Anti-infection medical application for skin wound and preparation method of anti-infection medical application

The polyurethane film is treated with 3D micro-nano laser etching technology and combined with antibiotics to form an efficient antibacterial dressing, which solves the problems of insufficient moisture permeability and antibacterial performance of existing antibacterial dressings and achieves effective protection and healing of skin wounds.

CN118767199AActive Publication Date: 2024-10-15TONGJI HOSPITAL ATTACHED TO TONGJI MEDICAL COLLEGE HUAZHONG SCI TECH

Patent Information

Application Number
CN202411012343.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Existing antibacterial wound dressings have deficiencies in moisture permeability, softness, and antibacterial properties, making it difficult to effectively prevent skin wound infections and may lead to the emergence of antibiotic-resistant pathogens.

Method used

The polyurethane film is processed using 3D micro-nano laser etching technology to form micro-nano structures, which enhances the drug-loading capacity of antibiotics, and is combined with antibiotics such as β-lactams and polycyclic lactones to form an efficient antibacterial dressing.

Benefits of technology

It can significantly enhance the antibacterial effect, effectively inhibit bacterial infection and inflammatory response, accelerate wound healing without affecting the original mechanical properties and moisture permeability of the polyurethane film, and has the advantages of customized drug release process and high energy saving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767199A_ABST
    Figure CN118767199A_ABST
Patent Text Reader

Abstract

The invention discloses a skin wound anti-infection medical application and a preparation method thereof, and relates to the field of biomedical materials and wound care. The medical application comprises a polyurethane film and an antibiotic loaded on the polyurethane film. The preparation method comprises the following steps: step 1, carrying out etching processing on a polyurethane film by adopting a 3D micro-nano laser etching instrument; and step 2, incubating by using antibiotics after etching, and storing at low temperature to obtain the medical application. The prepared novel application has a good antibacterial effect on the basis of not influencing the original mechanical property and moisture permeability of the polyurethane film. According to the invention, bacterial infection and inflammatory response of rat skin wounds can be effectively inhibited, and an important treatment reference is provided for rehabilitation of clinical skin soft tissue wounds, pollution and other chronic skin diseases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of biomedical materials and wound care, and in particular to a medical dressing for resisting infection of skin wounds and a preparation method thereof. Background Art

[0002] Skin trauma is extremely common in daily life, whether it is a minor abrasion or a deep laceration, it may cause infection of varying degrees. As the first line of defense of the human body, once the integrity of the skin is damaged, especially under conditions of chronic pollution, these wounds are very susceptible to bacterial infection and induce persistent inflammatory responses, which not only delay the healing process, but also in severe cases may lead to sepsis and its related high medical burden.

[0003] The occurrence of infection after skin trauma involves multiple links. First, microorganisms enter the tissue through the damaged skin barrier and cause an inflammatory response. These microorganisms may come from the surrounding environment, contaminated objects, or the patient's own skin flora. Secondly, the host's immune response plays a vital role in controlling infection. However, when the immune response is insufficient or excessive, it may lead to the spread or aggravation of the infection. In addition, there are many types of infections caused by skin trauma, including but not limited to suppurative infections, fungal infections, etc. Supurative infections are mainly manifested by local redness, swelling, pain, fever and other symptoms. In severe cases, sepsis or septicemia may occur. Fungal infections are more common in patients with humid environments or long-term use of antibiotics, manifested as local itching, erythema, desquamation, etc. In clinical applications, in order to prevent excessive inflammatory response, bacterial infection or self-infection leading to treatment failure, it is usually necessary to use medical dressings on local wounds in combination with systemic anti-inflammatory and antibacterial drugs, which may lead to the generation of antibiotic-resistant pathogens.

