Preparation process of a washable, antibacterial, soft fabric and its application in towels

By aminating the cotton fibers and intercalation treatment with betaine sulfonate, combined with γ-(2,3-epoxypropoxy)propyltrimethoxysilane reaction, antibacterial cotton fibers and finishing agents were prepared, and the current solution was solved There are problems of degraded performance and lack of versatility of antibacterial fabrics, which improves antibacterial, washable and flame retardant properties and extends service life.

CN118756490BActive Publication Date: 2024-12-06NANTONG SIDEFU TEXTILE DECORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411241490.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The antibacterial properties of existing antibacterial fabrics declined after multiple washings, and the traditional towel preparation lacks multifunctional requirements such as antibacterial, washing-resistant, flame retardant, etc., which poses safety hazards and health risks.

Method used

The cotton fibers pretreated with sodium hydroxide are oxidized by sodium periodate and amylated by polyethyleneimine to form antibacterial cotton fibers, and are intercalated into zinc-aluminum layered bimetallic hydroxide through sulfonate betaine sulfonate, combining with γ- (2,3-epoxypropoxy)propyltrimethoxysilane reaction to prepare a finishing agent, and an antibacterial cotton yarn is made by twisting and spinning. Wash-resistant antibacterial soft fabric is prepared through textile and one-thick and rolling process. .

Benefits of technology

It achieves a coordinated improvement in the antibacterial, wash-resistant and flame-retardant properties of the fabric, extends the service life, and enhances the softness and wash-resistant properties of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000007840280000081
    Figure GHA0000007840280000081
Patent Text Reader

Abstract

The invention discloses a preparation process of a washable, antibacterial, and soft fabric and its application in towels, and relates to the field of fabrics. When preparing the washable, antibacterial, and soft fabric, the invention uses cotton fiber as a substrate, reacts the aminated cotton fiber with dicyandiamide to obtain an antibacterial cotton fiber containing a biguanide structure, twists and spins the antibacterial cotton fiber to obtain an antibacterial cotton yarn, and then weaves the antibacterial cotton yarn into a grey cloth; intercalates betaine phosphate into a layered double metal hydroxide, and then uses γ-(2,3-epoxypropoxy)propyltrimethoxysilane for grafting to obtain a finishing agent; and uses the finishing agent to further finish the grey cloth to obtain the fabric. The fabric prepared by the invention has excellent antibacterial properties, water-resistant properties, and flame-retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fabric preparation technology, specifically to a preparation process for a washable, antibacterial, and soft fabric and its application in towels. Background Technology

[0002] Cotton fiber is widely used in the production of towels due to its good water absorption, breathability and softness. However, due to the flammability of cotton fiber, there are safety hazards during use. In addition, as an essential personal item in people's daily lives, towels are prone to the growth of bacteria and mold on their surface, which can harm human health.

[0003] Currently available antibacterial fabrics often experience a significant decline in antibacterial performance after multiple washes, resulting in a reduced lifespan. Furthermore, the traditional towel manufacturing process rarely considers the multi-functionality of the fabric and seldom performs special finishing for antibacterial, washable, and flame-retardant properties. Therefore, there is a need to develop a towel fabric with antibacterial, washable, and flame-retardant functions. Summary of the Invention

[0004] The purpose of this invention is to provide a preparation process for a washable, antibacterial, and soft fabric and its application in towels, so as to solve the problems existing in the prior art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0006] A process for preparing a washable, antibacterial, and soft fabric, wherein the washable, antibacterial, and soft fabric is made by twisting and spinning antibacterial cotton fibers into antibacterial cotton yarn, weaving the antibacterial cotton yarn into a grey fabric, and then finishing the grey fabric with a finishing agent.

[0007] As an optimization, the antibacterial cotton fiber is prepared by pretreating cotton fiber with sodium hydroxide, oxidizing it with sodium periodate, amination it with polyethyleneimine, and then reacting it with dicyandiamide.

