Liquid-containing coating and preparation method thereof

By applying a composite coating of nano-silica and ethyl silicate on the cavity mirror lens, combined with a low surface energy liquid film, a pore frame structure is formed, which solves the problem of easy fogging and contamination of the cavity mirror lens and achieves remarkable results. Excellent anti-fog and anti-pollution effect, and extended service life.

CN118767220APending Publication Date: 2024-10-15SHAOXING UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410761216.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Endoscopic lenses are prone to fogging and contamination, which blocks the surgical field of vision and increases surgical risks and infection rates. Existing anti-fog coatings cannot effectively solve the problem of lens contamination.

Method used

A method of preparing a liquid-containing coating is used, and a composite coating of nano-silica and ethyl silicate is combined with a low surface energy liquid film to form a pore framework structure to achieve anti-fogging and anti-pollution effects. The method includes uniform stirring of nano-silica and ethyl silicate, hydrolysis of ethyl cellulose, soaking in trichloromethylsilane, infiltration of polyvinylpyrrole and spray treatment of distilled water to form a porous structured silicone coating. layer, and pour medical lubricant into the composite coating to form a liquid film.

Benefits of technology

It significantly improves the anti-fog and anti-pollution effect of the cavity mirror lens, prolongs its service life, and can quickly replenish the protective fluid when worn to prevent the flow loss of the protective fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004891122310000101
    Figure BDA0004891122310000101
Patent Text Reader

Abstract

The invention relates to the technical field of medical auxiliary instruments, in particular to a liquid-containing coating and a preparation method thereof.The method comprises the steps that nano-silica serves as a raw material to form a silica frame, a silica precursor is deposited in pores of the silica frame, and a composite coating is formed after hydrolysis and polycondensation; and finally, medical lubricating liquid is poured into the composite coating to obtain the liquid-containing coating. The defects that an existing endoscope lens is prone to atomization and pollution are overcome, the composite coating is matched with the low-surface-energy liquid film to form a liquid-containing layered structure, and the anti-atomization and anti-pollution effects are achieved and are quite remarkable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical auxiliary equipment, and in particular to a liquid-containing coating and a preparation method thereof. Background Art

[0002] Laparoscopic minimally invasive surgery uses a laparoscope lens to take real-time images of the surgical site. The surgeon analyzes and judges the real-time images and uses tiny instruments to perform local surgery. This laparoscopic minimally invasive surgery has the technical characteristics of less trauma, faster recovery, and faster rehabilitation. The laparoscope lens is equivalent to the surgeon's eyes, and a certain degree of clarity needs to be maintained during the operation. However, when the lens is fogged or contaminated, the surgeon's field of vision is blocked and the surgical site cannot be seen clearly, which seriously affects the progress of the operation and may even cause the operation to be interrupted until it is cleaned up before continuing the operation. However, the repeated removal and insertion of the laparoscope lens will not only affect the progress of the operation, but also increase the risk of surgery and the chance of infection. Therefore, the fogging and contamination of the laparoscope lens are technical difficulties that need to be solved urgently.

[0003] The conventional solution to the fogging of laparoscope lenses is to apply an anti-fog coating. However, the material requirements for anti-fog coatings are very high and the cost is extremely high. At the same time, anti-fog coatings cannot solve the problem of lens contamination. Therefore, laparoscope lenses provide a solution to solve both lens fogging and lens contamination. Summary of the invention

[0004] In view of the problems in the prior art, the present invention provides a method for preparing a liquid-containing coating. The method prepares a coating structure with a silicon-oxygen system as a pore frame, which solves the defects of the existing laparoscope lens that is easy to fog and contaminate. The composite coating is combined with a low surface energy liquid film to form a liquid-containing layered structure, which has the effect of preventing fogging and contamination, and the effect is quite significant.