[0004] As a medical material, dressings are used to cover wounds to isolate the external environment and provide a suitable environment for skin trauma to heal. Data on the global medical dressing market size show that the total size of the global wound dressing market in 2022 is US$13.7 billion, of which high-end dressings account for 54.47% and the market size is US$7.46 billion. It is estimated that by 2030, the global wound dressing market will reach US$19 billion, with a compound annual growth rate of 4.14%, and the high-end dressing market size is expected to reach US$10.6 billion, with a compound annual growth rate of 4.46%. The competition pattern of the domestic medical dressing industry shows that the market is mainly dominated by domestic manufacturers, mainly traditional products, while foreign manufacturers are mainly concentrated in the high-end wound dressing market, including Johnson & Johnson, 3M, Smith & Nephew, Medtronic, Coloplast, Convid, etc. Therefore, the Chinese and even global markets are in urgent need of and in short supply of advanced, cost-effective and high-end medical dressings for skin trauma (including infected trauma).

[0005] At present, most clinically available antibacterial wound dressings increase the antibacterial effect by spraying heavy metal elements on the surface of traditional dressings such as cotton fabrics and gauze strips, but their moisture permeability, softness and waterproofness are not ideal. Compared with traditional dressings, polyurethane medical dressings have obvious advantages in terms of sterility, transparency, softness and comfort, moisture permeability, water resistance and biocompatibility. Therefore, polyurethane dressings are widely used in clinical care for various non-chronic wounds and wound protection after specific surgeries or treatments. However, polyurethane medical dressings have certain deficiencies in hydrophilicity and antibacterial properties. Therefore, it is particularly important for us to develop new polyurethane medical dressings that promote wound healing and anti-infection functions.

[0006] Laser processing, with its highly precise technical characteristics, gives the film material a specific patterning capability within the processing area. This function is achieved by precisely editing the laser processing parameters, adjusting the processing path, or combining the use of masks, so that the film can achieve selective drug loading according to the patient's wound inflammation during the drug loading process. Laser processing is not limited to the physical processing of the film, it can also affect the drug adhesion ability by changing the surface chemical properties of the film. This means that by adjusting the laser processing parameters, the drug loading capacity of the film can be effectively regulated to achieve more precise and personalized treatment. The micro-nanostructure formed on the surface of the film is also believed to significantly affect the adhesion between the dressing and the antibiotic, thereby achieving passive control of the drug release rate. The application of this technology provides new ideas and methods for wound treatment and drug release in the medical field. This new dressing can not only be used for clinical treatment, but also has a wide range of application prospects in outdoor medical care. With the increasing demand for lightweight, intelligent and comfortable outdoor equipment, wound dressings will become particularly important for outdoor workers to quickly stop bleeding and prevent infection. Summary of the invention

[0007] In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a medical dressing for skin wounds to resist infection and a preparation method thereof. The new dressing prepared by the present invention can have a good antibacterial effect without affecting the original mechanical properties and moisture permeability of the polyurethane film. The present invention can effectively inhibit bacterial infection and inflammatory response of rat skin wounds, and provides an important treatment reference for clinical skin soft tissue trauma, pollution and other chronic skin disease rehabilitation.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] The invention provides a medical dressing for resisting infection of skin wounds. The medical dressing comprises a polyurethane film and an antibiotic loaded on the polyurethane film.

[0010] Preferably, the polyurethane film is made of an ultra-thin transparent material, and its average film thickness is 30-100 μm.

[0011] Preferably, the drug loading of the antibiotic on the polyurethane film is 0.0625-0.625 μg / mm 2 .

[0012] Preferably, the tensile strength of the polyurethane film is 5-15 MPa, the elongation at break is 400-700%, and the Young's modulus is 5-15 MPa.

[0013] Preferably, the moisture permeability of the polyurethane film is 200-400g / (m 2 ·24h).

[0014] Preferably, the antibiotic is selected from the group consisting of β-lactam antibiotics, macrolide antibiotics, aminoglycoside antibiotics, tetracycline antibiotics, lincomycin antibiotics, chloramphenicol antibiotics, polypeptide antibiotics, sulfonamides and quinolones.

