Preparation method of high-performance small-hole precise separation membrane
By using reactive porogens to generate nanobubbles during the preparation process of small-pore precision separation membranes, the membrane pore structure is controlled, solving the problems of porogen residue and low membrane performance, and realizing the preparation of high-performance small-pore precision separation membranes. It has excellent separation accuracy and permeation flux.
Patent Information
- Application Number
- CN202411087155.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-09
AI Technical Summary
In the existing preparation methods of small-pore precision separation membranes, porogens are easy to remain and affect the composition and quality of the permeate. Moreover, the membrane pore size distribution is wide and the porosity is low, resulting in a decrease in separation efficiency and permeation flux, making it difficult to prepare high-performance membranes.
Reactive porogens are used to generate nanobubbles in situ in the casting liquid to regulate the membrane pore structure. Nanobubbles with uniform sizes are generated in the casting liquid and coagulation bath through heating or acid-base reaction to modulate the membrane pore structure and prepare high-performance Small hole precision separation membrane.
A high-performance small pore precision separation membrane with uniform surface pore structure, small pore size and narrow distribution has been achieved. It has high selective separation capability and excellent permeation flux, avoids porogen residue, and improves separation accuracy and economic benefits.
Smart Images

Figure CN118767696A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of membrane separation, and in particular relates to a method for preparing a high-performance small-pore precision separation membrane. Technical Background
[0002] The small-pore precision separation membrane is a separation membrane with a pore size between that of ultrafiltration membrane and nanofiltration membrane. Its pore size is usually 1-10nm. Compared with the traditional polyamide nanofiltration membrane (pore size is usually less than 1nm), it has a larger adjustable pore size and can be used for the separation of organic small molecules of different molecular weights and organic small molecules and salts. It can retain organic small molecules to a certain extent, but has a very low retention rate for inorganic salts. Therefore, it has a wide range of applications in biomedical separation, high-salt dye wastewater treatment, food processing, electronic ultrapure water preparation, municipal drinking water, industrial wastewater, etc.
[0003] At present, the main methods for preparing small-pore precision separation membranes are interfacial polymerization, chemical crosslinking, self-assembly and non-solvent induced phase separation (NIPS). Among them, the NIPS method has become one of the most effective methods for preparing separation membranes due to its simple process, high film-making efficiency and low cost. The NIPS membrane preparation process mainly includes preparing casting solution, degassing, film formation, and immersing in a coagulation bath to prepare membrane materials. During the immersion in the coagulation bath, the solvent comes out of the solution membrane and enters the coagulation bath, and the non-solvent in the coagulation bath enters the solution membrane to solidify the solution membrane. Part of the added porogen is dissolved from the casting solution into the coagulation bath during the phase inversion process, and part of the porogen is retained in the final membrane structure. Since porogens are usually hydrophilic materials, although the porogens retained in the separation membrane structure can improve the hydrophilicity and anti-pollution properties of the membrane, the porogens will slowly precipitate during the use of the membrane and enter the permeate with the material, affecting the composition and quality of the permeate. This phenomenon of separation membrane precipitation itself should be avoided as much as possible for applications in fields with special requirements (such as biomedical separation, food separation, water purification, electronic grade ultrapure water and electronic grade reagents). In addition, the small-pore precision separation membrane prepared by the NIPS method usually has a wide pore size distribution and a low porosity, resulting in a decrease in the separation efficiency and permeation flux of the membrane, making it difficult to prepare a high-performance small-pore precision separation membrane.
[0004] CN113769586A discloses a double-layer polyvinylidene fluoride hollow fiber small pore precision separation membrane for dye desalination, wherein the small pore precision separation membrane has a neutral molecule MWCO of 1530Da and an average pore size of 1.21nm. Although it has a high retention rate of almost 100% for the dye chrome black T (Mn=461Da) with a small molecular weight and a high NaCl permeability of 96.8%, its pure water permeability is very low, only 14.2L / (m 2 ·h·bar).