[0005] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0006] A method for preparing a liquid-containing coating comprises the following steps:

[0007] Step 1, adding nano-silicon dioxide and ethyl silicate to ether and stirring evenly, filtering and drying to obtain biofilm nano-silicon dioxide, wherein the particle size of the nano-silicon dioxide is 10-100nm, the molar ratio of the nano-silicon dioxide to the ethyl silicate is 10-15:1, the concentration of the ethyl silicate in the ether is 5-10g / L, the stirring speed for uniform stirring is 100-300r / min, and the drying temperature is 40-50°C; this step utilizes the solubility of ethyl silicate in ether to form a homogeneous dispersion, and in this dispersion system, ethyl silicate directly acts on the surface of the nano-silicon dioxide to form a stable dispersion liquid, and during the drying process, the ether is converted into steam and directly removed to form nano-silicon dioxide containing an ethyl silicate liquid film;

[0008] Step 2, allowing the biofilm nano-silica to stand for 10-20 minutes, then adding it to the ethyl cellulose dispersion, stirring to obtain a mixed solution, spraying the mixed solution and sintering it at a constant temperature to obtain a silicon oxygen framework; the atmosphere of the standing is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9-10:1, and the temperature is 30-60°C; the ethyl cellulose dispersion is an ethanol solution of ethyl cellulose, and the concentration of the ethyl cellulose in ethanol is 10-20g / L, the mass ratio of the biofilm nano-silica to ethyl cellulose is 3:2-3, the stirring speed of the stirring is 300-500r / min, and the spray amount of the spray deposition is 0.1-0.3mL / cm 2 , the temperature is 50-70℃; the temperature of the constant temperature sintering is 200-230℃; this step uses the atmosphere containing water vapor to in-situ hydrolyze the ethyl silicate on the surface of the nano-silica to form a tetrahydroxy structure of silicate, that is, the surface of the nano-silica is rich in silanol; when the ethyl cellulose dispersion is mixed with the hydrolyzed biofilm-forming silicate, the hydrolyzed biofilm-forming silicate itself has the characteristic of being insoluble in ethanol, and the ethyl cellulose can be completely dissolved in water to play a dispersing role. Therefore, in the entire mixed solution, ethyl cellulose is used as a dispersant to form a homogeneous dispersion of the hydrolyzed biofilm-forming silicate; liquid film deposition is formed during the spray deposition process, and an ethyl cellulose-hydrolyzed nano-silica composite film is formed under temperature conditions. During the constant temperature sintering process, the ethyl cellulose is decomposed and removed in situ, and the hydrolyzed biofilm-forming silicate is polycondensed to form a silicon-oxygen framework with a porous structure. The silicic acid hydroxyl groups on the surface of the nano-silica form a polycondensation bond with the adjacent materials, and at the same time, the active hydroxyl groups on the surface of the nano-silica itself form a bond with the silicic acid hydroxyl groups to form a stable connection;

[0009] Step 3, adding trichloromethylsilane to ether and stirring evenly to form a dissolving solution, then immersing the silicon oxygen frame in the dissolving solution and stirring rapidly, taking it out and airing it to half dry, drying it and standing it to obtain a coated silicon oxygen frame, wherein the concentration of the trichloromethylsilane in the ether is 100-300g / L, the stirring speed for uniform stirring is 100-200r / min, the speed of rapid stirring is 800-1000r / min, the drying temperature is 20-30°C, and the atmosphere for standing is nitrogen The step is to form a low-concentration silicon ether liquid by utilizing the solubility of trichloromethylsilane in ether, and then penetrate the silicon ether liquid into the surface of the silicon-oxygen framework by immersion and rapid stirring, and form a surface liquid film of trichloromethylsilane under the action of drying and baking. During the standing process, the water vapor in the standing atmosphere and the trichloromethylsilane are hydrolyzed in situ to form a liquid film of surface hydrolysis product;

[0010] Step 4, adding polyvinyl pyrrolidone to methanol and stirring evenly to dissolve, then slowly adding ethyl silicate and methyl trimethoxy silane and rapidly dispersing until completely dissolved to form a mixed coating solution, then uniformly coating the mixed coating solution on the coated silicon oxygen frame, and scraping off the excess to obtain a composite prefabricated coating, wherein the concentration of the polyvinyl pyrrolidone in methanol is 500-700 g / L, the stirring speed is 200-300 r / min, the mass ratio of the ethyl silicate to the methyl trimethoxy silane is 5-8:1, the mass ratio of the polyvinyl pyrrolidone to the ethyl silicate is 1:0.8-1.3, and the rapid dispersion is Ultrasonic dispersion or mechanical stirring; the temperature used for the homogeneous coating is 5-10°C, and the homogeneous coating is repeated to ensure that the mixed coating liquid completely penetrates into the coated silicon oxygen framework; this step utilizes the solubility of polyvinyl pyrrolidone in methanol to form a viscous methanol solution, and adds ethyl silicate and methyltrimethoxysilane to form a good dissolution system to obtain a mixed coating liquid with a certain viscosity; the mixed coating liquid is repeatedly coated to completely penetrate into the pore structure of the coated silicon oxygen framework to achieve an excellent filling effect, and the low temperature environment of the coating can ensure that the coating layer on the surface of the coated silicon oxygen framework remains stable;