[0008] As an optimization, the finishing agent is prepared by intercalating sulfonate betaine into a zinc-aluminum layered bimetallic hydroxide and then reacting it with γ-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0009] As an optimization, the preparation process includes the following steps:

[0010] (1) Mix pretreated cotton fibers, sodium periodate, and pure water at a mass ratio of 1:1.5-2.5:100-150 until homogeneous. React at 50-60℃ for 1-2 hours. Add 0.05-0.1 times the mass of the pretreated cotton fibers in ethylene glycol and stir for 10-30 minutes. Wash 3-4 times with pure water, then redisperse the mixture in 100-150 times the mass of the pretreated cotton fibers in pure water. Add 2-3 times the mass of the cotton fibers in polyethyleneimine and use 0.1m... Adjust the pH to 8-9 with sodium hydroxide at 1 mol / L, react at 60-70℃ for 2-3 hours, wash 6-8 times with pure water, redisperse in 100-150 times the weight of the pretreated cotton fibers in pure water, add 3-5 times the weight of the pretreated cotton fibers in dicyandiamide, adjust the pH to 6-7 with 0.1 mol / L hydrochloric acid, continue the reaction for 3-4 hours, wash 5-6 times after the reaction is complete, and dry at 60-80℃ for 6-8 hours to obtain antibacterial cotton fibers;

[0011] (2) The intercalated modified layered bimetallic hydroxide and toluene were refluxed at 70°C for 4-6 h at a mass ratio of 1:100-200. Then, 0.01-0.05 times the mass of the intercalated modified layered bimetallic hydroxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane were added. The temperature was raised to 90-95°C and refluxed for 22-24 h. After filtration and washing with pure water 5-6 times, the product was dried at 60-80°C for 24-26 h to obtain the finishing agent.

[0012] (3) Antibacterial cotton fibers are twisted and spun into antibacterial cotton yarn, and then the antibacterial cotton yarn is spun into greige fabric; the finishing agent obtained in step (2) is prepared into a finishing agent solution of 60-80g / L with pure water, and the greige fabric is added to the finishing agent solution, wherein the bath ratio of the greige fabric to the finishing solution is 1:20-30. After soaking for 60-90 minutes, the fabric is pre-dried at 60-80℃ for 2 minutes through a dip-and-roll process, and then heated to 150-180℃ for 2-5 minutes to obtain the fabric.

[0013] As an optimization, the pretreated cotton fiber is obtained by immersing the cotton fiber in a 5wt% sodium hydroxide solution, letting it stand for 2-3 hours, washing it 6-7 times with pure water, and drying it at 60-80℃ for 12-14 hours.

[0014] As an optimization, the preparation method of the intercalated modified layered bimetallic hydroxide is as follows: aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and pure water are mixed evenly at a mass ratio of 1:4-6:7-10 to obtain solution A; 0.5-1 times the mass of aluminum nitrate nonahydrate betaine phosphate and pure water are mixed at a mass ratio of 1:100-120, and the pH is adjusted to 8-9 using 4 mol / L sodium hydroxide solution to obtain solution B; solution B is added dropwise to solution A at a dropping rate of 12-36 ml / min, and the pH of the reaction is maintained at 8-9 using 4 mol / L sodium hydroxide solution. After the addition of solution B is completed, the temperature is raised to 70-80℃, and the reaction continues for 4-6 h. After filtration and washing with pure water 3-4 times, the mixture is dried at 60-80℃ for 12-14 h to obtain the intercalated modified layered bimetallic hydroxide.

[0015] As an optimization, the molecular weight of the polyethyleneimine is 600 Da-10000 Da.

[0016] As an optimization, the dip-and-roll process has a dip-and-roll temperature of 20-50℃ and a roll-off rate of 60%-120%.

[0017] Compared with the prior art, the beneficial effects of the present invention are:

[0018] In preparing a washable, antibacterial, and soft fabric, this invention uses cotton fibers with good softness as a base. Aminated cotton fibers are reacted with dicyandiamide to obtain antibacterial cotton fibers containing a biguanide structure. These antibacterial cotton fibers are twisted and spun into antibacterial cotton yarn. The antibacterial cotton is then woven into a grey fabric. Phosphobetaine is intercalated into a zinc-aluminum layered bimetallic hydroxide, and then grafted with γ-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain a finishing agent. The finishing agent is used to further treat the grey fabric to obtain the finished fabric.

