Utilization method of catalytic cracking catalyst glue residues

By activating and mixing the catalytic cracking catalyst slag, a medium-to-large pore matrix material is prepared, which is used to prepare anti-metal pollution catalytic cracking additives. This solves the problems of resource waste and molecular sieve quality fluctuations, and achieves efficient anti-metal pollution. effectiveness and stability.

CN118767908AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310323565.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-15
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

The catalytic cracking catalyst slag cannot be effectively utilized, resulting in the waste of Si, Al and other resources, and the existing methods affect the crystallinity and quality fluctuations when preparing molecular sieves.

Method used

The anti-metal additive is prepared by slurrying the catalytic cracking catalyst slag and adding acid for activation treatment, mixing the aluminum source and the magnesium source to form a medium and macroporous matrix, and then mixing it with clay and binder and spray drying.

Benefits of technology

The prepared anti-metal additive has good anti-metal vanadium pollution effect, improves the gasoline yield and conversion rate, reduces the heavy oil yield, and has stable quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004152546350000081
    Figure BDA0004152546350000081
  • Figure BDA0004152546350000082
    Figure BDA0004152546350000082
Patent Text Reader

Abstract

The invention provides a utilization method of catalytic cracking catalyst glue residues, which utilizes the glue residues to prepare a catalytic cracking vanadium-resistant auxiliary agent, and comprises the following steps: (1) pulping the catalytic cracking catalyst glue residues; (2) carrying out primary modification and activation treatment on the glue residues by using acid for a period of time; (3) mixing an aluminum source and / or a magnesium source, aging at 80-120 DEG C, drying and washing to obtain a mesoporous and macroporous matrix; and (4) mixing and pulping the macroporous silicon-aluminum matrix, a binder and clay, and carrying out spray drying and washing. According to the method, the anti-metal additive with higher heavy oil cracking performance can be prepared from the glue residues.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste utilization, and relates to a method for utilizing catalytic cracking catalyst slag and application of active silicon-aluminum material prepared therefrom. Background Art

[0002] Catalytic cracking catalyst slag is a waste slag with Al2O3 and SiO2 as main components obtained by sedimentation, filtration and slag cutting of wastewater generated in the production of catalytic cracking catalyst. At present, the slag is mainly discarded directly without reuse, resulting in waste of resources such as Si and Al. If it is utilized by adopting industrially feasible and cost-effective technical routes, it can not only reduce the environmental protection pressure of enterprises, but also help reduce production costs and improve economic benefits.

[0003] Zhang Zhimin (Research on the Recycling Technology of Catalytic Cracking Catalyst Slag, Qilu Petrochemical, 2011, 39(3): 219-222) directly used the catalyst slag as the raw material for synthesizing molecular sieves by taking advantage of the high content of silicon, aluminum and other substances in the catalyst slag. However, this method will affect the crystallinity of the molecular sieve.

[0004] The existing method uses the rubber residue to prepare the molecular sieve. Although the rubber residue can be reused, it will cause the quality of the molecular sieve to fluctuate, thus limiting its application. Summary of the invention

[0005] The purpose of the present invention is to provide a new method for utilizing catalytic cracking catalyst residue, which utilizes the catalytic cracking catalyst residue to produce a catalytic cracking anti-vanadium additive. The residue is obtained by sedimentation, filtration and residue cutting of waste water generated in the production of catalytic cracking catalyst.

[0006] The present invention provides a method for utilizing catalytic cracking catalyst residue, which comprises the following steps:

[0007] (1) slurrying the catalytic cracking catalyst residue to obtain a slurry having a solid content of 5 to 15% by weight;

[0008] (2) adding acid to the slurry obtained in step (1), adjusting the pH value to 1-5, and reacting at above 30° C. to obtain an activated residue slurry;

[0009] (3) mixing the above activated residue slurry with an aluminum source and / or a magnesium source, preferably, the pH value of the obtained mixture is 8 to 11; aging at above 80° C., drying, and washing to obtain a meso-macroporous matrix;

[0010] (4) The medium- and macroporous matrix, binder, and clay are mixed and slurried, spray-dried, and washed to obtain a catalytic cracking anti-metal additive.

[0011] A technical solution, based on the dry weight of the catalytic cracking catalyst slag, the catalytic cracking catalyst slag (referred to as slag) contains 10-50 wt% Al2O3, 30-70 wt% SiO2, 2-15 wt% Na2O and 1-15 wt% RE2O3.