[0011] Step 5: Spray distilled water onto the surface of the composite prefabricated coating, and keep it at a constant temperature for 2-3 hours, heat it up and sinter it for 20-30 minutes, then cool it to room temperature and put it into an ethanol aqueous solution, stir and wash it several times, and dry it to obtain a composite coating. The spraying speed is 1-3mL / cm 2 , the temperature is 10-20 ℃, the temperature of constant temperature static is 100-110 ℃, the temperature of heating sintering is 180-200 ℃; the volume proportion of ethanol in the ethanol aqueous solution is 70-75%, the stirring speed of the stirring washing is 100-300r / min, and the temperature of the drying is 1120-150 ℃; this step uses distilled water to spray on the surface of the composite prefabricated coating, and uses the water absorption of polyvinyl pyrrolidone in the composite prefabricated coating to absorb the distilled water and homogeneously penetrate into the coating, and the methyltrimethoxysilane and ethyl silicate in the coating form an in-situ hydrolysis reaction, and the temperature during the constant temperature static process is adjusted. The in-situ polycondensation reaction is formed under the interval of the polyvinyl pyrrolidone solid, which plays a role in the polycondensation connection structure of the silicon-oxygen material. The polyvinyl pyrrolidone melts in the process of temperature rise sintering to form a viscous residual dynamic second fixation of the residual silicon-oxygen material, thereby obtaining a silicon-oxygen material with multiple pore structures; when the coating after the temperature rise sintering treatment is placed in an ethanol aqueous solution for stirring and washing, the solubility of the polyvinyl pyrrolidone itself ensures that it can be quickly dispersed in the ethanol aqueous solution, and the removal effect is achieved in the subsequent washing, thereby obtaining a silicon-oxygen structure with multiple pore structures, and the residual liquid is taken out in the drying process to obtain a clean composite coating;

[0012] Step 6, injecting a medical lubricating liquid into the composite coating and removing excess medical lubricating oil to obtain a liquid-containing coating, wherein the viscosity of the medical lubricating liquid is 10-1000 cSt, and the medical lubricating oil is injected by a negative pressure method; this step utilizes a negative pressure method to inject the composite coating until the pore structure of the entire composite coating is filled and a liquid film is formed on the surface of the composite coating.

[0013] The total thickness of the liquid-containing coating prepared by the above method is 450-600 μm, and the thickness of the liquid film is 120-150 nm.

[0014] The composite coating in the liquid-containing coating includes macropores with a pore size of 100-300 μm and micropores with a pore size of 0.1-0.4 μm.

[0015] It can be seen from the above description that the present invention has the following advantages:

[0016] 1. The present invention solves the defects of the existing laparoscope lens that it is easy to fog and pollute. A composite coating is used in combination with a low surface energy liquid film to form a liquid-containing layered structure on the surface of the laparoscope lens, which has the effect of preventing fogging and pollution, and the effect is quite significant.

[0017] 2. The present invention utilizes nano-silica as a framework connection point, and cooperates with the activity of silanol after hydrolysis of ethyl silicate to form a framework structure with stable connection and pores, providing conditions for the subsequent formation of multiple porous structures and coating stability; secondly, the present invention uses in-situ hydrolysis to achieve surface activation on the silicon-oxygen material, and forms a connection structure of the silicon-oxygen system with the silicon hydroxyl groups on other materials, thereby achieving the connection stability of the homogeneous system.

[0018] 3. The present invention uses silicon-based precursors as raw materials, and forms a transparent silicon-oxygen structure system by means of in-situ hydrolysis and controlled polycondensation. Polyvinyl pyrrolidone is used as a recyclable porogen to form a stable and firm pore dispersion structure.

