A method for preparing a lithium-ion battery composite material

Through the combination of graphite and multi-porous hard carbon composite materials and nano-silicon, the problems of low conductivity and volume expansion of silicon-based materials are solved, the conductivity and cyclic stability of the negative electrode materials of lithium batteries are improved, and high energy density and excellent cyclic performance.

CN118763210BActive Publication Date: 2024-11-22BEIJING IAMETAL NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411254853.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing silicon-based materials have poor battery electrical performance due to low electronic conductivity and poor ion conductivity, and there are problems such as large volume expansion and poor cycle stability during charging and discharging.

Method used

Using graphite and porous hard carbon composite materials as the substrate, nano-silicon is added to form graphite-hard carbon-silicon composite materials. Through graphite and porous hard carbon, the material can quickly achieve efficient transmission of ions and electrons, and reduce the silicon-based materials in Volume expansion during charging and discharging improves rate performance and cycle stability.

Benefits of technology

It significantly improves the conductivity of the material, reduces volume expansion during charging and discharging, improves the rate performance and cycle stability of the negative electrode material of lithium battery, and achieves high energy density and excellent cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763210B_ABST
    Figure CN118763210B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a negative electrode composite material for a lithium battery, comprising the following steps: (S1) after graphite and a polymer resin are uniformly mixed, solidification is completed under heating conditions, cooling, crushing, and granulation are performed to obtain composite particles; (S2) the composite particles and a pore-forming agent are uniformly mixed, pyrolysis is performed to form pores, the temperature is lowered, and calcination is performed to obtain a composite porous carbon material; the pore-forming agent includes a small molecule substance and a polymer substance; (S3) the composite porous carbon material is contacted with silane gas, and silane is deposited under heating conditions to obtain a graphite / hard carbon / silicon-based composite material; (S4) the graphite / hard carbon / silicon-based composite material is carbon-coated to obtain a product lithium battery negative electrode composite material. The negative electrode composite material obtained by the present invention has better thermal stability and conductivity, and exhibits high specific capacity, first coulomb efficiency, and cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for preparing a lithium ion battery composite material. Background Art

[0002] As people's requirements for battery energy density and cycle life continue to increase, existing graphite-based negative electrode materials (theoretical specific capacity of 372mAh / g) can no longer meet the requirements of high energy density batteries. Silicon materials have a high theoretical capacity (4200 mAh / g), so the market has turned its attention to silicon-based materials, but silicon itself is a semiconductor material with poor conductivity (conductivity of 2.52×10 -4 S / m), and the ionic conductivity and electronic conductivity are also lower than those of graphite materials, resulting in poor kinetic performance in batteries. In addition, silicon-based materials have problems such as large volume expansion and rapid capacity decay during charging and discharging, which also limits their application in batteries. Therefore, in order to achieve high energy density without causing capacity decay due to excessive volume expansion, considering the respective advantages of silicon-based materials and graphite-based negative electrode materials, the development of silicon-carbon composite materials can become a direction to solve the above problems.