[0012] According to any of the above technical solutions, in step (1), the particle size of the slurry obtained after beating is controlled at D(V, 0.5) ≤ 8 μm, such as 1-8 μm, and D(V, 0.9) ≤ 20 μm, such as 2-20 μm. The D(V, 0.9) means that the volume of particles with a particle diameter less than this value in the sample accounts for 90% of the total volume of all particles, and D(V, 0.5) means that the volume of all particles with a particle diameter less than this value accounts for 50% of the total volume of all particles. The particle size distribution is analyzed by a laser particle size analyzer, see standard NB / SH / T0951-2017.

[0013] According to any of the above technical solutions, the beating can be carried out by high-speed stirring or shearing with a shearing machine, which is well known to those skilled in the art.

[0014] According to any of the above technical solutions, the acid in step (2) can be an organic acid and / or an inorganic acid, and the organic acid can be one or more of formic acid, acetic acid, and oxalic acid, and the inorganic acid can be one or more of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.

[0015] According to any of the above technical solutions, in step (2), acid is added to the slurry obtained in step (1) to adjust the pH value to 1-5, such as 1.5-4 or 2-3. Then, the reaction is carried out at a temperature above 30°C, such as 30°C-90°C, 30-99°C or 60-90°C, and the reaction time is preferably 1-8 hours, such as stirring for 1-8 hours or 3-5 hours. The slurry residue is modified and activated by acid.

[0016] According to any of the above technical solutions, the aluminum source in step (3) is one or more of Al(NO3)3, AlCl3, Al2(SO4)3, pseudo-boehmite, and aluminum sol.

[0017] According to any of the above technical solutions, the magnesium source in step (3) is one or more of magnesium oxide, magnesium hydroxide, metallic magnesium, magnesium chloride, magnesium carbonate, and magnesium nitrate.

[0018] According to any of the above technical solutions, in step (3), the activated residue slurry is mixed with an aluminum source and / or a magnesium source. Preferably, the pH value of the resulting mixture is 8 to 11, for example, 9 to 11.

[0019] According to any of the above technical solutions, in step (3), the aging temperature is above 80° C., for example, 80 to 120° C.; and the aging time is preferably 2 to 12 hours.

[0020] According to any of the above technical solutions, the product after aging in step (3) is dried and washed to obtain a meso-macroporous matrix, wherein the washing can be carried out with water. After washing, the meso-macroporous matrix can be further dried.

[0021] According to any of the above technical solutions, preferably, the mesoporous matrix contains 0.01-3 wt % Na2O, 30-60 wt % such as 35-55 wt % Al2O3, 25-40 wt % such as 25-35 wt % SiO2, 2-15 wt % such as 4-10 wt % RE2O3 and 5-25 wt % such as 10-25 wt % MgO.

[0022] According to any of the above technical solutions, the specific surface area (BET method) of the mesoporous matrix is ​​150 to 300 m 2 / gFor example, 200-300m 2 / g.

[0023] According to any of the above technical solutions, the pore volume of the meso-macroporous matrix measured by the water drop method is 0.5 to 0.8 mL / g.

[0024] According to any of the above technical solutions, the pore size distribution is measured by low-temperature nitrogen adsorption capacity method and calculated by BJH method. For the mesoporous and macroporous matrix, the pore volume of mesoporous and macroporous pores with a pore diameter greater than 10 nm accounts for no less than 40%, for example, 45-80% of the total pore volume. The pore volume of mesoporous and macroporous pores with a pore diameter (referring to the diameter) greater than 10 nm refers to the pore volume of pores with a pore diameter greater than 10 nm and not exceeding 100 nm. The total pore volume refers to the pore volume of pores with a pore diameter greater than 0 and not exceeding 100 nm.

[0025] According to any of the above technical solutions, the clay in step (4) is one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.

[0026] In one embodiment, step (4) comprises: mixing clay, a binder and water for slurrying, adding an inorganic acid to adjust the pH value to 2.5 to 4.0, to obtain a first slurry; mixing the first slurry and the mesoporous matrix to obtain a second slurry, and spray drying, roasting and washing the obtained second slurry. For example, the roasting temperature may be 400-550° C., and the roasting time may be 1-4 hours. The additive obtained in this embodiment has a better anti-metal contamination effect, for example, after metal contamination, it can have better gasoline selectivity.