[0015] Further preferably, β-lactam antibiotics include penicillins, cephalosporins, other β-lactams, β-lactamase inhibitors and their combination preparations; macrolide antibiotics include erythromycin, roxithromycin, azithromycin, clarithromycin, etc.; aminoglycoside antibiotics include streptomycin, gentamicin, ethimicin, etc.; tetracycline antibiotics include tetracycline, oxytetracycline, doxycycline, etc.; lincomycin antibiotics include lincomycin and clindamycin; chloramphenicol antibiotics include chloramphenicol and thiomycin; polypeptide antibiotics include vancomycins such as vancomycin, norvancomycin, etc., polymyxins such as polymyxin B, bacitracin of bacitracin, etc.; sulfonamides and quinolones include sulfonamides, norfloxacin, levofloxacin, moxifloxacin, etc.

[0016] The present invention also provides a method for preparing a medical dressing for skin wounds to resist infection, the preparation method comprising:

[0017] Step 1: With the help of a 3D micro-nano laser etching instrument, the polyurethane film is etched by using a point scanning patterned continuous or intermittent laser etching method;

[0018] Step 2: After etching, incubate with antibiotics and store at low temperature to obtain the medical dressing.

[0019] Preferably, in step 1, the continuous laser etching method comprises:

[0020] The untreated polyurethane film is fixed on a ceramic plate substrate, and the focal length is adjusted so that the laser focuses on the middle layer of the polyurethane film; then an ultrafast laser is used to scan 1-2 times at a speed of 0.05-5m / s, a power of 500-1500mW and a spacing of 10-80μm to form the desired pattern on the polyurethane film.

[0021] Preferably, in step 1, the interval laser etching method includes:

[0022] The untreated polyurethane film is fixed on the ceramic plate substrate, and the focal length is adjusted so that the laser focuses on the middle layer of the polyurethane film; then, an ultrafast laser is used to perform X-axis linear scanning at a speed of 0.1-0.5m / s, a power of 800-1200mW and a spacing of 10-20μm. After waiting for 0-4 minutes for the bubbles generated by etching to disappear, the laser is moved 5-10μm along the Y axis for another laser etching to form the desired pattern on the polyurethane film.

[0023] Further preferably, the heat accumulation time in the interval laser etching method is 1-3 minutes.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention has successfully pioneered a controlled drug release technology based on ultrafast laser surface treatment of polyurethane films. By finely controlling laser processing parameters (such as processing power, scanning line spacing, intermittent scanning mode and other process parameters), the customized transformation of the micro-nano structure on the surface of the polyurethane film has been successfully achieved, and the drug loading can be adjusted and optimized. The beneficial effects of this technology include customized drug release process, enhanced drug loading effect, maintenance or improvement of film performance, broadening application fields and high efficiency and energy saving. These advantages make this technology have broad application prospects and potential in the fields of medicine, biology, and medicine. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The ultrastructure of the polyurethane dressing combined with antibiotics assisted by 3D micro-nano laser etching technology; Figure 1 a in the figure is the film thickness characterization of the polyurethane film (SEM image), Figure 1 b is the surface morphology of the polyurethane film with high drug loading (SEM image). Figure 1 Figure c is the surface morphology of the polyurethane film with low drug loading (SEM image).

[0027] Figure 2 Stress-strain curve of polyurethane dressing assisted by 3D micro-nano laser etching technology with antibiotic incorporation.

[0028] Figure 3 The moisture permeability of polyurethane dressing combined with antibiotics assisted by 3D micro-nano laser etching technology.

[0029] Figure 4 The effect of 3D micro-nano laser intensity on the drug loading of polyurethane dressing; Figure 4 a and d in the figure are the two-dimensional plane and three-dimensional fluorescence confocal images with a laser scanning power of 730mW, respectively. Figure 4 b and e in the figure are the two-dimensional plane and three-dimensional fluorescence confocal images with a laser scanning power of 790mW, respectively. Figure 4 Figures c and f are the two-dimensional and three-dimensional fluorescence confocal images, respectively, with a laser scanning power of 850 mW.