[0005] In view of the problems existing in the prior art, the present invention provides a new method for preparing a small-pore precision separation membrane, which uses in-situ generated nanobubbles as porogens to modulate the membrane pore structure. There is no need to add conventional hydrophilic porogens that are prone to residue and precipitation. The prepared high-performance small-pore precision separation membrane has important application prospects in the fields of biomedical separation, food separation, healthy water, electronic-grade ultrapure water and electronic-grade reagent preparation. Summary of the invention
[0006] The present invention aims to provide a method for preparing a small-pore precision separation membrane, wherein a reactive porogen is added to the casting solution, and a reaction can occur during the heating process of the casting solution and / or the phase transformation process of the solidification bath and / or the subsequent membrane treatment process to generate in-situ molecular-level nanobubbles with uniform size and uniform distribution, and the phase transformation process is regulated and the membrane pore structure is modulated to prepare a high-performance small-pore precision separation membrane. The technical solution of the present invention is as follows:
[0007] A method for preparing a small-pore precision separation membrane comprises the following steps:
[0008] (1) adding a film-forming polymer and an auxiliary agent to a solvent, dissolving them at 20-70° C., naturally cooling to below 60° C., and vacuum degassing at this temperature to form a solution 1. The vacuum degassing time may be 7-9 hours, preferably 7.5-8.5 hours;
[0009] Add the reactive porogen to the same solvent and stir to dissolve at 20-40° C., and perform vacuum degassing at this temperature to form a solution 2. The vacuum degassing time may be 3.5-5 hours, preferably 3.5-4 hours;
[0010] Slowly pouring solution 2 into solution 1 and keeping the mixture at 40-60° C. for a period of time to form a casting solution. The keeping time may be, for example, 3-5 hours, preferably 3.5-4 hours;
[0011] Wherein, the solvent ratio in solution 1 and solution 2 is 4:1, the content of film-forming polymer is 12%-30%, the content of reactive porogen is 2%-14%, and the content of auxiliary agent is 0-10%, based on the total weight of the casting solution;
[0012] (2) forming a solution film with a thickness of 100-500 μm from the casting solution obtained in step (1);
[0013] (3) Soaking the solution membrane of step (2) in a coagulation bath with a pH value of 7-14, and leaving it in the coagulation bath for not less than 30 seconds to obtain a small-pore precision separation membrane;
[0014] (4) immersing the small-pore precision separation membrane obtained in step (3) in an aqueous solution of a certain pH value at a certain temperature for 1 to 8 hours, so that the unreacted reactive porogen in step (3) is further reacted completely;
[0015] (5) The small-pore precision separation membrane treated in step (4) is placed in distilled water for cleaning, and then placed in distilled water or glycerol solution for treatment and then stored.
[0016] In step (1), the film-forming polymer is a polymer material that can be used to prepare a film, preferably one or two of the materials selected from polysulfone (PSf), polyethersulfone (PES), polyvinylidene fluoride (PVDF), polyvinyl chloride (PVC), polyphenylene sulfide (PPS), polyimide (PI), etc.
[0017] The solvent is a solvent that can dissolve the film-forming polymer, preferably one or more solvents such as N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and dimethyl sulfoxide (DMSO).
[0018] The reactive porogen refers to a substance that can be dissolved or uniformly dispersed in the casting solution and can decompose to generate gas under certain conditions. Preferably, one or more of azobisisobutyronitrile, diisopropyl azodicarboxylate, diethyl azodicarboxylate, azodicarbonamide, sodium borohydride, and p-toluenesulfonyl hydrazide are used as the reactive porogen.
[0019] The auxiliary agent refers to a small molecule solvent that can promote the dissolution of the reactive porogen or adjust the liquid phase of the casting film, preferably one or more of water, tetrahydrofuran, methanol, glycerol, etc.
[0020] In step (2), the solution state membrane coating can be carried out by any conventional suitable method, including but not limited to knife coating, brush coating, spray coating, etc. Alternatively, the membrane can be prepared in the form of a supported or self-supporting hollow fiber membrane.
[0021] In step (3), during the immersion in the coagulation bath, the casting liquid and the coagulation bath undergo phase transformation, and at the same time, the reactive porogen contacts the coagulation bath to undergo a chemical reaction to generate nanobubbles. The hydrophobic and oleophobic properties of the generated nanobubbles are used to adjust the phase transformation rate and thereby regulate the membrane pore structure.
[0022] The coagulation bath is an aqueous solution medium that can react with the reactive porogen and generate nanobubbles, and can be adjusted to different pH values by acid or alkali, generally pH 7-14, for example, pH 7.0, 7.5, 8.5, 9.0, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, etc. The temperature of the coagulation bath is room temperature to 70° C. The acid used to adjust the pH value can be selected from hydrochloric acid and sulfuric acid solution, and the alkali can be selected from sodium hydroxide or potassium hydroxide solution.
