High-mechanical-strength atomoxetine hydrochloride double-phase microneedle and preparation method thereof

By using materials such as pullulan and Gantrez to prepare biphasic microneedles with high mechanical strength, the problems of microneedle penetration and incomplete drug release are solved, and efficient drug transport and drug delivery are achieved.

CN118766833APending Publication Date: 2024-10-15ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410702208.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The mechanical strength of existing microneedles is insufficient, making it difficult to completely penetrate the skin, and drug release is incomplete, affecting drug delivery efficiency.

Method used

Using pullulan, Gantrez S-97, Gantrez AN-119 and other materials as the tip matrix, EC, polylactic acid and other materials as the insoluble backing layer, biphasic microneedles with high mechanical strength are prepared through specific proportions and process conditions. This ensures that the drug does not migrate from the needle body layer to the backing layer, thereby improving the efficiency of transdermal drug delivery.

Benefits of technology

The mechanical strength and drug release efficiency of the microneedle are significantly improved, ensuring that the drug can completely penetrate the skin and be effectively transported into the body, meeting the penetration requirements and efficient drug delivery requirements of different skin parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005038299240000011
    Figure HDA0005038299240000011
  • Figure HDA0005038299240000012
    Figure HDA0005038299240000012
  • Figure HDA0005038299240000013
    Figure HDA0005038299240000013
Patent Text Reader

Abstract

The invention discloses a high-mechanical-strength atomoxetine hydrochloride double-phase microneedle and a preparation method thereof, and relates to the field of pharmaceutical preparations. The atomoxetine hydrochloride double-phase microneedle comprises a needle tip part and a backing layer, wherein the needle tip part is prepared from active pharmaceutical ingredients and water-soluble materials including a Pulullan (PL) polymer, a polymethyl vinyl ether-maleic anhydride copolymer and a polymethyl vinyl ether-maleic anhydride copolymer (Gantrez); the backing layer is composed of a hydrophobic material, such as ethyl cellulose (EC). According to the prepared double-phase microneedle, the medicine is gathered at the needle body part of the microneedle, the hydrophobic backing layer prevents the medicine from migrating to the backing layer, and it is ensured that the medicine in the needle body is transferred into the body. A microneedle body is prepared by compounding pullulan (PL), a polymethyl vinyl ether-maleic anhydride copolymer (Gantrez AN-119) and a polymethyl vinyl ether-maleic anhydride copolymer (Gantrez S-97), and compared with a common microneedle, the mechanical strength of the double-phase microneedle prepared by adopting the preparation method can be improved by 5-10 times; the enhancement of the mechanical strength of the microneedle can improve the transdermal penetration ability and the drug delivery efficiency of the microneedle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of medical technology, and more specifically, to a high-mechanical-strength atomoxetine hydrochloride biphasic microneedle and a preparation method thereof. Background Art

[0002] As a new type of transdermal drug delivery method, microneedles can break the barrier effect of the stratum corneum to create drug channels without touching the nerve fibers and blood vessels in the epidermis and dermis, and the channels formed by the microneedles can heal in a short time, thus avoiding the risk of infection. Although microneedles have the dual advantages of transdermal drug delivery and injection, their wide application is hindered by their low drug loading, incomplete drug release, and incomplete penetration of the skin due to weak mechanical strength of the needle body. By optimizing the polymer material of the microneedle body layer, a biphasic microneedle with ultra-high strength is prepared to ensure the complete penetration of the microneedle, which can greatly improve the drug transmission efficiency. The water-soluble needle layer material and the insoluble backing layer material are combined to prepare a biphasic microneedle. The biphasic microneedle can gather the drug in the needle body layer of the microneedle, prevent the drug from migrating from the needle body layer to the backing layer, avoid the drug that migrates to the backing layer from being transported into the body, and ensure the complete transport of the drug in the microneedle.

[0003] Biphasic microneedles have the advantage of good drug release, but while ensuring rapid drug transport, improving the mechanical strength of microneedles is still a major challenge for drug formulation developers. Deng et al. (Biomaterials science, 2023, 11, 5605-5617) prepared biphasic microneedles using polystyrene as the backing layer and PVP as the tip material of the microneedle. The microneedles prepared by this method have a weak strength of only 0.7N / needle, and the microneedles cannot fully penetrate the skin. In addition, the drug release of the microneedle in 72 hours is about 60%, and the drug release is incomplete.