[0019] First, the cotton fibers are pretreated with sodium hydroxide. Sodium hydroxide, with its strong alkalinity, can effectively remove impurities from the surface of the cotton fibers, preparing them for subsequent modification. Then, the hydroxyl groups on the surface of the cotton fibers are oxidized to aldehyde groups by sodium periodate. A large number of amino groups are introduced into the cotton fibers through the Schiff base reaction between polyethyleneimine and aldehyde groups. The amino groups can undergo an addition reaction with dicyandiamide, thereby forming a biguanide structure on the cotton fibers, providing antibacterial properties to the cotton fibers.

[0020] Secondly, betaine phosphate is intercalated into zinc-aluminum layered bimetallic hydroxide via a co-precipitation reaction, imparting excellent antibacterial properties to the zinc-aluminum layered bimetallic hydroxide. Simultaneously, the layered structure of the zinc-aluminum layered bimetallic hydroxide protects the betaine phosphate from external environmental influences, enhancing the wash resistance of the fabric during subsequent modification of antibacterial cotton fibers. Then, γ-(2,3-epoxypropoxy)propyltrimethoxysilane is used to introduce epoxy groups onto the surface of the betaine phosphate-intercalated zinc-aluminum layered bimetallic hydroxide, resulting in a finishing agent with epoxy functional groups on the surface. The introduction of oxygen groups allows zinc-aluminum layered bimetallic hydroxides with phosphate betaine intercalation to be firmly grafted onto the surface of fabrics made of cotton fibers containing biguanide structures via covalent bonds, further enhancing the fabric's washability. The biguanide structure and phosphate betaine exhibit a synergistic antibacterial effect, further enhancing the fabric's antibacterial properties. The nitrogen element in the biguanide structure, the phosphorus and silicon elements in the antibacterial agent, and the layered structure of the layered bimetallic hydroxides jointly promote the fabric's flame retardant properties. Thus, the fabric prepared by this invention combines softness, washability, antibacterial properties, and flame retardancy. Detailed Implementation

[0021] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0022] Example 1:

[0023] A process for preparing a washable, antibacterial, and soft fabric, the process comprising the following steps:

[0024] (1) After immersing cotton fibers in a 5wt% sodium hydroxide solution and letting them stand for 2 hours, wash them 6 times with pure water and dry them at 60℃ for 12 hours, mix the pretreated cotton fibers, sodium periodate and pure water at a mass ratio of 1:1.5:100 evenly, react at 50℃ for 1 hour, add 0.1 times the mass of the pretreated cotton fibers in ethylene glycol and stir for 30 minutes, wash them 4 times with pure water, redisperse them in 100 times the mass of the pretreated cotton fibers in pure water, add 3 times the mass of the pretreated cotton fibers in polyethyleneimine with a molecular weight of 600, adjust the pH to 8 with 0.1mol / L sodium hydroxide, react at 60℃ for 3 hours, wash them 8 times with pure water, redisperse them in 100 times the mass of the pretreated cotton fibers in pure water, add 5 times the mass of the pretreated cotton fibers in dicyandiamide, adjust the pH to 6 with 0.1mol / L hydrochloric acid, continue to react for 4 hours, wash them 6 times after the reaction is completed, and dry them at 80℃ for 8 hours to obtain antibacterial cotton fibers;

[0025] (2) Aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and water were mixed at a mass ratio of 1:4:7 for 50 min to obtain solution A. 0.5 times the mass of aluminum nitrate nonahydrate betaine phosphate and pure water were mixed at a mass ratio of 1:100. The pH was adjusted to 8 using 4 mol / L sodium hydroxide solution to obtain solution B. Solution B was added dropwise to solution A at a rate of 12 ml / min. The pH of the reaction was maintained at 8 using 4 mol / L sodium hydroxide solution. After the addition of solution B was completed, the temperature was raised to 70℃ and the reaction continued. After reacting for 6 hours, the mixture was filtered and washed four times with pure water, then dried at 60°C for 14 hours to obtain the intercalated modified layered bimetallic hydroxide. The intercalated modified layered bimetallic hydroxide and toluene were reacted at a mass ratio of 1:100 and refluxed at 70°C for 6 hours. γ-(2,3-epoxypropoxy)propyltrimethoxysilane (0.01 times the mass of the intercalated modified layered bimetallic hydroxide) was added, the temperature was raised to 90°C, and the mixture was refluxed for 24 hours. After filtration and washing six times with pure water, the mixture was dried at 80°C for 24 hours to obtain the finishing agent.