[0023] In step (4), the aqueous solution with a certain pH value is an aqueous solution whose pH value is adjusted to 7-14 by acid or alkali, the pH value is the same as the pH value of the coagulation bath in step (3), the immersion time is 0.5 to 48 hours, and the temperature of the coagulation bath is room temperature to 70° C. The unreacted reactive porogen in step (3) reacts therein to generate nanobubbles.
[0024] The process of generating nanobubbles by decomposing the reactive porogen may occur in steps (1) to (4), or in steps (1) to (3), or in step (3), wherein the nanobubbles generated in step (1) are generated by the self-decomposition of the reactive porogen at a certain temperature, and the bubbles generated in steps (2) to (4) are mainly generated by the reaction of the reactive porogen with a weak acid or a strong base, and also include some nanobubbles generated by the self-decomposition of the reactive porogen due to temperature increase.
[0025] According to the method of the present invention, the reactive porogen can react chemically in three stages, namely, the heating process of the casting liquid, the phase transformation process of the solidification bath, or the subsequent membrane treatment process, to generate nanobubbles of uniform size and uniform distribution. The generation of nanobubbles can be regulated in the three stages, and the advantages are: the first stage is in the casting liquid (for one of the above steps (1) and (2)), the generated nanobubbles affect the viscosity of the casting liquid, thereby affecting the phase transformation process and ultimately affecting the membrane pore structure, so that the viscosity of the casting liquid can be regulated by treating the casting liquid at a certain temperature, thereby achieving the regulation of the membrane pore size. The second stage is in the phase transformation process, the generated nanobubbles directly regulate the phase transformation process, promote the uniformity of the phase transformation process, and make the surface pore structure of the prepared separation membrane structure more uniform (corresponding to the above step (3)). Therefore, the nanobubble generation rate can be regulated by controlling the solidification bath alkali concentration, thereby achieving the regulation of the phase transformation process, and finally achieving the regulation of the membrane pore size and surface porosity. The third stage is the generation of nanobubbles in the post-treatment process, which is conducive to pore formation, improving the overall porosity, and further improving the permeation flux of the membrane (corresponding to the above step (4)). Therefore, the amount of the reaction porogen added can be adjusted to further adjust the amount remaining in the third stage, thereby ultimately achieving the regulation of the overall porosity of the membrane. The three stages do not necessarily generate nanobubbles in each stage, for example, nanobubbles may be generated in the first stage, the second stage, and the third stage; nanobubbles may be generated only in the first and second stages; or nanobubbles may be generated only in the second stage.
[0026] The present invention further relates to a small-pore precision separation membrane prepared by the method of the present invention, wherein the small-pore precision separation membrane can be a flat membrane, or can be in various membrane forms such as a hollow fiber membrane, a liner membrane, and a tubular membrane.
[0027] The permeation separation performance of the obtained small pore precision separation membrane was tested according to the following method:
[0028] The permeation separation performance of the small-pore precision separation membrane was tested using a cross-flow filtration device, where the effective membrane area used for the test was 7.1 cm 2 , the test pressure is 1 bar, and the test temperature is 25±0.5℃.
[0029] The calculation formula of water flux is as follows (1):
[0030]
[0031] Where J is the water flux of the membrane (L·m 2 ·h), V is the volume of water permeating the membrane (L), A is the effective area of the membrane (m 2 ), △t is the penetration time (h).
[0032] The small-pore precision separation membrane obtained by the method of the present invention has a uniform pore structure, small pore size, and narrow distribution. Its average pore diameter is in the range of 1-8nm, and its surface porosity is high, which can reach 15%. The membrane has good selective separation. While ensuring high efficiency interception of small molecule dyes (up to 99.9%), it has a low interception rate for inorganic salts such as Na2SO4, CaSO4, and NaCl. For example, the interception rate for sodium chloride solution is less than 5%. At the same time, the pure water flux can reach up to 600L / (m 2 ·h), has excellent separation performance. Compared with the existing membrane products of the same level of pore size, the pure water permeation flux is significantly improved, and the separation accuracy is higher. The comprehensive permeation separation performance is better than the existing small-pore separation membrane. And the obtained small-pore precision separation membrane maintains good mechanical properties, for example, its tensile strength can reach 8MPa.