[0027] According to any of the above technical solutions, preferably, based on dry weight, the catalytic cracking anti-metal additive contains 10-40 wt % such as 15-35 wt % of clay, 20-40 wt % such as 22-35 wt % of binder and 40-70 wt % of the meso-macroporous matrix.

[0028] The present invention further provides a meso-macroporous matrix material, which contains 0.01-3 wt % of Na2O, 30-60 wt % of Al2O3, 25-40 wt % of SiO2, 2-15 wt % of RE2O3 and 5-25 wt % of MgO, and the specific surface area of ​​the meso-macroporous matrix material is preferably 150-300 m 2 / g, the pore volume by water drop method is preferably 0.5-0.8mL / g, and the pore size is greater than 10nm, and the proportion of macropores is more than 40%.

[0029] In one embodiment, the meso-macroporous matrix material is prepared according to a method comprising steps (1) to (3) of any of the above technical solutions.

[0030] The catalytic cracking catalyst slag utilization method provided by the present invention can utilize the slag to prepare a medium- and macroporous matrix material with good performance, and then utilize the material to prepare a metal-pollution-resistant catalytic cracking additive. The additive obtained by the method has a good anti-metal vanadium pollution effect. For example, after vanadium pollution, the mixture with the main catalytic cracking catalyst can have a higher gasoline yield, a higher conversion rate, and a lower heavy oil yield. The catalytic cracking anti-metal pollution additive prepared by the method has stable quality. DETAILED DESCRIPTION

[0031] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.

[0032] The used slag 1#: solid content is 25 wt%, based on the dry weight of the slag, it contains 9.0 wt% Na2O, 23.0 wt% Al2O3, 48.0 wt% SiO2, and 9.2 wt% RE2O3; it comes from China Petrochemical Catalyst Co., Ltd., and is the waste slag obtained by sedimentation, filtration and slag cutting operations of wastewater generated in the production of catalytic cracking catalysts.

[0033] Kaolin was produced by Suzhou Kaolin Company with a solid content of 72% by weight;

[0034] Pseudoboehmite was produced by Aluminum Corporation of China and had a solid content of 62.0 wt.%;

[0035] The aluminum oxide content in the aluminum sol is 21.5% by weight;

[0036] Hydrochloric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 36%;

[0037] Magnesium oxide was produced by Beijing Chemical Plant and was analytically pure;

[0038] Aluminum sulfate solution: 90 g Al2O3 / L, produced by Qilu Branch of Sinopec Catalyst Co., Ltd.;

[0039] Magnesium chloride solution: 100 g MgO / L, produced by Qilu Branch of Sinopec Catalyst Co., Ltd.

[0040] Sodium aluminate solution: 105 g Al2O3 / L, produced by Qilu Branch of Sinopec Catalyst Co., Ltd.

[0041] The specific surface area was analyzed using the NB / SH / T 0959-2017 method, and the pore size distribution was analyzed using the BJH method using the adsorption data obtained under this condition;

[0042] The composition of the samples was determined by X-ray fluorescence spectroscopy (XRF);

[0043] The apparent bulk density of catalytic cracking catalyst was determined using NB / SH / T 0954-2017;

[0044] The water drop method pore volume of catalytic cracking catalyst was determined using NB / SH / T 0955-2017;

[0045] NB / SH / T 0964-2017 was used to determine the wear index of catalytic cracking catalyst.

[0046] Preparation Example 1 of Meso-Macroporous Matrix

[0047] The glue residue 1# was slurried evenly with deionized water under high-speed stirring conditions to obtain a glue residue slurry, wherein D(V,0.5) was 3.7 microns and D(V,0.9) was 8.2 microns;

[0048] Adding hydrochloric acid to adjust the pH value of the slurry to 2, stirring for 4 hours at 90° C. to react, to obtain an activated slurry with a concentration of 100 g / L in terms of oxides (the total amount of sodium oxide, aluminum oxide, silicon oxide and rare earth oxide, wherein the rare earth oxide is calculated as RE2O3);

[0049] The activated residue slurry was mixed with sodium aluminate solution, magnesium chloride solution and aluminum sulfate solution in a volume ratio of 5:2:1:1. The pH value of the mixture was 9.1. The mixture was reacted at 120°C for 4 hours, and then dried and washed to obtain the macroporous matrix MA-1. According to analysis, the specific surface area of ​​MA-1 is 218m 2 / g, medium and large pores with a pore size greater than 10nm account for 78.3%, and the pore volume by water drop method is 0.78ml / g; in terms of weight percentage, the Na2O content is 0.16%, the Al2O3 content is 48.9%, the SiO2 content is 27.3%, the MgO content is 12.1%, and the RE2O3 content is 5.6%.