[0030] Figure 5 The effect of 3D micro-nano laser etching spacing on the drug loading of polyurethane dressings; Figure 5 a in the figure is a fluorescence confocal image with a scanning line spacing of 22 μm. Figure 5 b in the figure is a fluorescence confocal image with a scanning line spacing of 20 μm. Figure 5 c in the figure is a fluorescence confocal image with a scanning line spacing of 18 μm. Figure 5 d in the figure is a fluorescence confocal image with a scanning line spacing of 16 μm. Figure 5 e in the figure is a fluorescence confocal image with a scanning line spacing of 14 μm. Figure 5 f in the figure is a fluorescence confocal image with a scanning line spacing of 12 μm.

[0031] Figure 6 The effect of 3D micro-nano laser etching interval on the drug loading of polyurethane dressing; Figure 6 a in the figure is a continuously scanned fluorescence confocal image. Figure 6 b in the figure is a fluorescence confocal image with an interval scan of 0 minutes. Figure 6 The c in the figure is a fluorescence confocal image scanned at intervals of 1 minute. Figure 6 The d in the figure is a fluorescence confocal image scanned at intervals of 2 minutes. Figure 6 The e in the figure is a fluorescence confocal image scanned at intervals of 3 minutes. Figure 6 The f in the figure is a fluorescent confocal image scanned at intervals of 4 minutes.

[0032] Figure 7 The drug loading capacity of polyurethane dressing combined with antibiotics assisted by 3D micro-nano laser etching technology is improved.

[0033] Figure 8 The degree of bacterial inhibition of polyurethane dressing combined with antibiotics assisted by 3D micro-nano laser etching technology in vitro; Figure 8 a in the figure is a physical picture of the antibacterial zone of the unprocessed and un-drug loaded polyurethane dressing. Figure 8 Figure b is a physical picture of the antibacterial zone of the unprocessed polyurethane dressing directly loaded with drugs. Figure 8Figure c is a physical picture of the antibacterial zone of the drug-loaded polyurethane dressing after laser processing. Figure 8 The d in the figure is the statistical diameter of the inhibition zone of the above three dressings.

[0034] Fig. 9 The effect of 3D micro-nano laser etching technology on the healing of rat skin wounds using an antibiotic-combined polyurethane dressing. Fig. 9 a in the figure is the healing effect of unprocessed and un-drug-loaded polyurethane dressing on rat skin wounds. Fig. 9 b in the figure is the effect of unprocessed polyurethane dressing directly loaded with drugs on the healing of rat skin wounds. Fig. 9 Figure c shows the effect of laser-processed drug-loaded polyurethane dressing on the healing of rat skin wounds. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with the accompanying drawings, embodiments and experimental examples. Of course, the protection scope of the present invention is not limited to the following embodiments. Professional and technical personnel in the field can understand that various changes and modifications can be made to the present invention without departing from the spirit of the present invention. The present invention generally and / or specifically describes the materials and test methods used in the experiment. Although many materials and operating methods used to achieve the purpose of the present invention are well known in the art, the present invention is still described as detailed as possible here. The following examples further illustrate the present invention, rather than limiting the present invention. Any equivalent transformation that is only formal and not substantial based on the concept of the present invention should be regarded as the scope of the technical solution of the present invention.

[0036] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0037] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0038] The 3D micro-nano laser etching instrument used in the present invention is provided by the team of Professor Xiong Wei of Wuhan National Research Center for Optoelectronics, Huazhong University of Science and Technology. The device outputs ultrashort pulse lasers with a wavelength covering 266-2000nm, a frequency of 1-2000kHz, and a pulse width of 15ps; the maximum scanning speed of the galvanometer can reach 75m / s; and the maximum average power of the laser can reach 100W.

[0039] Skin and soft tissue trauma is often accompanied by acute and chronic infections, which seriously hinder the repair process of skin and soft tissue, and may cause serious systemic infection and spread, endangering life. In order to solve this problem, the present invention utilizes the polyurethane substrate layer with good biocompatibility and physical properties to ensure the safety and comfort of the dressing. After 3D micro-nano laser etching, the outer layer of the polyurethane still maintains good moisture permeability and waterproofness, protecting the wound from external pollution, while allowing water to evaporate and avoiding the creation of an overly humid environment. 3D micro-nano laser etching technology enhances the antibiotic loading of the polyurethane film, provides effective antibacterial effects, can prevent wound infection, and accelerate the healing process. The preparation method of the wound dressing is simple, easy to mass produce, and has good market application prospects.