[0026] (3) Antibacterial cotton fibers are twisted and spun into antibacterial cotton yarn, and then the antibacterial cotton yarn is spun into greige fabric; the finishing agent obtained in step (2) is prepared into a 60g / L finishing agent solution with pure water and the greige fabric is added to the finishing agent solution, wherein the bath ratio of greige fabric to finishing solution is 1:30. After soaking for 90 minutes, the fabric is subjected to a one-dip-one-pinch process with a padding temperature of 50℃ and a padding rate of 120%. It is pre-dried at 60℃ for 2 minutes and then heated to 150℃ for 5 minutes to obtain the fabric.

[0027] Example 2:

[0028] A process for preparing a washable, antibacterial, and soft fabric, the process comprising the following steps:

[0029] (1) After immersing cotton fibers in a 5 wt% sodium hydroxide solution and letting them stand for 2.5 h, wash them 7 times with pure water and dry them at 70 °C for 13 h to obtain pretreated cotton fibers; mix the pretreated cotton fibers, sodium periodate and pure water at a mass ratio of 1:2:125 evenly, react them at 55 °C for 1.5 h, add 0.07 times the mass of the pretreated cotton fibers in ethylene glycol and stir for 20 min, wash them 4 times with pure water, redisperse them in 125 times the mass of the cotton fibers in pure water, and add the pretreated cotton fibers. Polyethyleneimine with a molecular weight of 1800, at 2.5 times its mass, was added. The pH was adjusted to 8.5 using 0.1 mol / L sodium hydroxide. After reacting at 65°C for 2.5 h, the mixture was washed 8 times with pure water and redispersed in 125 times its mass of pure water containing the pretreated cotton fibers. Dicyandiamide, at 4 times its mass of the pretreated cotton fibers, was added. The pH was adjusted to 6.5 using 0.1 mol / L hydrochloric acid. The reaction was continued for 3.5 h. After the reaction was completed, the mixture was washed 6 times and dried at 70°C for 7 h to obtain antibacterial cotton fibers.

[0030] (2) Aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and water were mixed at a mass ratio of 1:5:9 for 40 min to obtain solution A. 0.7 times the mass of aluminum nitrate nonahydrate betaine phosphate and pure water were mixed at a mass ratio of 1:110. The pH was adjusted to 8.5 using 4 mol / L sodium hydroxide solution to obtain solution B. Solution B was added dropwise to solution A at a rate of 20 ml / min. The pH of the reaction was maintained at 8.5 using 4 mol / L sodium hydroxide solution. After the addition of solution B was completed, the temperature was raised to 75℃. The reaction was continued for 5 hours, filtered, and washed four times with pure water. The mixture was then dried at 70°C for 14 hours to obtain the intercalated modified layered bimetallic hydroxide. The intercalated modified layered bimetallic hydroxide and toluene were reacted at a mass ratio of 1:150 and refluxed at 70°C for 5 hours. γ-(2,3-epoxypropoxy)propyltrimethoxysilane (0.03 times the mass of the intercalated modified layered bimetallic hydroxide) was added, the temperature was raised to 92°C, and the mixture was refluxed for 23 hours. After filtration and washing six times with pure water, the mixture was dried at 70°C for 25 hours to obtain the finishing agent.

[0031] (3) Antibacterial cotton fibers are twisted and spun into antibacterial cotton yarn, and then the antibacterial cotton yarn is spun into greige fabric; the finishing agent obtained in step (2) is prepared into a 70g / L finishing agent solution with pure water and the greige fabric is added to the finishing agent solution, wherein the bath ratio of greige fabric to finishing solution is 1:25. After soaking for 70min, the fabric is subjected to a one-dip-one-pinch process with a padding temperature of 30℃ and a padding rate of 100%. It is pre-dried at 70℃ for 2min and then heated to 130℃ for 5min to obtain the fabric.