[0033] Compared with the prior art, the present invention has the following advantages:
[0034] 1. The method of the present invention adopts a reactive porogen, which has good dispersibility in the casting liquid and can achieve molecular-level dissolution and dispersion in the casting liquid. In the phase transformation film-forming process, molecular-level nanobubbles are generated in situ by heating or acid-base catalytic reaction decomposition. The molecular-level nanobubbles are used as porogens, and the membrane pore structure is regulated by the ultra-high stability, self-pressurized solubility, oleophobicity and hydrophobicity of the molecular-level nanobubbles; the reactive porogen is uniformly dispersed in the casting liquid, so that the generated nanobubbles are more uniform in size, smaller in size, and more stable, which is more conducive to the preparation of small-pore precision separation membranes with uniform pore sizes.
[0035] 2. The nanobubbles produced by the reactive porogen have the "double-repellent" characteristics of being repellent to organic solvents (solvents in the casting solution) and hydrophobic (water in the coagulation bath). During the phase inversion process, once the casting solution comes into contact with the coagulation bath, the reactive porogen in the casting solution reacts with the acid-base medium in the coagulation bath to generate nanobubbles. The presence of nanobubbles prevents the double diffusion process of the solvent in the casting solution and the non-solvent in the coagulation bath, which can change the exchange process between the solvent in the solution film and the solvent in the coagulation bath during the phase inversion process, regulate the diffusion rate of the two, and play a role in regulating the film-forming kinetics process, and independently regulate the surface pore structure and distribution to obtain a small-pore precision separation membrane with high separation accuracy and high flux. This is different from the uncontrollable kinetic process of double diffusion of solvent and non-solvent in the traditional NIPS method. Although the traditional NIPS method can also produce small-pore (<10nm) separation membranes, they generally have fewer pores, low surface porosity, and a wider pore distribution, which leads to low water flux (generally around 100L / (m 2 h) or less) and low separation accuracy.
[0036] 3. The good solubility and dispersibility of the reactive porogen in the casting solution make it possible to adjust the membrane porosity by changing the amount of the reactive porogen added.
[0037] 4. Reactive porogens can be decomposed to produce nanobubbles in a variety of ways, such as by heating, acid / base reaction, etc., which provides more possibilities for the controllability of the process.
[0038] 5. The molecular weight of reactive porogens is low, and their decomposition products are usually gas molecules (such as CO2, O2, H2 and / or small molecule alkanes, etc.), which can easily overflow directly after post-treatment and membrane drying, and there is almost no porogen residue, resulting in very little precipitate during the use of the membrane, thereby reducing the pollution and damage of the precipitate to the separated product. Different from the traditional NIPS method, which uses hydrophilic macromolecules as porogens and has the problem of porogen residues and difficulty in cleaning, this is of great significance for applications in the fields of biomedical separation, food and beverage separation, healthy water, electronic ultrapure water and electronic grade reagent preparation.
[0039] 6. In the present invention, except for the reactive porogen, no other conventional hydrophilic porogen that is easy to remain and precipitate is added. The reactive porogen used is completely removed during the phase transformation and post-treatment process without residue, which significantly improves the problem of organic precipitation in the separation membrane, avoids the problem of high organic content in the coagulation bath caused by the entry of large molecular porogens into the coagulation bath during the traditional NIPS film formation process, simplifies the organic solvent recovery process in the later coagulation bath, greatly reduces the organic solvent recovery cost, and improves economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1This is a scanning electron microscope photograph of the small pore precision separation membrane obtained in Example 1.
[0041] Figure 2 This is a scanning electron microscope photograph of the separation membrane obtained in Comparative Example 1.
[0042] Figure 3 The graph is a pore size distribution graph of the membranes obtained in Example 1 and Comparative Example 1.
[0043] Figure 4 The graph is a graph of the pore size distribution of the membranes obtained in Example 2 and Example 4. DETAILED DESCRIPTION
[0044] The present invention is further described in detail below in conjunction with specific examples. The embodiments are only used to illustrate the present invention and do not constitute a limitation. Several modifications and improvements made by those skilled in the art without departing from the concept technology involved in the present invention all belong to the protection scope of the present invention.