[0040] The present invention will be further described below in conjunction with the embodiments.

[0041] Example 1

[0042] The continuous laser etching process includes: fixing the untreated polyurethane film on the ceramic plate substrate, and adjusting the focal length so that the laser focuses on the middle layer of the film. Then use an ultrafast laser to scan 1-2 times at a speed of 0.05-5m / s, a power of 500-1500mW and a spacing of 10-80μm to form linear, tic-tac-toe or checkerboard shapes. Then incubate with clindamycin-FITC fluorescein drug diluted in PBS solution and store at 4°C for two hours. Finally, use a Nikon Ni-E fluorescence confocal microscope to observe the drug loading, and use FIJI software to obtain a three-dimensional fluorescence intensity image. The effect of laser power on the drug loading of polyurethane patch is as follows: Figure 4 As shown in the figure, by adjusting the processing power parameters, the drug loading is increased by 18 times compared with the unprocessed area, and on this basis, it is increased by 42 times by adjusting the line spacing, as shown in the figure. Figure 5 and 7 shown.

[0043] Example 2

[0044] The interval laser etching process includes: fixing an untreated or oxygen plasma treated polyurethane film on a ceramic plate substrate, and adjusting the focal length so that the laser focuses on the middle layer of the film. Then use an ultrafast laser to perform X-axis linear scanning at a speed of 0.1-0.5m / s, a power of 800-1200mW and a spacing of 10-20μm. After waiting for the bubbles generated by etching to disappear at an interval of 0-4 minutes, move 5-10μm along the Y axis for laser etching again. Then incubate with clindamycin-FITC fluorescent drug diluted with PBS solution and store at 4°C for two hours. Finally, use a Nikon Ni-E fluorescence confocal microscope to observe the drug loading, and use FIJI software to obtain a three-dimensional fluorescence intensity image. This interval scanning method can avoid ablation caused by heat accumulation and achieve a larger effective drug loading (see Figure 6 ).like Figure 6 As shown, the heat accumulation time is 1-3 minutes. Figure 7 As shown, Example 2 can increase the drug loading by 53 times through the intermittent scanning method, and through the prior plasma cleaning treatment, the drug loading of the dressing can be increased by a total of 61 times.

[0045] Example 3

[0046] The polyurethane dressing prepared in Example 1 is used for illustration. The cross section of the dressing film is observed using SEM, and the average thickness of the dressing film is about 30-100 μm (see Figure 1 The processed polyurethane film with high drug loading is characterized by a rough area with a width of about 20 μm (see Figure 1 b); the polyurethane film with low drug loading after processing is characterized by obvious grooves (see Figure 1 c) in.

[0047] Example 4

[0048] The polyurethane dressing with the maximum drug loading prepared in Example 2 was used for illustration. The mechanical properties of the polyurethane film before and after processing were tested using a single-column tabletop material tensile test system. Samples were cut by cutting to produce dumbbell-shaped strips with a length of 40 mm, a width of 30 mm, and an inner width of 20 mm. Tensile tests were performed at a tensile rate of 15 mm / min. Five sets of parallel samples were set for each film strip (see Figure 2 PU-U represents unprocessed polyurethane film; PU-U-AL represents unprocessed polyurethane film incubated with drug loading; PU-S-AL represents processed and incubated polyurethane film loaded with drug. The mechanical properties of the polyurethane film are as follows Figure 2 As shown, its tensile strength is 5-15 MPa, its elongation at break is 400-700%, and its Young's modulus is 5-15 MPa.