[0019] 4. The present invention utilizes the pore connectivity within the composite coating to ensure the stability of the protective liquid, achieves anti-fog and anti-fouling effects, and can quickly replenish when worn, thereby extending the service life. The composite coating of the silicon-oxygen system itself belongs to a porous structure system, which can lock the protective liquid and prevent the flow loss of the protective liquid. DETAILED DESCRIPTION

[0020] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.

[0021] Example 1

[0022] A method for preparing a liquid-containing coating comprises the following steps:

[0023] Step 1, adding nano-silicon dioxide and ethyl silicate to diethyl ether and stirring at a speed of 100 r / min, filtering and drying at 40° C. to obtain biofilm-forming nano-silicon dioxide, wherein the particle size of the nano-silicon dioxide is 10-100 nm, the molar ratio of the nano-silicon dioxide to the ethyl silicate is 10:1, and the concentration of the ethyl silicate in the diethyl ether is 5 g / L;

[0024] Step 2, let the biofilm nano-silica stand for 10-20 minutes, then add it to the ethyl cellulose dispersion, stir evenly to obtain a mixed solution, spray-deposit the mixed solution and sinter at a constant temperature to obtain a silicon oxygen framework; the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9:1, and the temperature is 30°C; the ethyl cellulose dispersion is an ethanol solution of ethyl cellulose, and the concentration of the ethyl cellulose in ethanol is 10g / L, the mass ratio of the biofilm nano-silica to ethyl cellulose is 3:2, the stirring speed of the uniform stirring is 300r / min, and the spray amount of the spray deposition is 0.1mL / cm 2 , the temperature is 50°C; the temperature of the constant temperature sintering is 200°C;

[0025] Step 3, adding trichloromethylsilane to ether and stirring evenly to form a dissolving solution, then immersing the silicon oxygen frame in the dissolving solution and stirring rapidly, taking it out and airing it to half dry, drying it and standing it to obtain a coated silicon oxygen frame, the concentration of the trichloromethylsilane in the ether is 100g / L, the stirring speed for uniform stirring is 100r / min, the speed of rapid stirring is 800r / min, the drying temperature is 20°C, the standing atmosphere is an atmosphere of nitrogen and water vapor, and the volume ratio of water vapor to nitrogen is 1:10, and the temperature is 5°C;

[0026] Step 4, adding polyvinyl pyrrolidone to methanol and stirring evenly to dissolve, then slowly adding ethyl silicate and methyl trimethoxy silane and rapidly dispersing until completely dissolved to form a mixed coating solution, then uniformly coating the mixed coating solution on the coated silicon oxygen frame, and scraping off the excess to obtain a composite prefabricated coating, wherein the concentration of the polyvinyl pyrrolidone in methanol is 500 g / L, the stirring speed is 200 r / min, the mass ratio of the ethyl silicate to methyl trimethoxy silane is 5:1, and the mass ratio of the polyvinyl pyrrolidone to ethyl silicate is 1:0.8, and the rapid dispersion adopts mechanical stirring; the temperature adopted for the homogeneous coating is 5°C, and the homogeneous coating adopts a repeated coating method to ensure that the mixed coating solution completely penetrates into the coated silicon oxygen frame;

[0027] Step 5: Spray distilled water onto the surface of the composite prefabricated coating, and keep it at a constant temperature for 2 hours, heat it up and sinter it for 20 minutes, then cool it to room temperature and put it into an ethanol aqueous solution, stir and wash it several times, and dry it to obtain a composite coating. The spraying speed is 1 mL / cm2 , the temperature is 10°C, the temperature of the constant temperature static is 100°C, the temperature of the temperature rising sintering is 180°C; the volume proportion of ethanol in the ethanol aqueous solution is 70%, the stirring speed of the stirring washing is 100r / min, and the temperature of the drying is 150°C;

[0028] Step 6, injecting the medical lubricating liquid into the composite coating and removing excess medical lubricating oil to obtain a liquid-containing coating, wherein the viscosity of the medical lubricating liquid is 20 cSt, and the medical lubricating oil is injected by a negative pressure method, and the medical lubricating liquid adopts the "Saio" series of Weihai Huakang Biomaterial Technology Co., Ltd.

[0029] The composite coating in the liquid-containing coating contains macropores with a pore size of 100-300 μm and micropores with a pore size of 0.1-0.4 μm.