[0004] The patent (CN 113332588 B) discloses a microneedle product with EC as a waterproof backing layer and hyaluronic acid (HA) and polyvinyl pyrrolidone (PVP) as a composite matrix material for the treatment of oral diseases. Although the addition of PVP improves the mechanical strength of the microneedle, the mechanical strength of the prepared microneedle is only 0.268N-0.339N / needle, which affects the penetration of the microneedle (Example 14); PVP is easy to absorb moisture, and when the relative humidity reaches 40%, the mechanical strength decreases significantly. When the relative humidity reaches 80%, the microneedle begins to deform and loses the ability to penetrate the skin (Example 11). In addition, the microneedle disclosed in the patent includes a needle body prepared from a soluble polymer, a matrix layer prepared from a soluble polymer (PVP), and a waterproof backing layer composed of an adhesive layer and a waterproof layer. Since the matrix layer connected to the needle tip is a water-soluble polymer, the drug will migrate from the microneedle tip to the matrix layer, and the drug that migrates to the matrix layer cannot enter the body, reducing the drug transmission efficiency. In order to improve the drug delivery efficiency of microneedles, the strength of the needle tip needs to be enhanced to meet the penetration ability of the microneedles in different skin parts; at the same time, the backing layer connected to the microneedle body layer needs to be made of a water-insoluble material to avoid the reverse migration of drugs from the needle body layer to the backing layer, thereby ensuring that the drugs are delivered into the body and exert the corresponding therapeutic effect.

[0005] Based on the above problems, in order to prepare microneedle products with good mechanical strength and rapid drug release, it is necessary to conduct in-depth research on the structure of microneedles, the types of composite materials, and the prescription ratio. During the research, it was unexpectedly discovered that pullulan (PL), Gantrez S-97, and Gantrez AN-119 can be used to prepare dual-phase microneedles with excellent mechanical strength according to specific proportions and process conditions. Compared with the microneedles reported in the literature and patents, the needle tip strength of the microneedles prepared by the above method can be increased by 10 times to 4N / needle. The reason for the significant improvement in the strength of the microneedles may be that the carboxyl groups of Gantrez S-97 and the carboxyl groups produced by the hydrolysis of Gantrez AN-119 form hydrogen bonds with the polymer molecules to improve the mechanical strength of the microneedles and enhance the transdermal puncture ability of the microneedles; in addition, the Gantrez polymer has good adhesion, which can increase the connectivity between the needle body and the backing material, which helps to improve the mechanical strength of the microneedles. The dual-phase microneedle product disclosed in the present invention has a backing layer composed of a water-insoluble polymer, and the drug will not migrate from the needle body layer to the backing layer, ensuring that all the drugs in the microneedle are delivered into the body.

[0006] Increasing the mechanical strength of microneedles usually reduces the drug release rate of microneedle products, and is also accompanied by incomplete drug release. Therefore, it is necessary to conduct in-depth research and optimization on the formulation and process of microneedle products. Improving the mechanical strength of microneedles will not delay the speed and degree of drug release. The drug release study of microneedles proves that the microneedles prepared by the present invention have both high mechanical strength and rapid and complete drug release characteristics.

[0007] In summary, the present invention discloses a method for preparing atomoxetine hydrochloride biphasic microneedles with high mechanical strength based on a variety of composite materials, wherein pullulan (PL), polyvinyl alcohol (PVA), chitosan (CS), Gantrez AN-119, Gantrez AN-139, Gantrez AN-169, Gantrez S-97 and Gantrez S-96 are selected as the needle tip matrix materials of the biphasic microneedles; EC, polylactic acid (PLA), polylactic acid-glycolic acid copolymer (PLGA) and polystyrene (PS) are used as the insoluble backing layer materials of the microneedles. Under the condition of meeting the high delivery efficiency of the active drug of the biphasic microneedles, the mechanical strength of the microneedles is enhanced, the requirements for the penetration of the microneedles in different skin parts are met, and the drugs are delivered into the body.