[0049] Example 5

[0050] The polyurethane dressing with the maximum drug loading prepared in Example 2 is used for illustration. The moisture permeability analysis of the polyurethane film adopts the provisions of GB / T 12704.1-2009. An equal amount of desiccant CaCl2 is added to the moisture permeable cup, and the mouth of the cup is covered with a polyurethane film, which is sealed to ensure that water vapor can only be transmitted through the polyurethane film. The moisture permeable cup is then placed in a constant temperature and humidity chamber. The program is set to 23°C and a relative humidity of 50%. After 24 hours, the mass of CaCl2 in the moisture permeable cup is measured. Figure 3 The moisture permeability of the polyurethane film before and after processing is shown in Figure 2. PU-U represents the unprocessed polyurethane film; PU-U-AL represents the unprocessed polyurethane film incubated with drug loading; PU-S-AL represents the processed and drug-loaded polyurethane film. Figure 3 As shown, its moisture permeability is 200-400 grams per square meter per 24 hours.

[0051] Example 6

[0052] The polyurethane dressing with the maximum drug loading prepared in Example 2 is used for illustration. The antibacterial experiment is carried out using Staphylococcus aureus (S. aureus). The culture medium is weighed according to the ratio of 100ml deionized water: 0.5g yeast extract: 1g tryptone: 0.58g sodium chloride, and is sterilized at high pressure for use. Take the frozen Staphylococcus aureus in a -40℃ refrigerator, thaw at room temperature, absorb the bacterial liquid and add it to the culture solution in a ratio of 1:1000 and shake it fully, and put it into a 37℃ constant temperature shaking box for culturing 8-10h. Take a sterile agarose plate and evenly spread the bacterial suspension on the surface of the plate. Put the coated plate into a constant temperature incubator, set the incubator temperature to 37℃, and the incubation time is 24 hours.

[0053] Cut the polyurethane film into 1cm*1cm pieces and soak them in medical alcohol for 15min before drying. Paste the test sample on the Staphylococcus aureus plate, cover the plate and place it in a 37℃ constant temperature incubator for 24h, 48h, and 72h. Use a ruler to count the diameter of the inhibition zone at each time point (see Figure 8 PU-U represents unprocessed polyurethane film; PU-U-AL represents unprocessed polyurethane film incubated with drug; PU-S-AL represents processed and incubated polyurethane film loaded with drug. The degree of bacterial inhibition of polyurethane dressing combined with antibiotics in vitro by 3D micro-nano laser etching technology Figure 8 As shown, the diameter of the inhibition zone of Staphylococcus aureus in the PU-S-AL group was significantly larger than that in the PU-U-AL and PU-U groups.

[0054] Example 7

[0055] The polyurethane dressing with the maximum drug loading prepared in Example 2 is used for illustration. The main purpose of the animal experiment is to evaluate the effects of different dressings on wound inflammatory response by establishing an infectious wound model. The experiment selected SD rats as experimental subjects, and used Staphylococcus aureus as the pathogen of traumatic wounds. Staphylococcus aureus was cultured in LP liquid culture medium to the logarithmic phase, and the concentration of the bacterial solution was adjusted for later use. The animals were anesthetized, the skin was prepared, and the back wound was prepared. It was appropriate to open 2 cm on both sides of the back spine, 1x1 cm 2 Pocket-shaped wound, contacting the dermis. Bacterial liquid was dripped into the wound to create a model.

[0056] The polyurethane film was cut into 2cm*2cm samples and soaked in medical alcohol for 15 minutes and then dried. The test sample was attached to the wound of the rat and fixed. After standing for 24 hours, the purulent secretion of the rat skin wound was observed ( Fig. 9 ). PU-U represents unprocessed polyurethane film; PU-U-AL represents unprocessed polyurethane film incubated with drug; PU-S-AL represents processed and incubated polyurethane film loaded with drug. The arrow indicates the location of purulent secretion under the dressing. 3D micro-nano laser etching technology assisted antibiotic-combined polyurethane dressing to inhibit skin wound infection in rats Fig. 9 As shown, after 24 hours of static rest, the purulent secretions on the skin wounds of rats in the PU-S-AL group were significantly reduced compared with those in the PU-U-AL and PU-U groups.