[0050] Example 2 of Preparation of Meso-Macroporous Matrix

[0051] The glue residue 1# was slurried evenly with deionized water under high-speed stirring conditions, and its D(V,0.5) was 2.6 microns and D(V,0.9) was 5.9 microns; the glue residue slurry was obtained.

[0052] Adding hydrochloric acid to adjust the pH value of the glue residue slurry to 2.5, stirring for 4 hours at 90° C. to react, to obtain an activated glue residue slurry, wherein the concentration of the activated glue residue slurry is 100 g / L in terms of oxide;

[0053] The activated residue slurry was mixed with sodium aluminate solution, magnesium chloride solution and aluminum sulfate solution in a volume ratio of 13:3:3:1. The pH value of the mixture was 10.5. The mixture was reacted at 100°C for 4 hours. After drying and washing, the macroporous matrix MA-2 was obtained. The specific surface area of ​​the matrix MA-2 was 271.2 m 2 / g, medium and large pores with pore diameters greater than 10nm account for 76.1%, the pore volume by water drop method is 0.67ml / g, and in terms of weight percentage, the Na2O content is 0.8%, the Al2O3 content is 38.2%, the SiO2 content is 34.1%, the MgO content is 17.1%, and the RE2O3 content is 6.1%.

[0054] Example 3 of Preparation of Meso-Macroporous Matrix

[0055] The glue residue 1# was slurried evenly with deionized water under high-speed stirring conditions, and its D(V,0.5) was 3.1 microns and D(V,0.9) was 7.2 microns; the glue residue slurry was obtained.

[0056] Adding hydrochloric acid to adjust the pH value of the glue residue slurry to 2.6, stirring at 90° C. for 4 hours to react, to obtain an activated glue residue slurry, wherein the concentration of the activated glue residue slurry in terms of oxide is 100 g / L;

[0057] The activated residue was mixed with sodium aluminate solution, magnesium chloride solution and aluminum sulfate solution in a volume ratio of 11:3:4.5:3. The pH value of the mixture was 10.9. The mixture was reacted at 90°C for 4 hours. After drying and washing, the medium- and macroporous matrix MA-3 was obtained. The specific surface area of ​​MA-3 was 201.3 m 2 / g, medium and large pores with pore diameters greater than 10nm account for 49.6%, and the pore volume by water drop method is 0.52ml / g; percentage content: Na2O content is 0.3%, Al2O3 content is 41.6%, SiO2 content is 25.8%, MgO content is 21.5%, and RE2O3 content is 4.9%.

[0058] Anti-vanadium additive preparation example 1

[0059] Add 0.83 kg kaolin, 1.61 kg pseudo-boehmite and 0.7 kg

[0060] The aluminum sol was stirred for 120 min, hydrochloric acid was added to adjust the pH to 3.0, and stirring was continued for 60 minutes to obtain a slurry. 4.06 kg of the above-mentioned meso-macroporous matrix MA-1 was added to the first slurry and stirred for 60 minutes to obtain a second slurry. The second slurry;

[0061] The product was spray dried at an outlet temperature of 220°C, calcined at 450°C for 2h, washed twice (each washing was carried out at a water: auxiliary agent = 10:1 (weight ratio)) and dried to obtain microspheres, which were recorded as M-1.

[0062] Examples 2 to 4 of the preparation of anti-vanadium additives

[0063] Examples 2, 3, and 4 were prepared in the same manner as Example 1, except that Examples 2, 3, and 4 were prepared with different contents of meso-macroporous matrix MA-1, MA-2, and MA-3, respectively, and were denoted as M-2, M-3, and M-4.