[0008] Atomoxetine Hydrochloride is the first non-stimulant drug used to treat attention deficit hyperactivity disorder (ADHD). Currently, the dosage forms on the market mainly include capsules and oral solutions. There is a lack of effective treatment for patients who are not convenient to take medicine. Therefore, it is necessary to provide a new drug delivery method for atomoxetine hydrochloride to meet the treatment needs of patients of different ages and physical conditions. Summary of the invention

[0009] The present invention aims to provide an atomoxetine hydrochloride biphasic microneedle having good mechanical strength and high drug delivery efficiency.

[0010] The first objective of the present invention is to provide a dual-phase microneedle with high mechanical strength based on a composite material. The composite material can improve the mechanical strength of the microneedle to adapt to the requirements of microneedle insertion in different skin parts. At the same time, the improvement of the mechanical strength of the microneedle will not affect the transmission speed and degree of the drug, thus meeting clinical needs.

[0011] The second object of the present invention is to provide a biphasic microneedle for improving the efficiency of microneedle drug delivery. The biphasic microneedle has a water-insoluble backing layer, which can prevent the migration of drugs from the needle body layer to the backing layer, ensure the complete release of drugs in the microneedle into the body, and achieve the purpose of efficient drug delivery.

[0012] The soluble microneedle array based on the composite material of the present invention adopts 1cm 2 There are 50 to 200 microneedles distributed on the surface, and the distance between each needle is 500 to 1200 μm.

[0013] The double-phase microneedle tip layer of the present invention is prepared by compounding a plurality of materials, and a double-phase microneedle with high mechanical strength is provided through the interaction between the plurality of composite materials.

[0014] The biphasic microneedle of the present invention uses an insoluble material such as EC as the backing layer of the biphasic microneedle to prevent the drug from migrating from the needle body layer to the backing layer, thereby improving the transdermal drug delivery efficiency of the microneedle.

[0015] The present invention also provides a method for preparing the above-mentioned high mechanical strength atomoxetine hydrochloride biphasic microneedle, comprising the following steps: quantitatively weighing pullulan (PL), polyvinyl alcohol (PVA), chitosan (CS), methyl vinyl ether-maleic anhydride series compounds (Gantrez AN-119, Gantrez AN-139, Gantrez AN-169) and polyvinyl ether-maleic acid copolymer (Gantrez S-96, Gantrez S-97) and dissolving them in water, adding drugs, stirring them fully after dissolution, mixing them evenly, and obtaining a microneedle body layer solution. Quantitatively weighing an insoluble polymer, such as EC, adding it to anhydrous ethanol, dissolving it and stirring it evenly to obtain a microneedle backing layer solution. Filling the microneedle body solution into a PDMS mold, and after centrifugation into the mold, scraping off the excess solution. The backing layer solution of the microneedle is filled in the PDMS mold with the needle body layer, and the remaining part of the microneedle mold is filled by centrifugation. The excess solution is scraped off, and after the microneedle is dried, it is demoulded and set aside.

[0016] The obtained needle body layer matrix solution is obtained by dissolving a polymer in a solvent, and the concentration of the needle body layer polymer solution is 10%-40%.

[0017] The obtained backing layer solution is obtained by dissolving the polymer in a solvent, and the concentration of the backing layer solution is 10%-40%.

[0018] Based on the above technical solution, the present invention has the following effects:

[0019] (1) The present invention prepares biphasic microneedles by using a variety of composite materials, which can effectively improve the mechanical strength of the microneedles, thereby meeting the requirements for the insertion of biphasic microneedles into different parts of the skin, ensuring the effective insertion of the microneedles and the release of drugs in the body.

[0020] (2) The microneedle of the present invention enhances the mechanical strength of the microneedle while not affecting the transmission speed of the microneedle drug and the degree of drug release.

[0021] (3) The present invention prepares atomoxetine hydrochloride biphasic microneedles with clinical value, which have a biphasic structure, can prevent the drug from migrating from the needle body layer to the needle seat backing layer, and have a high drug transmission efficiency.