[0030] Example 2

[0031] A method for preparing a liquid-containing coating comprises the following steps:

[0032] Step 1, adding nano-silicon dioxide and ethyl silicate to ether and stirring evenly, filtering and drying to obtain biofilm nano-silicon dioxide, wherein the particle size of the nano-silicon dioxide is 10-100 nm, the molar ratio of the nano-silicon dioxide to ethyl silicate is 15:1, the concentration of the ethyl silicate in ether is 10 g / L, the stirring speed for uniform stirring is 300 r / min, and the drying temperature is 50° C.;

[0033] Step 2, let the biofilm nano-silica stand for 20 minutes, then add it to the ethyl cellulose dispersion, stir it evenly to obtain a mixed solution, spray-deposit the mixed solution and sinter it at a constant temperature to obtain a silicon oxygen framework; the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 10:1, and the temperature is 60°C; the ethyl cellulose dispersion is an ethanol solution of ethyl cellulose, and the concentration of ethyl cellulose in ethanol is 20g / L, the mass ratio of the biofilm nano-silica to ethyl cellulose is 1:1, the stirring speed of the uniform stirring is 500r / min, and the spray amount of the spray deposition is 0.3mL / cm 2 , the temperature is 70°C; the temperature of the constant temperature sintering is 230°C;

[0034] Step 3, adding trichloromethylsilane to ether and stirring evenly to form a dissolving solution, then immersing the silicon oxygen frame in the dissolving solution and stirring rapidly, taking it out and airing it to half dry, drying it and standing it to obtain a coated silicon oxygen frame, the concentration of the trichloromethylsilane in the ether is 300g / L, the stirring speed for uniform stirring is 200r / min, the speed of rapid stirring is 1000r / min, the drying temperature is 30°C, the standing atmosphere is an atmosphere of nitrogen and water vapor, and the volume ratio of water vapor to nitrogen is 1:15, and the temperature is 10°C;

[0035] Step 4, adding polyvinyl pyrrolidone to methanol and stirring evenly to dissolve, then slowly adding ethyl silicate and methyl trimethoxy silane and rapidly dispersing until completely dissolved to form a mixed coating solution, then uniformly coating the mixed coating solution on the coated silicon oxygen frame, and scraping off the excess to obtain a composite prefabricated coating, wherein the concentration of the polyvinyl pyrrolidone in methanol is 700 g / L, the stirring speed is 300 r / min, the mass ratio of the ethyl silicate to methyl trimethoxy silane is 8:1, and the mass ratio of the polyvinyl pyrrolidone to the ethyl silicate is 1:1.3, and the rapid dispersion adopts mechanical stirring; the temperature adopted for the homogeneous coating is 10°C, and the homogeneous coating adopts a repeated coating method to ensure that the mixed coating solution completely penetrates into the coated silicon oxygen frame;

[0036] Step 5: Spray distilled water onto the surface of the composite prefabricated coating, and keep it at a constant temperature for 3 hours, heat it up and sinter it for 30 minutes, then cool it to room temperature and put it into an ethanol aqueous solution, stir and wash it several times, and dry it to obtain a composite coating. The spraying speed is 3mL / cm 2 , the temperature is 20°C, the temperature of constant temperature static is 110°C, the temperature of heating sintering is 200°C; the volume proportion of ethanol in the ethanol aqueous solution is 75%, the stirring speed of the stirring washing is 300r / min, and the temperature of the drying is 200°C;

[0037] Step 6, injecting the medical lubricating liquid into the composite coating, and removing the excess medical lubricating oil to obtain a liquid-containing coating, the viscosity of the medical lubricating liquid is 300 cSt, and the medical lubricating oil is injected by a negative pressure method, and the medical lubricating liquid adopts the "Saio" series of Weihai Huakang Biomaterial Technology Co., Ltd.

[0038] The composite coating in the liquid-containing coating contains macropores with a pore size of 100-300 μm and micropores with a pore size of 0.1-0.4 μm.