[0045] The reagents and raw materials used in the examples of the present invention are not particularly limited and can all be purchased commercially.
[0046] Example 1
[0047] 12g polyethersulfone and 2g tetrahydrofuran were added to 59.2g N,N-dimethylformamide solvent, stirred at 70°C for 8h, then transferred to a vacuum oven for degassing for 1h and cooled to 40°C, recorded as solution 1. 12g azobisisobutyronitrile was added to 14.8g N,N-dimethylformamide solvent and dissolved at 40°C and vacuum degassed to form solution 2, then solution 2 was slowly poured into solution 1 and heated to 60°C for 4 hours to form a casting liquid, and the casting liquid was evenly coated on a glass plate at a speed of 1500mm / min using an automatic coating machine, and the liquid film thickness was controlled to be 100μm, and then immediately placed in a coagulation bath with a pH of 8 and a temperature of 70°C for phase transformation into a membrane for 30 minutes. The membrane was then soaked in the above solution for 24h to remove residual solvent and reactive porogen. Finally, the membrane was soaked in a 50% glycerol aqueous solution for 2h, and then dried naturally to obtain a small pore precision separation membrane. The obtained membrane pore size is 8.2nm, and the maximum pore size distribution is 3-20nm (pore size and pore size distribution are as shown in Figure 1 and Figure 3 As shown), permeate flux 600.9L / (m 2 h), the retention of inorganic sodium sulfate, calcium sulfate, sodium chloride and other salts is less than 5%, and the membrane strength is 3.5MPa.
[0048] Depend on Figure 1 It can be seen from the scanning electron microscope photo that the membrane surface of this embodiment has a large number of pores and a relatively uniform pore size. Therefore, the membrane can achieve high-throughput and precise separation. Figure 3It can be seen from the curve graph that the membrane surface pore size concentration of this embodiment is high, the pore size is uniform, and the pore size distribution is narrow.
[0049] Example 2
[0050] 30g of polysulfone and 2g of ethanol were dissolved in 48g of N,N-dimethylformamide / dimethyl sulfoxide (mass ratio 3:1) solvent, stirred at 70℃ for 8h, then transferred to a vacuum oven for degassing for 1h and cooled to 40℃, recorded as solution 1. 8g of azodicarbonamide was added to 12g of N,N-dimethylformamide / dimethyl sulfoxide (mass ratio 3:1) and dissolved at 60℃ and vacuum degassed to form solution 2, then solution 2 was slowly poured into solution 1 and heated to 60℃ and kept warm for 4 hours to form a casting solution. Then, an automatic coating machine was used to evenly coat the solution on a glass plate at a speed of 1500mm / min, and the thickness of the liquid film was controlled to be 500μm, and then immediately placed in a coagulation bath at pH=14 and temperature of 60℃ for phase transformation to form a film for 30 minutes. The film was then immersed in an aqueous solution at pH=14 and temperature of 20℃ for 24h to remove residual solvent and reactive porogen. Finally, the membrane was immersed in a 50% glycerol aqueous solution for 2 h. The pore size of the resulting membrane was significantly reduced to 1.3 nm, and the maximum width of the pore size distribution was narrow, only 0.4-3 nm (pore size and pore size distribution are shown in Figure 2). Figure 4 As shown), the membrane permeation flux is 100.8L / (m 2 h), which is conducive to the separation of small molecules and salts, with a retention rate of less than 5% for sodium chloride and a membrane strength of 8.5 MPa. Figure 4 It can be seen from the curve graph that the pore size distribution of the membrane in Example 2 is narrower and the pore size is more uniform.
[0051] Example 3
[0052] 30g polyethersulfone and 1g tetrahydrofuran were dissolved in 48.8g N,N-dimethylformamide solvent, stirred at 70℃ for 8h, then transferred to a vacuum oven for degassing for 1h and cooled to 60℃, recorded as solution 1. 8g sodium borohydride was added to 12.2g N,N-dimethylformamide and dissolved at 60℃ and vacuum degassed to form solution 2, then solution 2 was slowly poured into solution 1 and heated to 60℃ and kept warm for 4 hours to form a casting liquid. Then an automatic coating machine was used to evenly coat the glass plate at a speed of 1500mm / min, and the liquid film thickness was controlled to be 200μm, and then immediately placed in a coagulation bath at pH=6 and temperature of 20℃ for phase transformation to form a film for 30 minutes. Then the membrane was immersed in an aqueous solution at pH=7 and temperature of 20℃ for 24h to remove residual solvents and reactive porogens. Finally, the membrane was immersed in a 50% glycerol aqueous solution for 24h. The membrane pore size was 3.8 nm and the permeation flux was 180.5 L / (m 2 ·h), the tensile strength of the film can reach 8.3MPa.