[0022] (4) The biphasic microneedles prepared by the present invention can provide a new dosage form option for the clinical application of atomoxetine hydrochloride. DETAILED DESCRIPTION

[0023] In order to facilitate the understanding of the present invention, the biphasic microneedle prepared by the present invention is further described below in conjunction with specific examples. All embodiments of the present invention are given below, but the protection scope of the present invention is not limited thereto.

[0024] The present invention verifies that the present invention can effectively improve the mechanical strength of the microneedles and gather the drugs in the needle body of the microneedles through the morphology, mechanical properties, drug distribution, solubility properties, and in vitro transdermal delivery tests of the microneedles, thereby improving the transdermal drug delivery efficiency.

[0025] The in vitro transdermal drug delivery efficiency determination method used in the following examples and comparative examples is as follows:

[0026] In order to determine the transdermal drug delivery efficiency of microneedles, the present invention immersed the treated pig skin in PBS buffer for 30 minutes to maintain its elasticity, inserted the microneedles into the ex vivo skin, dissolved the remaining microneedles in the mobile phase, taped the insertion site six times, dissolved the tape in the mobile phase to dissolve the residual drug, and used high performance liquid chromatography to determine the amount of residual drug to calculate the amount of drug entering the skin. The transdermal drug delivery efficiency of the biphasic microneedles can be determined by the above detection.

[0027] The present invention uses a texture analyzer to test the mechanical strength of the microneedle.

[0028] The present invention uses fluorescent dyes to prepare biphasic microneedles, and observes the distribution of fluorescent materials through a laser confocal microscope to show the structural characteristics of the microneedles and the distribution of drugs in various structural units of the microneedles. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The morphological diagrams are of the microneedles of the microneedle arrays prepared in Examples 1 to 2 and Comparative Examples 1 to 3. A (Example 1), B (Example 2), C (Comparative Example 1), D (Comparative Example 2), E (Comparative Example 3).

[0030] Figure 2 The following are the in vitro skin insertion diagrams of the microneedle array microneedles prepared in Examples 1 to 2 and Comparative Examples 1 to 3. A (Example 1), B (Example 2), C (Comparative Example 1), D (Comparative Example 2), E (Comparative Example 3).

[0031] Figure 3 These are the in vitro dissolution diagrams of the microneedle arrays prepared in Example 4 and Comparative Example 4. Red represents drugs: A (before dissolution of the microneedles in Example 4), B (no drug residue in the backing layer after dissolution of the microneedles in Example 4), C (before dissolution of the microneedles in Comparative Example 4), and D (drug residue in the backing layer after dissolution of the microneedles in Comparative Example 4).

[0032] Figure 4The laser confocal microscope scans of the microneedle arrays prepared in Example 4 and Comparative Example 4 are shown. A (microneedle tip layer scan of Example 4), B (backing layer scan of Example 4), C (3D structure of Example 4), D (microneedle tip layer scan of Comparative Example 4), E (backing layer scan of Comparative Example 4), and F (3D structure of Comparative Example 4).

[0033] Figure 5 These are the mechanical property test results of the microneedle arrays prepared in Examples 1 to 2 (n=3).

[0034] Figure 6 The in vitro transdermal drug delivery efficiency of the microneedle arrays prepared in Examples 1 to 2 and Comparative Example 4 (n=3).

[0035] Example 1

[0036] (1) Preparation of microneedle body layer matrix solution

[0037]

[0038] (2) Preparation of microneedle backing layer matrix solution

[0039]

[0040] Dissolve PL, GantrezAN-119, and Gantrez S-97 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride to dissolve, and mix evenly to obtain a microneedle body layer matrix solution. Dissolve PLA in dichloromethane to obtain a microneedle backing layer matrix solution. Cast the body layer solution, centrifuge for 15 minutes to allow the solution to fill the body layer of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer of the microneedle. Scrape off the excess solution, dry at 37°C for 48 hours, and then demold to obtain a microneedle.

[0041] Figure 1 (A) is a morphological diagram of the microneedle, the microneedle has a good morphology and the needle formation rate is 100%; Figure 2 (B) is the insertion diagram of the microneedle, with an insertion rate of 99%; Figure 5 The mechanical strength of the microneedle is 4.31N / needle. The microneedle can be completely dissolved within 10 minutes after insertion into the skin, and the in vitro transdermal drug delivery efficiency is 92.8±2.6%.