[0039] Example 3

[0040] A method for preparing a liquid-containing coating comprises the following steps:

[0041] Step 1, adding nano-silica and ethyl silicate to ether and stirring evenly, filtering and drying to obtain biofilm nano-silica, wherein the particle size of the nano-silica is 10-100 nm, the molar ratio of the nano-silica to ethyl silicate is 13:1, the concentration of the ethyl silicate in ether is 8 g / L, the stirring speed for even stirring is 200 r / min, and the drying temperature is 45° C.;

[0042] Step 2, let the biofilm nano-silica stand for 15 minutes, then add it to the ethyl cellulose dispersion, stir it evenly to obtain a mixed solution, spray-deposit the mixed solution and sinter it at a constant temperature to obtain a silicon oxygen framework; the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 10:1, and the temperature is 50°C; the ethyl cellulose dispersion is an ethanol solution of ethyl cellulose, and the concentration of ethyl cellulose in ethanol is 15g / L, the mass ratio of the biofilm nano-silica to ethyl cellulose is 3:2, the stirring speed of the uniform stirring is 400r / min, and the spray amount of the spray deposition is 0.2mL / cm 2 , the temperature is 60°C; the temperature of the constant temperature sintering is 210°C;

[0043] Step 3, adding trichloromethylsilane to ether and stirring evenly to form a dissolving solution, then immersing the silicon oxygen frame in the dissolving solution and stirring rapidly, taking it out and airing it to half dry, drying it and standing it to obtain a coated silicon oxygen frame, wherein the concentration of the trichloromethylsilane in the ether is 200g / L, the stirring speed for even stirring is 150r / min, the speed of rapid stirring is 900r / min, the drying temperature is 25°C, the standing atmosphere is an atmosphere of nitrogen and water vapor, and the volume ratio of water vapor to nitrogen is 1:13, and the temperature is 8°C;

[0044] Step 4, adding polyvinyl pyrrolidone to methanol and stirring evenly to dissolve, then slowly adding ethyl silicate and methyl trimethoxy silane and rapidly dispersing until completely dissolved to form a mixed coating solution, then uniformly coating the mixed coating solution on the coated silicon oxygen frame, and scraping off the excess to obtain a composite prefabricated coating, wherein the concentration of the polyvinyl pyrrolidone in methanol is 600 g / L, the stirring speed is 250 r / min, the mass ratio of the ethyl silicate to methyl trimethoxy silane is 7:1, the mass ratio of the polyvinyl pyrrolidone to the ethyl silicate is 1:1, and the rapid dispersion adopts mechanical stirring; the temperature adopted for the homogeneous coating is 8°C, and the homogeneous coating adopts a repeated coating method to ensure that the mixed coating solution completely penetrates into the coated silicon oxygen frame;

[0045] Step 5: Spray distilled water onto the surface of the composite prefabricated coating, and keep it at a constant temperature for 3 hours, heat it up and sinter it for 25 minutes, then cool it to room temperature and put it into an ethanol aqueous solution, stir and wash it several times, and dry it to obtain a composite coating. The spraying speed is 2mL / cm 2 , the temperature is 15°C, the temperature of the constant temperature static is 105°C, the temperature of the temperature rising sintering is 190°C; the volume proportion of ethanol in the ethanol aqueous solution is 75%, the stirring speed of the stirring washing is 200r / min, and the temperature of the drying is 180°C;

[0046] Step 6, injecting the medical lubricating liquid into the composite coating, and removing the excess medical lubricating oil to obtain a liquid-containing coating, the viscosity of the medical lubricating liquid is 50 cSt, and the medical lubricating oil is injected by a negative pressure method, and the medical lubricating liquid adopts the "Saio" series of Weihai Huakang Biomaterial Technology Co., Ltd.

[0047] The composite coating in the liquid-containing coating contains macropores with a pore size of 100-300 μm and micropores with a pore size of 0.1-0.4 μm.

[0048] Example 4

[0049] A method for preparing a liquid-containing coating comprises the following steps:

[0050] Step 1, adding nano-silicon dioxide and ethyl silicate to ether and stirring evenly, filtering and drying to obtain biofilm nano-silicon dioxide, wherein the particle size of the nano-silicon dioxide is 10-100 nm, the molar ratio of the nano-silicon dioxide to the ethyl silicate is 12:1, the concentration of the ethyl silicate in the ether is 7 g / L, the stirring speed for even stirring is 200 r / min, and the drying temperature is 42° C.;