[0053] Example 4
[0054] This example repeats Example 2, except that no auxiliary agent is added.
[0055] 30g of polysulfone was dissolved in 48g of N,N-dimethylformamide / dimethyl sulfoxide (mass ratio 3:1) solvent, stirred at 70℃ for 8h, then transferred to a vacuum oven for degassing for 1h and cooled to 40℃, recorded as solution 1. 8g of azodicarbonamide was added to 12g of N,N-dimethylformamide / dimethyl sulfoxide (mass ratio 3:1) and dissolved at 60℃ and vacuum degassed to form solution 2, then solution 2 was slowly poured into solution 1 and heated to 60℃ and kept warm for 4 hours to form a casting solution. Then, an automatic coating machine was used to evenly coat the solution on a glass plate at a speed of 1500mm / min, and the thickness of the liquid film was controlled to be 500μm, and then immediately placed in a coagulation bath at pH=14 and temperature of 60℃ for phase transformation to form a film for 30 minutes. The film was then immersed in an aqueous solution at pH=14 and temperature of 20℃ for 24h to remove residual solvent and reactive porogen. Finally, the membrane was immersed in a 50% glycerol aqueous solution for 2 h. The resulting membrane had a pore size of 2.9 nm and a pore size distribution width of 1-10 nm (pore size and pore size distribution as shown in Figure 4 As shown), the membrane permeation flux is 70L / (m 2 h). Figure 4 It can be seen from the curve that, relative to Example 2, the membrane pore size distribution of Example 4 is wider and the pore size is larger, indicating that the additive has a good regulating effect on the pore size and distribution of the small pore membrane.
[0056] Example 5
[0057] 30g of polysulfone was stirred in 48g of N,N-dimethylformamide solvent at 70℃ for 8h, then transferred to a vacuum oven for degassing for 1h and cooled to 40℃, which was recorded as solution 1. 8g of sodium borohydride was added to 12g of N,N-dimethylformamide and dissolved at 60℃ and vacuum degassed to form solution 2, then solution 2 was slowly poured into solution 1 and heated to 60℃ and kept warm for 4 hours to form a casting liquid. Then, an automatic coating machine was used to evenly coat the glass plate at a speed of 1500mm / min, and the liquid film thickness was controlled to be 200μm. Then, it was immediately placed in a coagulation bath at pH=7 and temperature of 25℃ for phase transformation to form a film for 30 minutes. Then, the film was immersed in an aqueous solution at pH=7 and temperature of 20℃ for 24h to allow the remaining reactive porogen to continue to react and remove residual solvents. Finally, the film was immersed in a 50% glycerol aqueous solution for 2h. The membrane pore size was 3.3 nm, the maximum width of the pore size distribution was narrow, only 1-8 nm, and the membrane permeation flux was 180.7 L / (m 2h), which is conducive to the separation of small molecules and salts, with a sodium chloride retention rate of less than 5% and a membrane strength of 8.5 MPa.
[0058] Comparative Example 1
[0059] This comparative example 1 repeats Example 1, except that no reactive porogen is added.
[0060] 12g polyethersulfone and 2g tetrahydrofuran were added to 59.2g N,N-dimethylformamide solvent, stirred at 70℃ for 8h, then transferred to a vacuum oven for degassing for 1h and cooled to 40℃, recorded as solution 1. Then 14.8g N,N-dimethylformamide solvent was added to it, dissolved at 40℃ and vacuum degassed as solution 2, then solution 2 was slowly poured into solution 1 and heated to 60℃ for 4 hours to form a casting liquid, and then an automatic coating machine was used to evenly coat it on a glass plate at a speed of 1500mm / min, and the liquid film thickness was controlled to be 100μm, and then immediately placed in a coagulation bath with a pH of 8 and a temperature of 70℃ for phase transformation into a membrane for 30 minutes. Then the membrane was immersed in the above solution for 24h to remove residual solvent and reactive porogen. Finally, the membrane was immersed in a 50% glycerol aqueous solution for 2h, and a small pore precision separation membrane was obtained after natural drying. The pore size of the obtained membrane is 20nm and has a wide distribution (10-65nm) (the pore size and pore size distribution are as follows Figure 2 and Figure 3 However, the membrane permeation flux is very low (i.e., there are few pores on the surface), only 15L / (m 2 h).