[0042] Example 2

[0043] (1) Preparation of microneedle body layer matrix solution

[0044]

[0045] (2) Preparation of microneedle backing layer matrix solution

[0046]

[0047] Dissolve PL, GantrezAN-139, and Gantrez S-97 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride to dissolve, and mix evenly to obtain a microneedle body layer matrix solution. Dissolve EC N20 in anhydrous ethanol to obtain a microneedle backing layer matrix solution. Cast the needle body solution, centrifuge for 15 minutes to allow the solution to fill the needle body part of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer part of the microneedle. Scrape off the excess solution, dry at 40°C for 24 hours, and demold to obtain a microneedle.

[0048] Figure 1 (B) is a morphological diagram of the microneedles, which have good morphology and a needle formation rate of 100%; Figure 2 (B) is the insertion diagram of the microneedle, with an insertion rate of 100%; Figure 5 The mechanical strength of the microneedle is 4.74N / needle, and the microneedle can be completely dissolved within 10 minutes after being inserted into the skin. Figure 6 The in vitro transdermal drug delivery efficiency is 96.5±1.2%. The reason for the significant improvement in microneedle strength may be that the carboxyl groups of Gantrez S-97 and Gantrez AN-119 hydrolyzed form hydrogen bonds with polymer molecules, thereby improving the mechanical strength of the microneedles, enhancing the transdermal puncture ability of the microneedles, and improving the transdermal drug delivery efficiency.

[0049] Example 3

[0050] (1) Preparation of microneedle body layer matrix solution

[0051]

[0052] (2) Preparation of microneedle backing layer matrix solution

[0053]

[0054] Dissolve PL, GantrezAN-119, and Gantrez S-97 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride to dissolve, and mix evenly to obtain a microneedle needle layer matrix solution. Dissolve EC N20 in anhydrous ethanol to obtain a microneedle backing layer matrix solution. Cast the needle layer solution, centrifuge for 15 minutes to allow the solution to fill the needle layer part of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer part of the microneedle. Scrape off the excess solution, dry at 45°C for 36 hours, and demold to obtain a microneedle.

[0055] The microneedles have good morphology, with a needle formation rate of 97% and an insertion rate of 97%. The mechanical strength is 4.08N / needle. As shown in the figure, the microneedles can be completely dissolved within 10 minutes after being inserted into the skin. The in vitro transdermal drug delivery efficiency is 90.20±1.74%. The dissolution rate of the microneedles increases with the increase of the PL ratio. Therefore, the composite material can effectively improve the mechanical strength of the microneedles and improve the transdermal drug delivery efficiency.

[0056] Example 4

[0057] (1) Preparation of microneedle body layer matrix solution

[0058]

[0059] (2) Preparation of microneedle backing layer matrix solution

[0060]

[0061] PL and Gantrez AN-119 were dissolved in distilled water to prepare a solution, and the three were evenly mixed according to the prescription ratio. The red fluorescent dye Rhodamine-B simulated drug was added, dissolved and mixed evenly to obtain the microneedle needle layer matrix solution. EC N20 was dissolved in anhydrous ethanol, and the green fluorescent dye coumarin-6 was added to obtain the microneedle backing layer matrix solution. The needle layer solution was cast, centrifuged for 15 minutes to allow the solution to fill the needle layer part of the microneedle, and then the backing layer solution was cast, and centrifuged for 10 minutes to allow the solution to fill the backing layer part of the microneedle. The excess solution was scraped off, and the microneedles were demolded after drying at 50°C for 24 hours to obtain microneedles.

[0062] The microneedles have good morphology, with a needle formation rate of 100% and an insertion rate of 96%; the mechanical strength of the microneedles is 3.99N / needle, the microneedles can be completely dissolved within 15 minutes after insertion into the skin, and the in vitro transdermal drug delivery efficiency is 88.17±3.2%.