[0051] Step 2, let the biofilm nano-silica stand for 10-20 minutes, then add it to the ethyl cellulose dispersion, stir evenly to obtain a mixed solution, spray-deposit the mixed solution and sinter at a constant temperature to obtain a silicon oxygen framework; the standing atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9:1, and the temperature is 40°C; the ethyl cellulose dispersion is an ethanol solution of ethyl cellulose, and the concentration of the ethyl cellulose in ethanol is 18g / L, the mass ratio of the biofilm nano-silica to the ethyl cellulose is 1:1, the stirring speed of the uniform stirring is 400r / min, and the spray amount of the spray deposition is 0.2mL / cm 2 , the temperature is 55°C; the temperature of the constant temperature sintering is 220°C;

[0052] Step 3, adding trichloromethylsilane to ether and stirring evenly to form a dissolving solution, then immersing the silicon oxygen frame in the dissolving solution and stirring rapidly, taking it out and airing it to half dry, drying and standing to obtain a coated silicon oxygen frame, the concentration of the trichloromethylsilane in the ether is 150g / L, the stirring speed for uniform stirring is 200r / min, the speed of rapid stirring is 1000r / min, the drying temperature is 25°C, the standing atmosphere is an atmosphere of nitrogen and water vapor, and the volume ratio of water vapor to nitrogen is 1:12, and the temperature is 7°C;

[0053] Step 4, adding polyvinyl pyrrolidone to methanol and stirring evenly to dissolve, then slowly adding ethyl silicate and methyl trimethoxy silane and rapidly dispersing until completely dissolved to form a mixed coating solution, then uniformly coating the mixed coating solution on the coated silicon oxygen frame, and scraping off the excess to obtain a composite prefabricated coating, the concentration of the polyvinyl pyrrolidone in methanol is 600g / L, the stirring speed is 250r / min, the mass ratio of the ethyl silicate to methyl trimethoxy silane is 6:1, the mass ratio of polyvinyl pyrrolidone to ethyl silicate is 1:1.2, the rapid dispersion adopts mechanical stirring; the temperature adopted for the homogeneous coating is 7°C, and the homogeneous coating adopts repeated coating to ensure that the mixed coating solution completely penetrates into the coated silicon oxygen frame;

[0054] Step 5: Spray distilled water onto the surface of the composite prefabricated coating, and keep it at a constant temperature for 2 hours, heat it up and sinter it for 30 minutes, then cool it to room temperature and put it into an ethanol aqueous solution, stir and wash it several times, and dry it to obtain a composite coating. The spraying speed is 2mL / cm 2 , the temperature is 15°C, the temperature of constant temperature static is 105°C, the temperature of heating sintering is 185°C; the volume proportion of ethanol in the ethanol aqueous solution is 72%, the stirring speed of the stirring washing is 150r / min, and the temperature of the drying is 170°C;

[0055] Step 6, injecting the medical lubricating liquid into the composite coating and removing excess medical lubricating oil to obtain a liquid-containing coating, wherein the viscosity of the medical lubricating liquid is 10-1000 cSt, and the medical lubricating oil is injected by a negative pressure method, and the medical lubricating liquid adopts the "Saio" series of Weihai Huakang Biomaterial Technology Co., Ltd.

[0056] The composite coating in the liquid-containing coating contains macropores with a pore size of 100-300 μm and micropores with a pore size of 0.1-0.4 μm.

[0057] The liquid-containing coatings of Examples 1-4 were tested as samples, and the results are as follows:

[0058]

[0059]

[0060] Among them, the coating thickness gauge tests the total thickness of the coating; the protective liquid is marked with fluorescent molecules, and then the liquid film thickness is tested using a laser confocal microscope; the visible-ultraviolet spectrophotometer characterizes the transmittance in the full wavelength range; bovine serum albumin is used to examine the anti-fouling property of the coating surface, and the bovine serum albumin liquid dropped onto the coating surface can quickly slide off, indicating that the coating is anti-fouling; in a small environmental test chamber, the temperature and humidity environment in the body is simulated, the protective cover containing the coating is put on the laparoscope, and the fogging and fog dissipation speed is recorded in the environmental chamber. If there is no fog in the lens field of view and the clarity of the laparoscope field of view does not decrease, it can be regarded as anti-fogging.

[0061] The above data show that the liquid-containing coating of the technical solution has good high light transmittance, and can effectively prevent smoke from forming on the lens surface, and can also prevent blood and protein liquid from adhering, thereby maintaining the clarity of the lens. The anti-fouling test after 48 hours performed well and met the use requirements.