[0032] Example 3:

[0033] A process for preparing a washable, antibacterial, and soft fabric, the process comprising the following steps:

[0034] (1) After immersing cotton fibers in a 5 wt% sodium hydroxide solution and letting them stand for 3 hours, wash them 7 times with pure water and dry them at 80℃ for 14 hours to obtain pretreated cotton fibers; mix the pretreated cotton fibers, sodium periodate, and pure water at a mass ratio of 1:2:125 evenly, react them at 60℃ for 1 hour, add 0.1 times the mass of the pretreated cotton fibers in ethylene glycol and stir for 30 minutes, wash them 4 times with pure water, and then redisperse them in 150 times the mass of the pretreated cotton fibers in pure water, and add the pretreated... Polyethyleneimine with a molecular weight of 10,000, at 3 times the weight of cotton fibers, was added. The pH was adjusted to 9 using 0.1 mol / L sodium hydroxide. After reacting at 70°C for 2 hours, the mixture was washed 6 times with pure water and redispersed in 150 times the weight of the pretreated cotton fibers in pure water. Dicyandiamide at 5 times the weight of the pretreated cotton fibers was added. The pH was adjusted to 7 using 0.1 mol / L hydrochloric acid. The reaction was continued for 3 hours. After the reaction was completed, the mixture was washed 6 times and dried at 80°C for 8 hours to obtain antibacterial cotton fibers.

[0035] (2) Aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and pure water were mixed at a mass ratio of 1:6:10 for 30 min to obtain solution A. Betaine phosphate, at a mass ratio of 1:120, was mixed with pure water at a mass ratio of 1:120. The pH was adjusted to 9 using 4 mol / L sodium hydroxide solution to obtain solution B. Solution B was added dropwise to solution A at a rate of 36 ml / min. The pH of the reaction was maintained at 9 using 4 mol / L sodium hydroxide solution. After the addition of solution B was completed, the temperature was raised to 80℃ and the reaction continued. After reacting for 4 hours, the mixture was filtered and washed four times with pure water, then dried at 80°C for 14 hours to obtain the intercalated modified layered bimetallic hydroxide. The intercalated modified layered bimetallic hydroxide and toluene were reacted at a mass ratio of 1:200 and refluxed at 70°C for 6 hours. γ-(2,3-epoxypropoxy)propyltrimethoxysilane (0.05 times the mass of the intercalated modified layered bimetallic hydroxide) was added, the temperature was raised to 95°C, and the mixture was refluxed for 22 hours. After filtration and washing six times with pure water, the mixture was dried at 70°C for 24 hours to obtain the finishing agent.

[0036] (3) Antibacterial cotton fibers are twisted and spun into antibacterial cotton yarn, and then the antibacterial cotton yarn is spun into greige fabric; the finishing agent obtained in step (2) is prepared into an 80g / L finishing agent solution with pure water and the greige fabric is added to the finishing agent solution, wherein the bath ratio of greige fabric to finishing solution is 1:20. After soaking for 60 minutes, the fabric is subjected to a one-dip-one-pinch process with a padding temperature of 20℃ and a padding rate of 120%. It is pre-dried at 60℃ for 2 minutes and then heated to 150℃ for 5 minutes to obtain the fabric.

[0037] Comparative Example 1

[0038] The difference between Comparative Example 1 and Example 2 is that step (1) is omitted. Step (3) of Example 2 is modified as follows: pure cotton fibers are twisted and spun into pure cotton yarn, and then the pure cotton yarn is spun into greige fabric. The finishing agent obtained in step (2) is prepared into a 70 g / L finishing agent solution with pure water. The greige fabric is added to the finishing agent solution, wherein the bath ratio of the greige fabric to the finishing solution is 1:25. After soaking for 70 min, the fabric undergoes a one-dip-one-pinch process with a padding temperature of 30°C and a padding rate of 100%. It is pre-dried at 70°C for 2 min and then heated to 130°C for 5 min to obtain the fabric.

[0039] Comparative Example 2

[0040] The difference between Comparative Example 2 and Example 2 is that step (2) is modified as follows: aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and pure water are mixed at a mass ratio of 1:6:10 for 30 min to obtain solution A; phosphate betaine (one times the mass of aluminum nitrate nonahydrate) and pure water are mixed at a mass ratio of 1:120, and the pH is adjusted to 9 using 4 mol / L sodium hydroxide solution to obtain solution B. Solution B is added dropwise to solution A at a rate of 36 ml / min, and the pH of the reaction is maintained at 9 using 4 mol / L sodium hydroxide solution. After the addition of solution B is completed, the temperature is raised to 80°C, and the reaction continues for 4 h. After filtration and washing with pure water 4 times, the solution is dried at 80°C for 14 h to obtain the finishing agent. The remaining steps are the same as in Example 2.