[0063] In vitro dissolution Figure 3 (A: before dissolution, B: no drug residue after dissolution) shows that after the EC N20 biphasic microneedles with a water-insoluble backing layer are applied to the skin, there is a slight red or even no red color in the backing layer of the microneedles, indicating that there is almost no drug residue in the backing layer. The study further confirmed that the use of the water-insoluble backing layer EC N20 can effectively prevent the migration of drugs to the backing layer, and can also avoid drug adhesion to the microneedles during the application process, thereby effectively improving the transdermal drug delivery efficiency.

[0064] The confocal scanning results are as follows Figure 4(A: microneedle tip layer scan B: microneedle backing layer scan C: microneedle 3D structure), it can be observed in the microneedle that the red fluorescent dye rhodamine-B only exists in the needle body layer of the microneedle and is evenly distributed, and the green fluorescent dye coumarin-6 only exists in the backing layer, further proving that the biphasic microneedle can ensure that the drug is completely encapsulated in the microneedle body by blocking the diffusion effect of the drug.

[0065] Example 5

[0066] (1) Preparation of microneedle body layer matrix solution

[0067]

[0068] (2) Preparation of microneedle backing layer matrix solution

[0069]

[0070] Dissolve PL and Gantrez AN-139 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride to dissolve, and mix evenly to obtain a microneedle needle layer matrix solution. Dissolve EC N20 in anhydrous ethanol to obtain a microneedle backing layer matrix solution. Cast the needle layer solution, centrifuge for 15 minutes to allow the solution to fill the needle layer part of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer part of the microneedle. Scrape off the excess solution, dry at 55°C for 16 hours, and then demold to obtain a microneedle.

[0071] The microneedles have good morphology, with a needle formation rate of 98% and an insertion rate of 95%; the mechanical strength is 3.67N / needle, and the microneedles can be completely dissolved within 10 minutes after insertion into the skin. The in vitro transdermal drug delivery efficiency is 83.56±2.8%.

[0072] Example 6

[0073] (1) Preparation of microneedle body layer matrix solution

[0074]

[0075] (2) Preparation of microneedle backing layer matrix solution

[0076]

[0077] Dissolve PVA, Gantrez AN-139, and Gantrez S-96 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug propranolol hydrochloride to dissolve, and mix evenly to obtain a microneedle body matrix solution. Dissolve PS in 1,4-dioxane to obtain a microneedle backing layer matrix solution. Cast the needle body solution, centrifuge for 15 minutes to allow the solution to fill the needle body part of the microneedle, then cast the backing solution, centrifuge for 10 minutes to allow the solution to fill the backing part of the microneedle. Scrape off the excess solution, dry at 50°C for 24 hours, and then demold to obtain a microneedle.

[0078] The microneedles have good morphology, with a needle formation rate of 100% and an insertion rate of 99%; the mechanical strength is 4.48N / needle, and the microneedles can be completely dissolved within 15 minutes after insertion into the skin. The in vitro transdermal drug delivery efficiency is 94.56±3.2%.

[0079] Example 7

[0080] (1) Preparation of microneedle body layer matrix solution

[0081]

[0082] (2) Preparation of microneedle backing layer matrix solution

[0083]

[0084] Dissolve CS and Gantrez AN-169 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug diclofenac sodium to dissolve, and mix evenly to obtain a microneedle body matrix layer solution. Dissolve PLA and PLGA in dichloromethane to obtain a microneedle backing layer matrix solution. Cast the body layer solution, centrifuge for 15 minutes to allow the solution to fill the body layer of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer of the microneedle. Scrape off the excess solution, dry at 50°C for 20 hours, and demold to obtain a microneedle.

[0085] The microneedles have good morphology, with a needle formation rate of 97% and an insertion rate of 97%; the mechanical strength is 4.05N / needle, and the microneedles can be completely dissolved within 15 minutes after insertion into the skin. The in vitro transdermal drug delivery efficiency is 88.29±2.3%.

[0086] Comparative Example 1

[0087] (1) Preparation of microneedle body layer matrix solution

[0088]

[0089] (2) Preparation of microneedle backing layer matrix solution

[0090]

[0091] Dissolve PL and Gantrez AN-119 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride, and mix evenly to obtain a microneedle body layer matrix solution. Dissolve EC N20 in anhydrous ethanol to obtain a microneedle backing layer matrix solution. Cast the body layer solution, centrifuge for 15 minutes to allow the solution to fill the body layer of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing part of the microneedle. Scrape off the excess solution, dry at 50°C for 20 hours, and demold to obtain a microneedle.

