting, adding the reaction product to ethyl acetate, then standing to separate, washing and drying the organic phase, and then vacuum filtering, and rotary evaporating the filtrate to obtain the intermediate 2; the ratio of the intermediate 1, formic acid, and hydrogen peroxide solution in step A2 is 10 mmol: 40-50 mmol: 30-35 mL; the mass fraction of the hydrogen peroxide solution is 25-30%; Step A3: 2,6-di-tert-butylphenol, paraformaldehyde, potassium tert-butoxide, and tert-butanol are stirred for reaction. After the reaction, the reaction product is cooled and then subjected to silica gel column chromatography using a mixed solvent to obtain intermediate 3. The amount ratio of the 2,6-di-tert-butylphenol, paraformaldehyde, potassium tert-butoxide, and tert-butanol in Step A3 is 4 g: 2.5-3.5 g: 8-10 mmol: 40-50 mL; the mixed solvent is a mixture of ethyl acetate and petroleum ether in a volume ratio of 1:7-9; Step A4: stirring and reacting intermediate 2, intermediate 3, perfluorohexylethyl alcohol, aluminum phosphotungstate, and anhydrous toluene. After the reaction, the reaction product is cooled and then added to ethyl acetate. The organic phase is allowed to stand for stratification, washed and dried, and then vacuum filtered. The filtrate is rotary evaporated to obtain a modified fatty acid ester; the amount ratio of intermediate 2, intermediate 3, perfluorohexylethyl alcohol, aluminum phosphotungstate, and anhydrous toluene in step A4 is 10 mmol: 15-20 mmol: 15-20 mmol: 0.3-0.5 g: 80-100 mL; Wherein, the modified alumina is prepared by the following steps: Hexafluorobutyl acrylate and silane coupling agent KH-570 are stirred for reaction, and then azobisisobutyronitrile solution is added dropwise with stirring. After the addition is completed, stirring and reacting are continued, and then the temperature is lowered and the pH is adjusted with hydrochloric acid solution. Then, nano-alumina is added and stirring and reacting is continued. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed and dried to obtain modified alumina. The amount ratio of hexafluorobutyl acrylate, silane coupling agent KH-570, azobisisobutyronitrile solution and nano-alumina is 0.1-2.1g:0.8-3.2g:40-50mL:1g; the azobisisobutyronitrile solution is a solution formed by dissolving azobisisobutyronitrile in anhydrous ethanol at a ratio of 0.05-0.07g:20mL; the mass fraction of the hydrochloric acid solution is 8-12%; and the nano-alumina has a particle size of 70nm and an α-crystal form.

2. A method for preparing the high temperature and saturated salt resistant lubricant for drilling fluid according to claim 1, characterized in that: The following steps are involved: Step 1: Weigh 62.5-82.5 parts of modified fatty acid ester, 1.5-5.5 parts of modified alumina, 0.5-0.7 parts of emulsifier and 0.1-0.3 parts of defoaming agent according to weight parts and set aside; Step 2: Add modified fatty acid ester, modified alumina, emulsifier and defoamer into a mixer, stir and mix for 0.5-1.5 hours at a temperature of 40-60° C. and a stirring rate of 300-400 r / min to obtain a high temperature and saturated salt resistant lubricant for drilling fluid.

3. The method for preparing a high temperature and saturated salt resistant lubricant for drilling fluid according to claim 2, characterized in that: The emulsifier is one of sorbitan monooleate and polysorbate 80; the defoaming agent is DF-103 defoaming agent.