[0057] Results: The present invention successfully constructs a novel polyurethane wound dressing with antibiotics combined with 3D micro-nano laser etching technology, overcoming the shortcomings of the prior art. The polyurethane dressing material includes ultra-thin transparent polyurethane processed by 3D micro-nano laser etching and antibiotics.

[0058] In summary, the present invention uses polyurethane with excellent biocompatibility and physical properties as a substrate to ensure the safety and comfort of the dressing. The outer layer of polyurethane treated by 3D micro-nano laser etching technology not only maintains good moisture permeability and waterproofness, protects the wound from contamination, but also allows water to evaporate to avoid excessive wetting of the wound. In addition, this technology also enhances the antibiotic loading capacity of the polyurethane film, effectively prevents wound infection and accelerates healing. The preparation process of the wound dressing is simple, suitable for large-scale production, and has good market application potential.

[0059] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A medical dressing for skin wounds to resist infection, characterized in that: The medical dressing comprises a polyurethane film and an antibiotic loaded on the polyurethane film.

2. The medical dressing for skin wound infection prevention according to claim 1, characterized in that: The polyurethane film is an ultra-thin transparent material, and its average film thickness is 30-100 μm.

3. The medical dressing for skin wound infection prevention according to claim 1, characterized in that: The antibiotic loading on the polyurethane film is 0.0625-0.625 μg / mm 2 .

4. The medical dressing for skin wound infection prevention according to claim 1, characterized in that: The tensile strength of the polyurethane film is 5-15 MPa, the elongation at break is 400-700%, and the Young's modulus is 5-15 MPa.

5. The medical dressing for skin wound infection prevention according to claim 1, characterized in that: The moisture permeability of the polyurethane film is 200-400g / (m 2 ·24h).

6. The medical dressing for skin wound infection prevention according to claim 1, characterized in that: The antibiotics are selected from the group consisting of β-lactam antibiotics, macrolide antibiotics, aminoglycoside antibiotics, tetracycline antibiotics, lincomycin antibiotics, chloramphenicol antibiotics, polypeptide antibiotics, sulfonamides and quinolones.

7. A method for preparing a medical dressing for skin wound infection according to any one of claims 1 to 6, characterized in that: The preparation method comprises: Step 1: With the help of a 3D micro-nano laser etching instrument, the polyurethane film is etched by using a point scanning patterned continuous or intermittent laser etching method; Step 2: After etching, incubate with antibiotics and store at low temperature to obtain the medical dressing.

8. The method for preparing the medical dressing for skin wound infection resistance according to claim 7, characterized in that: In step 1, the continuous laser etching method includes: The untreated polyurethane film is fixed on a ceramic plate substrate, and the focal length is adjusted so that the laser focuses on the middle layer of the polyurethane film; then an ultrafast laser is used to scan 1-2 times at a speed of 0.05-5m / s, a power of 500-1500mW and a spacing of 10-80μm to form the desired pattern on the polyurethane film.

9. The method for preparing the medical dressing for skin wound infection resistance according to claim 7, characterized in that: In step 1, the interval laser etching method includes: The untreated polyurethane film is fixed on the ceramic plate substrate, and the focal length is adjusted so that the laser focuses on the middle layer of the polyurethane film; then, an ultrafast laser is used to perform X-axis linear scanning at a speed of 0.1-0.5m / s, a power of 800-1200mW and a spacing of 10-20μm. After waiting for 0-4 minutes for the bubbles generated by etching to disappear, the laser is moved 5-10μm along the Y axis for another laser etching to form the desired pattern on the polyurethane film.

10. The method for preparing the medical dressing for skin wound infection resistance according to claim 9, characterized in that: The heat accumulation time in the interval laser etching method is 1-3 minutes.

Citation Information

Patent Citations

  • Polyurethane film as well as preparation method and application thereof

    CN113005773A

  • Antibacterial film using inorganic bactericides dispersions and making process of antibacterial film

    KR101007180B1

Cited By

  • Preparation method of medicine carrying layer of medical application and medical application

    CN120346186A