[0092] Figure 1 (C) is the morphology of the microneedle, the microneedle has poor formability, many bubbles, a needle formation rate of 77%, and an irregular appearance; Figure 2 (C) is the insertion rate of the microneedle, which is 58%, and it is difficult to successfully insert the microneedle into the skin.

[0093] Comparative Example 2

[0094] (1) Preparation of microneedle body layer matrix solution

[0095]

[0096] (2) Preparation of microneedle backing layer matrix solution

[0097]

[0098] Dissolve PL and Gantrez S-97 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride to dissolve, and mix evenly to obtain the microneedle body layer matrix solution. Dissolve PS in 1,4-dioxane to obtain the microneedle backing layer matrix solution. Cast the needle body layer solution, centrifuge for 15 minutes to allow the solution to fill the needle body layer part of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer part of the microneedle. Scrape off the excess solution, dry at 40°C for 48 hours, and then demold to obtain the microneedle.

[0099] Figure 1 (D) is a morphological diagram of microneedles. The microneedles have poor formability, many bubbles, and irregular appearance. The needle formation rate is 88%. Figure 2 (D) is a diagram of microneedle insertion, with an insertion rate of 68%. The microneedles are easily broken during insertion and are difficult to insert completely.

[0100] Comparative Example 3

[0101] (1) Preparation of microneedle body layer matrix solution

[0102]

[0103] (3) Preparation of microneedle backing layer matrix solution

[0104]

[0105] Dissolve PL, GantrezAN-119, and Gantrez S-97 in distilled water to prepare a solution, mix the three evenly according to the prescription ratio, add the active drug atomoxetine hydrochloride to dissolve, and mix evenly to obtain a microneedle body layer matrix solution. Dissolve EC N20 in anhydrous ethanol to obtain a microneedle backing layer matrix solution. Cast the body layer solution, centrifuge for 15 minutes to allow the solution to fill the body layer of the microneedle, then cast the backing layer solution, centrifuge for 10 minutes to allow the solution to fill the backing layer of the microneedle. Scrape off the excess solution, dry at 40°C for 36 hours, and demold to obtain a microneedle.

[0106] Figure 1 (E) is a morphological diagram of microneedles. The microneedles have poor formability, many bubbles, and irregular appearance. The needle formation rate is 90%. Figure 2 (E) is the insertion diagram of the microneedle, and the insertion rate is 77%. This may be due to the low proportion of pullulan (PL), which leads to poor toughness of the microneedle and easy breakage of the microneedle during insertion.

[0107] Comparative Example 4

[0108] (1) Preparation of microneedle matrix solution

[0109]

[0110] (3) Preparation of microneedle backing layer matrix solution

[0111]

[0112] PL and Gantrez AN-119 were dissolved in distilled water to prepare a solution, and the three were evenly mixed according to the prescription ratio. The red fluorescent dye Rhodamine-B was added to simulate the drug and dissolved, and mixed evenly to obtain the microneedle needle layer matrix solution. PL was dissolved in distilled water, and the green fluorescent dye coumarin-6 was added to dissolve to obtain the microneedle backing layer matrix solution. Centrifuge for 15 minutes to allow the solution to fill the needle body layer of the microneedle, and then cast the backing layer solution and centrifuge for 10 minutes to allow the solution to fill the backing layer of the microneedle. Scrape off the excess solution, dry at 50°C for 20 hours, and then demold to obtain the microneedle.

[0113] The microneedles have good morphology and a mechanical strength of 4.67N / needle. The microneedles can be completely dissolved within 10 minutes after being inserted into the skin. Figure 6 The in vitro transdermal drug delivery efficiency of the microneedles was 35.03±2.84%. Figure 3(C: before dissolution, D: drug residue after dissolution) shows that the backing layer is more obviously red after the microneedles are dissolved, indicating that the drug migrates to the backing layer, resulting in a large amount of drug residue in the backing layer of the microneedles.