[0003] Patents such as CN117766745A, CN117117151A, CN118173733A, CN118026162A, and CN117819540A disclose some silicon-carbon composite materials, in which hard carbon is generally used as a coating layer, and the hard carbon material and graphite material cannot be well combined, and their electrochemical performance is limited. CN109592660A discloses a hard carbon / graphite composite material, and the preparation method includes the following steps: S1: adding carbon-containing biomass shell powder to an acidic solution, performing microwave hydrothermal reaction in a closed environment at 100-180°C, washing, and removing impurities to obtain a hard carbon precursor. S2: Disperse graphite in a dispersant, add the hard carbon precursor, stir, dry, and pre-carbonize at 500-700°C for 1-5 hours under an inert atmosphere to obtain a pre-carbonized hard carbon / graphite composite material precursor; the mass ratio of the graphite to the hard carbon precursor is 0.1-1:1; S3: Carbonize the pre-carbonized hard carbon / graphite composite material precursor at 800-1300°C for 2-8 hours under a flowing inert atmosphere to obtain a hard carbon / graphite composite material. CN117059785A discloses a nano-silicon / biomass hard carbon / graphite composite negative electrode material, and its preparation method comprises the following steps: (1) mixing palm nut shell powder, nano-silicon and a chelating agent, and drying to obtain a gel; (2) pre-oxidizing the gel obtained in step (1) at 300°C to 450°C, crushing, washing and drying to obtain a nano-silicon / biomass hard carbon composite material precursor; (3) mixing the nano-silicon / biomass hard carbon composite material precursor obtained in step (2), graphite and a binder to obtain a slurry; (4) spray granulating the slurry obtained in step (3) to obtain composite material particles; (5) carbonizing the composite material particles obtained in step (4) at 1000°C to 1600°C, and cooling to obtain a nano-silicon / biomass hard carbon / graphite composite negative electrode material. However, its electrochemical performance needs to be improved, especially the cycle stability at high rate. CN111244407A discloses a hard carbon / graphite composite negative electrode material, and its preparation method includes the following steps: S1: cross-linking a hard carbon source to obtain a hard carbon precursor, wherein the hard carbon source is a thermoplastic polymer compound or a non-thermoplastic polymer compound; when the hard carbon source is a thermoplastic polymer compound, the temperature of the cross-linking reaction is 0 to 50°C below the softening point of the hard carbon source; when the hard carbon source is a non-thermoplastic polymer compound, the temperature of the cross-linking reaction is 250 to 350°C below the coking temperature of the hard carbon source; S2: mixing graphite, a hard carbon precursor and an additive in liquid phase and then drying; S3: pre-carbonization treatment and carbonization treatment; S4: surface coating treatment.CN112993248A discloses a method for preparing an artificial graphite-hard carbon negative electrode material, comprising the following steps: dissolving a binder in a solvent, adding artificial graphite and mixing, then adding spherical hard carbon material and conductive agent and mixing to obtain a mixture, and then pyrolyzing the mixture; the pyrolysis parameters are: heating from 30 to 35°C to 300 to 400°C at a heating rate of 2 to 6°C / min and keeping warm for 3 to 5 hours, then heating to 550 to 600°C at a heating rate of 2 to 6°C / min and keeping warm for 4 to 6 hours, and finally heating to 850 to 950°C at a heating rate of 2 to 6°C / min and keeping warm for 6 to 8 hours, and cooling to 20 to 25°C with the furnace. These patents generally directly mix graphite and hard carbon materials, but the electrochemical performance is still not excellent enough. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that the existing silicon-based materials have poor battery electrical performance due to low electronic conductivity and poor ion conductivity, and have poor cycle stability due to large volume expansion during the charge and discharge process. The present invention provides a lithium battery negative electrode composite material, which is formed by adding nano-silicon to a graphite-hard carbon-silicon composite material using graphite and a multi-porous hard carbon composite material as a substrate. The graphite and multi-porous hard carbon ensure that the material can quickly realize efficient transmission of ions and electrons, greatly improve the electrical conductivity of the material, reduce the volume expansion of the silicon-based material during the charge and discharge process, and further improve the rate performance and cycle stability of the silicon-based negative electrode material.

[0005] To achieve the above effects, the present invention provides a method for preparing a lithium battery negative electrode composite material, comprising the following steps:

[0006] (S1) After the graphite and the polymer resin are uniformly mixed, solidification is completed under heating conditions, cooling, crushing, and granulation are performed to obtain composite particles;

[0007] (S2) the composite particles and the pore-forming agent are uniformly mixed, pyrolyzed to form pores, cooled, and calcined to obtain a composite porous carbon material;

[0008] (S3) contacting the composite porous carbon material with silane gas and performing silane deposition under heating conditions to obtain a graphite / hard carbon / silicon-based composite material;

[0009] (S4) The graphite / hard carbon / silicon-based composite material is carbon-coated to become the product lithium battery negative electrode composite material.