[0062] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for preparing a liquid-containing coating, characterized in that: The steps include: Step 1, adding nano-silica and ethyl silicate into ether and stirring evenly, filtering and drying to obtain biofilm-forming nano-silica; Step 2, allowing the biofilm nano-silica to stand for 10-20 minutes, then adding it to the ethyl cellulose dispersion, stirring it to obtain a mixed solution, spraying and depositing the mixed solution, and sintering it at a constant temperature to obtain a silicon-oxygen framework; Step 3, adding trichloromethylsilane to ether and stirring evenly to form a dissolving solution, then immersing the silicon oxygen framework in the dissolving solution and stirring rapidly, taking it out and airing it to half dry, drying it and standing it to obtain a coated silicon oxygen framework; Step 4, adding polyvinyl pyrrolidone to methanol and stirring evenly to dissolve, then slowly adding ethyl silicate and methyltrimethoxysilane and rapidly dispersing until completely dissolved to form a mixed coating solution, then uniformly coating the mixed coating solution on the coated silicon oxygen frame, and scraping off the excess to obtain a composite prefabricated coating; Step 5, spraying distilled water onto the surface of the composite prefabricated coating, and standing at a constant temperature for 2-3 hours, heating and sintering for 20-30 minutes, and then cooling to room temperature and placing in an ethanol aqueous solution for stirring and washing for multiple times, and drying to obtain a composite coating; Step 6, injecting the medical lubricating liquid into the composite coating and removing excess medical lubricating oil to obtain a liquid-containing coating.

2. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The particle size of the nano-silica in step 1 is 10-100 nm, the molar ratio of the nano-silica to ethyl silicate is 10-15:1, the concentration of ethyl silicate in ether is 5-10 g / L, the stirring speed for uniform stirring is 100-300 r / min, and the drying temperature is 40-50°C.

3. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The static atmosphere in step 2 is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9-10:1, and the temperature is 30-60°C; the ethyl cellulose dispersion is an ethanol solution of ethyl cellulose, and the concentration of the ethyl cellulose in ethanol is 10-20g / L, the mass ratio of the biofilm nano-silica to the ethyl cellulose is 3:2-3, the stirring speed for uniform stirring is 300-500r / min, and the spray amount of the spray deposition is 0.1-0.3mL / cm 2 , the temperature is 50-70℃; the temperature of the constant temperature sintering is 200-230℃.

4. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The concentration of trichloromethylsilane in diethyl ether in step 3 is 100-300 g / L, the stirring speed for uniform stirring is 100-200 r / min, the speed of rapid stirring is 800-1000 r / min, the temperature of the drying is 20-30°C, the static atmosphere is an atmosphere of nitrogen and water vapor, and the volume ratio of water vapor to nitrogen is 1:10-15, and the temperature is 5-10°C.

5. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The concentration of polyvinyl pyrrolidone in methanol in step 4 is 500-700g / L, the stirring speed is 200-300r / min, the mass ratio of ethyl silicate to methyltrimethoxysilane is 5-8:1, the mass ratio of polyvinyl pyrrolidone to ethyl silicate is 1:0.8-1.3, the rapid dispersion adopts ultrasonic dispersion or mechanical stirring; the temperature adopted for the homogeneous coating is 5-10°C, and the homogeneous coating adopts repeated coating to ensure that the mixed coating liquid completely penetrates into the coating silicon oxygen frame.

6. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The spray speed in step 5 is 1-3 mL / cm 2 The temperature is 10-20°C, the temperature of constant temperature standing is 100-110°C, and the temperature of heating sintering is 180-200°C; the volume proportion of ethanol in the ethanol aqueous solution is 70-75%, the stirring speed of the stirring washing is 100-300r / min, and the temperature of the drying is 1120-150°C.

7. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The viscosity of the medical lubricating liquid in step 6 is 10-1000 cSt, and the medical lubricating oil is injected using a negative pressure method.

8. The method for preparing a liquid-containing coating according to claim 1, characterized in that: The total thickness of the liquid-containing coating in step 5 is 450-600 μm, and the thickness of the liquid film is 120-150 nm.

9. The method for preparing a liquid-containing coating according to claim 8, characterized in that: The composite coating in the liquid-containing coating includes macropores with a pore size of 100-300 μm and micropores with a pore size of 0.1-0.4 μm.