[0114] The confocal scanning results are as follows Figure 4 As shown in (D: microneedle tip layer scan E: microneedle backing layer scan F: 3D structure of microneedle), the red fluorescent dye diffuses from the needle body layer to the backing layer of the microneedle and cannot gather at the tip of the microneedle; when applied to the skin, only the needle tip dissolves the drug, and the drug in the backing layer cannot enter the skin, thus reducing the transdermal drug delivery efficiency of the microneedle.

[0115] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. In addition, several modifications and improvements may be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A high mechanical strength atomoxetine hydrochloride biphasic microneedle and a preparation method thereof, characterized in that: In terms of mass percentage, the biphasic microneedle includes the following ingredients: 1% to 25% active drug ingredients; 40% to 75% water-soluble polymers, such as pullulan, methyl vinyl ether-maleic anhydride and polymethyl vinyl ether-maleic acid copolymer series compounds, as the needle body layer matrix material, and the proportion of pullulan in the needle body layer matrix material is greater than 80%; 10% to 40% water-insoluble polymer as the backing layer, and the total amount is 100%.

2. The high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1, characterized in that: The microneedle body layer contains at least one water-soluble polymer with a content of 40% to 75%. The polymer can be pullulan (PL), polyvinyl alcohol (PVA), chitosan (CS) or a blend thereof.

3. The high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1 is characterized in that: the microneedle body layer contains at least one polymethyl vinyl ether-maleic anhydride copolymer, with a content of 2% to 20%. The type of polymethyl vinyl ether-maleic anhydride is PMVE / MAH (Gantrez AN-119), PMVE / MAH (Gantrez AN-139), PMVE / MAH (Gantrez AN-169) or a mixture thereof, preferably PMVE / MAH (Gantrez AN-119).

4. The high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1, characterized in that: the microneedle body layer contains a polymethyl vinyl ether-maleic acid copolymer, the content of which is 0% to 20%. The polymethyl vinyl ether-maleic acid copolymer series compound is of the type PVM / MA (Gantrez S-97), PVM / MA (Gantrez S-96) or a mixture thereof, preferably PVM / MA (Gantrez S-97).

5. The high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1, characterized in that: The microneedle backing layer contains at least one water-insoluble polymer, such as ethyl cellulose (EC), polystyrene (PS), polylactic acid (PLA), polylactic acid-co-glycolic acid (PLGA), or a mixture thereof, with a content of 10% to 40%, preferably 20%. The type of ethyl cellulose is EC N10, EC N20 or EC N50, preferably EC N20.

6. According to the high mechanical strength atomoxetine hydrochloride biphasic microneedle of claim 1, the microneedle body layer contains pullulan (PL), polymethyl vinyl ether-maleic anhydride copolymer (PMVE / MAH) and / or polymethyl vinyl ether-maleic acid copolymer (PVM / MA), and the proportion of pullulan (PL) in the microneedle body layer is greater than 80%.

7. The high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1, characterized in that: The content of the active pharmaceutical ingredient is 1-25%, and may be atomoxetine hydrochloride, propranolol hydrochloride, or diclofenac sodium.

8. The method for preparing the high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1, characterized in that The drying temperature ranges from 30°C to 65°C, preferably 40°C.

9. The high mechanical strength atomoxetine hydrochloride biphasic microneedle according to claim 1, characterized in that: The dual-phase microneedle is a cone, the height of the microneedle body is 300-1200 μm, and the bottom diameter of the dual-phase microneedle body is 100-500 μm.

10. The method for preparing the high mechanical strength atomoxetine hydrochloride biphasic microneedles according to claims 1-9, characterized in that: Dissolve PL, Gantrez AN-119, and Gantrez S-97 in water to prepare solutions, add active drugs to dissolve and mix, and obtain needle body layer matrix solution. Dissolve water-insoluble polymers, such as EC N20, in a suitable organic solvent to obtain a backing layer matrix solution. Cast the needle body layer solution, centrifuge to fill the needle body layer part of the microneedle, and then cast the backing layer solution, centrifuge to fill the backing layer part of the microneedle. Scrape off the excess solution, dry and demold, and obtain a dual-phase microneedle.