[0041] Comparative Example 3

[0042] The difference between Comparative Example 3 and Example 2 is that step (2) is modified as follows: aluminum nitrate nonahydrate, zinc nitrate hexahydrate, and pure water are mixed at a mass ratio of 1:5:9 for 40 min to obtain solution A; the pH of solution A is adjusted to 8.5 using a 4 mol / L sodium hydroxide solution, the temperature is raised to 75°C, and the reaction continues for 5 h. After filtration and washing with pure water 4 times, the solution is dried at 70°C for 14 h to obtain layered bimetallic hydroxide; the layered bimetallic hydroxide and toluene are refluxed at 70°C for 5 h at a mass ratio of 1:150, γ-(2,3-epoxypropoxy)propyltrimethoxysilane is added at 0.03 times the mass of the layered bimetallic hydroxide, the temperature is raised to 92°C, and the reaction continues for 23 h. After filtration and washing with pure water 6 times, the solution is dried at 70°C for 25 h to obtain the finishing agent. The remaining steps are the same as in Example 2.

[0043] Test case

[0044] The antibacterial rate of Examples 1-3, Comparative Examples 1-3, and the pure cotton fabrics after 50 standard washes were tested according to GB / T 20944.3-2008. The limiting oxygen index of Examples 1-3, Comparative Examples 1-3, and the pure cotton fabrics after 50 standard washes was tested according to GB / T 5454-1997. The standard washing method was based on GB / T 5713-2013. The results are shown in Table 1.

[0045] Table 1

[0046]

[0047] A comparison of the experimental data of Examples 1-3, Comparative Example 1, and pure cotton fabric in Table 1 shows that the fabric prepared by the present invention has good antibacterial properties, water resistance, and flame retardant properties.

[0048] By comparison, the antibacterial rate of Examples 1-3 was greater than that of Comparative Example 1, and the limiting oxygen index of Examples 1-3 was greater than that of Comparative Example 1. After 50 standard water washes, Examples 1-3 still had a high antibacterial rate and limiting oxygen index, while the antibacterial rate and limiting oxygen index of Comparative Example 1 decreased. This indicates that the biguanide structure on the prepared antibacterial cotton fiber provides certain antibacterial properties to the cotton fiber, and the introduction of a large number of amino groups on the antibacterial cotton fiber provides active sites for the incorporation of epoxy functional groups on the surface of the subsequent finishing agent. The nitrogen element on the antibacterial cotton fiber has certain flame retardant properties.

[0049] By comparison, the limiting oxygen index of Examples 1-3 was greater than that of Comparative Example 2. After 50 standard washes, Examples 1-3 still had a high antibacterial rate and limiting oxygen index, while the limiting oxygen index of Comparative Example 2 decreased. This is because γ-(2,3-epoxypropoxy)propyltrimethoxysilane introduces epoxy groups onto the surface of zinc-aluminum layered bimetallic hydroxide intercalated with phosphate betaine, resulting in a finishing agent with epoxy functional groups on the surface. The introduction of epoxy groups allows the zinc-aluminum layered bimetallic hydroxide intercalated with phosphate betaine to be firmly grafted onto the surface of fabrics made of cotton fibers containing biguanide structures through covalent bonds, further enhancing the washability of the fabric. The silicon element in the finishing agent has certain flame retardant properties.

[0050] By comparison, the antibacterial rate of Examples 1-3 was greater than that of Comparative Example 3, the limiting oxygen index of Examples 1-3 was greater than that of Comparative Example 3, and the limiting oxygen index of Comparative Example 3 was greater than that of Comparative Example 1. This indicates that the insertion of sulfonate betaine in the finishing agent further improved the antibacterial properties of the antibacterial cotton fiber, while the layered structure of the layered bimetallic hydroxide and the phosphorus element in phosphate betaine further improved the flame retardant properties of the fabric.

[0051] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.

Claims

1. A preparation process for a washable, antibacterial, soft fabric, characterized in that: The washable antibacterial soft fabric is made of antibacterial cotton fibers through twisting and spinning to form antibacterial cotton yarns, the antibacterial cotton yarns are woven into grey cloth, and the grey cloth is then finished with a finishing agent; the antibacterial cotton fibers are made of cotton fibers pretreated with sodium hydroxide, oxidized with sodium periodate, and then aminated with polyethyleneimine and reacted with dicyandiamide; the finishing agent is made by intercalating sulfonated betaine into zinc-aluminum layered double metal hydroxides and then reacting with γ-(2,3-epoxypropoxy)propyltrimethoxysilane.