[0010] Furthermore, in step (S1), the graphite is artificial graphite, and the particle size of the graphite is 2-50um, preferably 3-25um; the polymer resin is at least one of acrylonitrile butadiene, styrene resin, polyethylene resin, polypropylene, polystyrene, polymethyl methacrylate resin, polyformaldehyde resin, polycarbonate resin, epoxy resin, phenolic resin, furan resin, polyphenylene sulfide resin, and polyarylacetylene resin, all of which are powdered materials.

[0011] Furthermore, in step (S1), the mass ratio of the polymer resin and the graphite is 10-30:1, preferably 15-25:1. In a preferred embodiment of the present invention, the mass ratio of the polymer resin and the graphite is 17-20:1.

[0012] Furthermore, in step (S1), the equipment for uniformly mixing the polymer resin and the graphite is not particularly limited, including but not limited to a stirrer, a twin-screw mixer, a conical mixer or a particle mixer, and the mixing time is 2-8 hours, preferably 3-5 hours.

[0013] Furthermore, in step (S1), the curing condition is to treat at 150-200°C for 3-6h; the crushing is to crush the material to 5-10μm, and the crushing method includes but is not limited to jaw crushing, roller crushing, or air flow crushing; the granulation is to obtain particles with a particle size of 1-5mm, and the granulation method includes but is not limited to a granulator, ball mill or grinding.

[0014] Further, in step (S2), the pore-forming agent is at least one of a small molecule substance and a high molecule substance; the small molecule substance is selected from at least one of ammonium carbonate, ammonium bicarbonate, ammonium chloride, nitrogen silicate, carbon powder, urea, sodium sulfate, copper sulfate, sodium chloride, and calcium chloride; the high molecule substance is selected from at least one of polyvinyl alcohol, polymethyl methacrylate, polyvinyl butyral, polystyrene particles, and polyvinyl chloride; the number average molecular weight of the high molecule substance is 10,000-50,000, preferably 20,000-40,000. Preferably, the pore-forming agent is a compound of a small molecule substance and a high molecule substance in a mass ratio of 1-3:1-3.

[0015] More preferably, the pore former is a compound of ammonium salt, thiourea and polyvinyl alcohol in a mass ratio of 1-2: 1-2: 1-2. The inventor unexpectedly found that the compounded pore former can improve both the first efficiency and high rate cycle stability of the composite negative electrode material, although the reason is unknown.

[0016] Furthermore, in step (S2), the mass ratio of the composite particles to the pore-forming agent is 100:5-10; the pyrolysis pore-forming conditions are heat treatment at 200-300°C for 5-10h; and the calcination is carried out under an inert atmosphere at 500-800°C for 2-5h.

[0017] Further, in step (S3), the silane gas is selected from at least one of monosilane, disilane, and dichlorosilane, and the silane gas and protective gas are introduced into the reactor together, and the protective gas is selected from nitrogen and / or argon. The amount of silane gas introduced is controlled so that the silicon content in the composite material is 40-60wt%. For example, the ratio of the total mass of graphite and polymer resin to the silane gas flow rate is 2-3 kg·L / min.

[0018] Further, in step (S4), the carbon coating process is well known in the art, and is to place the material to be coated in a coating furnace, introduce a protective atmosphere as a carrier gas, and a carbon-containing process gas, and perform atmospheric carbon coating at 500-800°C, the flow rate of the carrier gas and the carbon-containing process gas is independently 1-3L / min, and the coating time is 5-20h. The protective atmosphere is nitrogen and / or argon, and the carbon-containing process gas is selected from at least one of methane, ethane, propane, ethylene, propylene, acetylene, and butadiene.

[0019] The lithium battery negative electrode composite material includes graphite, multi-porous hard carbon and silicon. The graphite is evenly dispersed in the resin, and solidified, crushed and granulated, and carbonized to form pores to obtain a composite material having graphite and multi-porous hard carbon. Then, the deposition of silicon-containing process gas is performed to achieve the addition of nano-silicon to obtain a negative electrode composite material of graphite, multi-porous hard carbon and silicon.