[0061] Depend on Figure 2 From the scanning electron microscope photos, it can be seen that the number of pores on the membrane surface of this comparative example is small and the pore sizes are uneven. Figure 3 As can be seen from the curve graph, the pore size distribution of the membrane is relatively wide and the surface pore size concentration is low. Therefore, it is difficult for the membrane to achieve high-throughput precision separation.
Claims
1. A method for preparing a small-pore precision separation membrane, The following steps are involved: (1) adding a film-forming polymer and an additive into a solvent, dissolving them at 20-70° C., naturally cooling them to below 60° C., and vacuum degassing them at this temperature to form a solution 1; The reactive porogen is added into the same solvent and dissolved by stirring at 20-40°C, and vacuum degassing is performed at this temperature to form solution 2; Slowly pour solution 2 into solution 1 and keep it at 40-60°C for a period of time to form a casting solution; (2) forming a solution film with a thickness of 100-500 μm from the casting solution obtained in step (1); (3) Soaking the solution membrane of step (2) in a coagulation bath with a pH value of 7-14, and leaving it in the coagulation bath for not less than 30 seconds to obtain a small-pore precision separation membrane; (4) immersing the small-pore precision separation membrane obtained in step (3) in an aqueous solution of a certain pH value at a certain temperature for 1 to 8 hours, so that the unreacted reactive porogen in step (3) is further reacted completely; (5) The small-pore precision separation membrane treated in step (4) is placed in distilled water for cleaning, and then placed in distilled water or glycerol solution for treatment and then stored.
2. The method for preparing a small-pore precision separation membrane according to claim 1, wherein in step (1), the membrane-forming polymer is one or two of polysulfone, polyethersulfone, polyvinylidene fluoride, polyvinyl chloride, polyphenylene sulfide, and polyimide; and the solvent is one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.
3. The method for preparing a small-pore precision separation membrane according to claim 1, wherein in step (1), the reactive porogen is one or more of azobisisobutyronitrile, diisopropyl azodicarboxylate, diethyl azodicarboxylate, azodicarbonamide, sodium borohydride, and p-toluenesulfonylhydrazide.
4. The method for preparing a small-pore precision separation membrane according to claim 1, wherein in step (1), the solvent ratio in solution 1 and solution 2 is 4:1, the content of film-forming polymer is 12%-30%, the content of reactive porogen is 2%-14%, and the content of auxiliary agent is 0-10%, based on the total weight of the casting solution. 5 . The method for preparing a small-pore precision separation membrane according to claim 1 , wherein in step (1), the auxiliary agent is selected from one or more of water, tetrahydrofuran, methanol, and glycerol.
6. The method for preparing a small-pore precision separation membrane according to claim 1, wherein in step (3), the pH value of the coagulation bath is 7-14, and the temperature of the coagulation bath is room temperature to 70°C.
7. The method for preparing a small-pore precision separation membrane according to claim 1, wherein in step (4), the pH value of the aqueous solution is 7-14, the immersion time is 0.5 to 48 hours, and the temperature of the aqueous solution is room temperature to 70°C.
8. The method for preparing a small-pore precision separation membrane according to claim 7, wherein the pH value of the aqueous solution is the same as the pH value of the coagulation bath in step (3).
9. The method for preparing a small-pore precision separation membrane according to claim 1, wherein the process of decomposing the reactive porogen to generate nanobubbles occurs in steps (1) to (4), or in steps (1) to (3), or in step (3).
10. A small pore precision separation membrane prepared according to the method of any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of double-layer hollow fiber loose nanofiltration membrane for dye desalination
CN113769586A
Gas-assisting film-forming method
CN103521086A
Preparation method of high-performance loose nanofiltration membrane
CN115532071A
Preparation method of high-porosity polyphenylene sulfide filter membrane
CN116617866A
Composite for silica-based film formation and silica-based film obtained from the composite
JP2007123633A