2. The preparation process of a washable, antibacterial and soft fabric according to claim 1, characterized in that: The preparation process comprises the following steps: (1) Pretreated cotton fiber, sodium periodate and pure water were mixed evenly in a mass ratio of 1:1.5-2.5:100-150, reacted at 50-60°C for 1-2h, 0.05-0.1 times the mass of the pretreated cotton fiber was added with ethylene glycol, stirred for 10-30min, washed with pure water for 3-4 times, and then redispersed in pure water with a mass of 100-150 times the mass of the pretreated cotton fiber, 2-3 times the mass of the cotton fiber was added with polyethyleneimine, and 0.1m ol / L of sodium hydroxide is used to adjust the pH to 8-9, react at 60-70°C for 2-3h, wash with pure water for 6-8 times, redisperse in pure water with a mass of 100-150 times of the pretreated cotton fiber, add dicyandiamide with a mass of 3-5 times of the pretreated cotton fiber, adjust the pH to 6-7 with 0.1mol / L of hydrochloric acid, continue to react for 3-4h, wash 5-6 times after the reaction is completed, and dry at 60-80°C for 6-8h to obtain antibacterial cotton fiber; (2) mixing the intercalation modified layered double hydroxide and toluene in a mass ratio of 1:100-200 at 70° C. for reflux reaction for 4-6 hours, adding γ-(2,3-epoxypropoxy)propyltrimethoxysilane in an amount of 0.01-0.05 times the mass of the intercalation modified layered double hydroxide, heating to 90-95° C., reflux reaction for 22-24 hours, filtering and washing with pure water for 5-6 times, and drying at 60-80° C. for 24-26 hours to obtain a finishing agent; (3) The antibacterial cotton fiber is twisted and spun into antibacterial cotton yarn, and then the antibacterial cotton yarn is woven into grey cloth; the finishing agent obtained in step (2) is prepared into a finishing agent solution of 60-80 g / L with pure water, and the grey cloth is added to the finishing agent solution, wherein the bath ratio of the grey cloth to the finishing solution is 1:20-30, and after immersion for 60-90 minutes, the fabric is pre-baked at 60-80° C. for 2 minutes through a dipping and rolling process, and then heated to 150-180° C. and baked for 2-5 minutes to obtain the fabric.

3. The preparation process of a washable, antibacterial and soft fabric according to claim 2, characterized in that: The pretreated cotton fibers are obtained by immersing the cotton fibers in a 5wt% sodium hydroxide solution, leaving the solution to stand for 2-3 hours, washing the cotton fibers with pure water for 6-7 times, and drying the fibers at 60-80°C for 12-14 hours.

4. The preparation process of a washable, antibacterial and soft fabric according to claim 2, characterized in that: The preparation method of the intercalation modified layered double metal hydroxide comprises: mixing aluminum nitrate nonahydrate, zinc nitrate hexahydrate and pure water in a mass ratio of 1:4-6:7-10 to obtain solution A; mixing betaine phosphate with a mass ratio of 0.5-1 times of the mass of aluminum nitrate nonahydrate and pure water in a mass ratio of 1:100-120, adjusting the pH to 8-9 with a 4 mol / L sodium hydroxide solution to obtain solution B, dripping solution B into solution A at a dripping rate of 12-36 ml / min, maintaining the reaction pH at 8-9 with a 4 mol / L sodium hydroxide solution, and after the dripping of solution B is completed, heating to 70-80° C., continuing the reaction for 4-6 hours, filtering with suction, washing with pure water for 3-4 times, and drying at 60-80° C. for 12-14 hours to obtain the intercalation modified layered double metal hydroxide.

5. The preparation process of a washable, antibacterial and soft fabric according to claim 2, characterized in that: The molecular weight of the polyethyleneimine is 600Da-10000Da.

6. According to the preparation process of a washable, antibacterial and soft fabric as claimed in claim 2, the padding temperature is 20-50°C and the padding rate is 60%-120%.

7. Use of the fabric prepared by the process for preparing a washable, antibacterial, soft fabric according to any one of claims 1 to 6 in towels.