[0020] The present invention mixes the graphite material and the resin uniformly, solidifies and crushes them into granules, so that the graphite is evenly dispersed in the resin, the bonding force between the graphite and the resin is enhanced, and the structural strength of the material and the utilization rate of the material are improved. Afterwards, the above-mentioned mixed material is pyrolyzed. During the pyrolysis process, the resin gradually decomposes and carbonizes to form a hard carbon material. These hard carbons are tightly combined with the graphite particles to form a stable graphite / hard carbon composite material. The composite material has higher density, better thermal stability and conductivity. The graphite / hard carbon composite material is mixed with a pore-forming agent in a certain proportion to form pores. Through the compatibility of the pore-forming agent, the size of the formed pores can be effectively controlled, providing an effective diffusion channel and a shorter diffusion distance for lithium ions, and reducing the polarization effect occurring during the charge and discharge process. At the same time, the high specific surface area and pore structure of the material allow more lithium ions to be embedded and de-embedded, reducing the growth of lithium dendrites of metal lithium during the charge and discharge process, thereby improving the cycle life and safety of the battery. In addition, the high specific surface area and pore structure can combine more lithium ions and provide a high capacity for the lithium battery. Compared with traditional graphite carbon negative electrode materials, this material will exhibit higher capacity performance.

[0021] Nano-silicon is deposited into the pores of graphite / porous hard carbon composite materials by vapor deposition. Silicon has a higher theoretical capacity (4200 mAh / g). Combining the advantages of high capacity of silicon and high electronic conductivity and ion conductivity of carbon-carbon composite materials, a lithium-ion battery negative electrode composite material with high energy density and excellent cycle performance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is the X-ray diffraction pattern of the negative electrode composite material prepared in Example 1;

[0023] Figure 2 This is a scanning electron microscope photograph of the negative electrode composite material prepared in Example 1;

[0024] Figure 3 Element distribution diagram of the negative electrode composite material prepared in Example 1;

[0025] Figure 4 is a transmission electron microscope image of the negative electrode composite material prepared in Example 1;

[0026] Figure 5 This is the first charge and discharge curve of the negative electrode composite material prepared in Example 1. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0028] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0029] The number average molecular weight of polyvinyl alcohol is about 26,000, and the number average molecular weight of polymethyl methacrylate is about 32,000.

[0030] Example 1

[0031] (S1) 1.25 kg of graphite and 21.25 kg of phenolic resin were added to a high-speed mixer and mixed for 3 hours to make the graphite and epoxy resin uniformly mixed. The material was placed in a pyrolysis furnace and cured at 180°C for 3.5 hours. After the curing was completed, the material was taken out and cooled to room temperature, and the material was crushed to 8 μm using a jet mill, and the powder was made into 2 mm composite particles by a granulator.

[0032] (S2) The materials are mixed evenly according to the mass ratio of composite particles: pore-forming agent of 100:10, wherein the pore-forming agent is ammonium carbonate, thiourea and polyvinyl alcohol in a mass ratio of 1:1:2, and pores are formed by pyrolysis in a rotary kiln under nitrogen protection atmosphere, the pyrolysis temperature is 300°C, and the holding time is 6 hours. After cooling, the material is taken out and sieved through a vibrating screen, and then calcined in a rotary kiln under nitrogen protection atmosphere, the calcination temperature is 500°C, and the holding time is 2 hours;

[0033] (S3) Continue to heat up, and when the temperature of the rotary kiln reaches 650°C, introduce a mixed gas of monosilane gas and nitrogen in a volume ratio of 1:1 into the furnace, with a gas flow rate of 16 L / min and a ventilation time of 10 hours, and obtain a graphite / hard carbon / silicon-based composite material after cooling and screening. The silicon content in the obtained composite material is 45.3wt%.

[0034] (S4) Place the graphite / hard carbon / silicon-based composite material in a coating furnace with carrier gas protection, raise the temperature to 500°C, and introduce acetylene into the furnace for gas-phase carbon coating. The nitrogen carrier gas flow rate is 3 L / min, the carbon source gas acetylene flow rate is 1.5 L / min, and the coating time is 10 h. After the coating is completed, cool it to obtain the product negative electrode composite material.

[0035] Figure 1 is the X-ray diffraction pattern of the negative electrode composite material obtained in Example 1, Figure 2 This is the element distribution diagram of the negative electrode composite material obtained in Example 1. From the XRD spectrum and the element distribution diagram, it can be seen that nano-silicon is uniformly deposited in the graphite / hard carbon composite carbon material. Figure 3 This is a scanning electron microscope photograph of the negative electrode composite material prepared in Example 1. Figure 4 This is a transmission electron microscope photograph of the negative electrode composite material prepared in Example 1.

[0036] Example 2

[0037] The other steps are the same as those in Example 1, except that in step (S2), the mass ratio of the composite particulate material to the pore-forming agent is 100:5.

[0038] Example 3

[0039] The other steps are the same as those in Example 1, except that in step (S2), the pore-forming agent is a compound of ammonium carbonate and polyvinyl alcohol in a mass ratio of 1:1.

[0040] Example 4

[0041] The other steps are the same as those in Example 1, except that in step (S2), the pore-forming agent is a mixture of thiourea and polyvinyl alcohol in a mass ratio of 1:1.

[0042] Example 5

[0043] The other steps are the same as those in Example 1, except that in step (S2), the pore-forming agent is ammonium carbonate, copper sulfate and polyvinyl alcohol compounded in a mass ratio of 1:1:2.

[0044] Example 6

[0045] The other steps are the same as those in Example 1, except that in step (S2), the pore-forming agent is ammonium carbonate, thiourea and polymethyl methacrylate compounded in a mass ratio of 1:1:2.

[0046] Example 7

[0047] The other steps are the same as those in Example 1, except that in step (S2), the pore-forming agent is urea, thiourea and polymethyl methacrylate compounded in a mass ratio of 1:1:2.

[0048] Example 8

[0049] The same operation as in Example 1 was performed, except that in step (S1), the raw material phenolic resin was replaced by epoxy resin.

[0050] Example 9

[0051] The same operation as in Example 1 was performed, except that in step (S1), the raw material phenolic resin was replaced by furan resin.

[0052] Comparative Example 1

[0053] The same operation as in Example 1 was performed, except that in step (S1), 1.25 kg of graphite, 21.25 kg of phenolic resin, and 0.21 kg of pore-forming agent (ammonium carbonate, thiourea, and polyvinyl alcohol in a mass ratio of 1:1:2) were added to a high-speed mixer and mixed evenly, and then directly added to a pyrolysis furnace to prepare a graphite / multiporous hard carbon composite material.

[0054] Comparative Example 2

[0055] The same operation as in Example 1 was performed, except that in step (S2), the pore-forming agent was ammonium carbonate and thiourea was compounded in a mass ratio of 1:1.

[0056] Comparative Example 3

[0057] The same operation as in Example 1 is performed, except that in step (S2), the pore-forming agent is polyvinyl alcohol.

[0058] Comparative Example 4

[0059] Using commercial graphite / silicon anode materials

[0060] Application Examples

[0061] Performance test of composite materials as negative electrode materials for lithium batteries

[0062] The composite negative electrode material obtained in the embodiment of the present invention and the negative electrode material of the comparative example were subjected to electrochemical performance test according to the following method: the negative electrode, Super P and carboxymethyl cellulose and styrene-butadiene rubber composite binder were mixed in a mass ratio of 80:10::10 to form a slurry (the mass ratio of CMC and SBR was 1:1), and the slurry was applied to a copper foil with a 250μm thick wet film preparation device, and then dried for 15 minutes and placed in a vacuum dryer for 8 hours to prepare a negative electrode composite material electrode sheet; then metallic lithium was used as the counter electrode, PP+ceramic coating was used as the diaphragm, 1mol / L LiPF6 (the solvent was a mixture of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a volume ratio of 1:1:1) was used as the electrolyte, and FEC with a volume fraction of 3% was added to the electrolyte, and button cells were assembled in an argon atmosphere in an inert gas glove box of a Mikaelona glove box. The above-assembled battery was subjected to charge and discharge tests on a LAND charge and discharge test system, and the charge and discharge range was 0.005V ~ 1.5V. According to the same method, the silicon-based composite materials obtained in the examples of the present invention and the comparative examples were used as negative electrode materials to assemble button-type lithium batteries. The electrochemical test results are listed in Table 1. Figure 5 This is the first charge and discharge curve after the negative electrode material is assembled into a battery in Example 1.

[0063] Table 1 Electrochemical test results

[0064] .

[0065] From the data in Table 1, it can be seen that the negative electrode composite material provided by the present invention shows excellent performance in lithium battery tests, with high specific capacity and first coulombic efficiency. The material preparation method of the present invention is simple and efficient, and the obtained composite material has higher density, better thermal stability and conductivity, as well as effective diffusion channels and shorter diffusion distances. The material shows extremely low expansion rate in lithium ion battery performance tests, and has high specific capacity, first coulombic efficiency and cycle stability, especially cycle stability at high rates.

Claims

1. A method for preparing a lithium battery negative electrode composite material, It is characterized in that The following steps are involved: (S1) After the graphite and the polymer resin are uniformly mixed, curing is completed under heating conditions, cooling, crushing, and granulation are performed to obtain composite particles; the mass ratio of the polymer resin to the graphite is 10-30:1; (S2) the composite particles and the pore-forming agent are uniformly mixed, pyrolyzed to form pores, cooled, and calcined to obtain a composite porous carbon material; the pore-forming agent includes a small molecule substance and a polymer substance; the pore-forming agent is a compound of ammonium salt, thiourea, and polyvinyl alcohol in a mass ratio of 1-2:1-2:1-2; (S3) contacting the composite porous carbon material with silane gas and performing silane deposition under heating conditions to obtain a graphite / hard carbon / silicon-based composite material; (S4) After carbon coating, the graphite / hard carbon / silicon-based composite material becomes the product lithium battery negative electrode composite material.

2. The method for preparing the negative electrode composite material according to claim 1, It is characterized in that In step (S1), the graphite is artificial graphite, and the particle size of the graphite is 2-50um; the polymer resin is at least one of acrylonitrile butadiene, styrene resin, polyethylene resin, polypropylene, polystyrene, polymethyl methacrylate resin, polyformaldehyde resin, polycarbonate resin, epoxy resin, phenolic resin, furan resin, polyphenylene sulfide resin, and polyarylacetylene resin.

3. The method for preparing the negative electrode composite material according to claim 1, It is characterized in that In step (S1), the curing condition is to treat at 150-200°C for 3-6 hours; the crushing is to crush the material into 5-10 μm; and the granulation is to obtain particles with a particle size of 1-5 mm.

4. The method for preparing the negative electrode composite material according to claim 1, It is characterized in that In step (S2), the mass ratio of the composite particles to the pore-forming agent is 100:5-10; the pyrolysis pore-forming condition is heat treatment at 200-300°C for 5-10h; the calcination is carried out under an inert atmosphere at 500-800°C for 2-5h.

5. The method for preparing the negative electrode composite material according to claim 1, It is characterized in that In step (S3), the silane gas is selected from at least one of monosilane, disilane, and dichlorosilane, and the silane gas and protective gas are introduced into the reactor together, and the protective gas is selected from nitrogen and / or argon; the amount of silane gas introduced is controlled so that the silicon content in the composite material is 40-60wt%.

6. A lithium battery negative electrode composite material, It is characterized in that The method is prepared by any one of claims 1 to 5.

7. A lithium battery negative electrode, It is characterized in that The negative electrode composite material comprises a negative electrode composite material prepared by the preparation method according to any one of claims 1 to 5.