[0064] Preparation Example 5 of Anti-vanadium Auxiliary Agent

[0065] The amount and type of raw materials used in the preparation are the same as those in Example 2, except that the medium- and macroporous matrix material is directly mixed with deionized water, kaolin, aluminum stone and aluminum sol and stirred for 120 minutes, hydrochloric acid is added to adjust the pH to 3.0 and stirred for 60 minutes, spray-dried at an outlet temperature of 220°C, calcined at 450°C for 2h, washed twice (each washing, water: auxiliary agent = 10:1 weight ratio) and dried to obtain microspheres, recorded as M-5.

[0066] The formulas and additive properties of the anti-vanadium additive preparation examples 1 to 5 are shown in Table 1.

[0067] Matrix Preparation Comparative Example 1

[0068] The glue residue 1# was slurried evenly with deionized water under high-speed stirring conditions, and its D(V,0.5) was 3.5 microns and D(V,0.9) was 8.0 microns; the glue residue slurry was obtained.

[0069] The slurry of the slag was directly mixed with sodium aluminate solution, magnesium chloride solution and aluminum sulfate solution in the same dry basis feed ratio as in Example 1. The pH value of the mixture was 12.5. The mixture was reacted at 120°C for 4 hours, and then dried and washed to obtain the matrix DMA-1. The specific surface area of ​​DMA-1 was 162 m 2 / g, medium and large pores with pore diameters greater than 10nm account for 15.2%, the pore volume by water drop method is 0.26ml / g, the Na2O content is 0.21wt%, the Al2O3 content is 47.2wt%, the SiO2 content is 28.8wt%, the MgO content is 11.2wt%, and the RE2O3 content is 6.1wt%.

[0070] Matrix Preparation Comparative Example 2

[0071] The glue residue 1# was slurried evenly with deionized water under high-speed stirring conditions, and its D(V,0.5) was 2.6 microns and D(V,0.9) was 5.9 microns; the glue residue slurry was obtained.

[0072] Add hydrochloric acid to adjust the pH value of the slurry to 2.5, stir at 90° C. for 4 h to react, and obtain activated slurry. The concentration of the slurry after slurry modification is 100 g / L.

[0073] The activated residue was mixed with sodium aluminate solution and aluminum sulfate solution in a volume ratio of 13:3:1, reacted at 100°C for 4 hours, and then dried and washed to obtain the matrix DMA-2. The specific surface area was 149 m 2 / g, medium and large pores with pore diameters greater than 10nm account for 21.8%. The pore volume by water drop method is 0.31ml / g; the weight percentage content is 0.8% for Na2O, 42.6% for Al2O3, 46.4% for SiO2, and 7.8% for RE2O3.

[0074] Matrix Preparation Comparative Example 3

[0075] The glue residue 1# was slurried evenly with deionized water under high-speed stirring conditions, and its D(V,0.5) was 2.6 microns and D(V,0.9) was 5.9 microns; a glue residue slurry was obtained, hydrochloric acid was added, and the pH value of the glue residue slurry was adjusted to 2.6, and the mixture was stirred at 90° C. for 4 hours to react, and an activated glue residue slurry was obtained, and the concentration of the activated glue residue slurry in terms of oxide was 100 g / L;

[0076] The activated residue was mixed with sodium aluminate solution and aluminum sulfate solution in a volume ratio of 11:3:3 at 90°C for 4 hours, and then dried and washed to obtain the matrix DMA-3. The specific surface area of ​​DMA-3 was 122.9 m 2 / g, medium and large pores with pore diameters greater than 10nm account for 9.6%, and the pore volume by water drop method is 0.23ml / g; weight percentage content: Na2O content is 0.8%, Al2O3 content is 54.1%, SiO2 content is 36.4%, and RE2O3 content is 5.6%.

[0077] Comparative Example 1 of Preparation of Anti-vanadium Additive

[0078] According to the method of Example 1, the auxiliary agent DM-1 was prepared using the matrix DMA-1.

[0079] Comparative Example 2 of Preparation of Anti-vanadium Additive

[0080] 1.6 kg of kaolin, 2.02 kg of pseudo-boehmite and 0.47 kg of aluminum sol were added to 10 kg of deionized water and stirred for 120 minutes. Hydrochloric acid was added to adjust the pH to 3.0, and stirring was continued for 60 minutes to obtain a first slurry.

[0081] 2.6 kg of the above-mentioned matrix DMA-2 and 4.3 L of magnesium chloride solution were added to the first slurry, stirred for 30 minutes, spray-dried at an outlet temperature of 220°C, calcined at 450°C for 2 hours, washed twice (each washing was carried out at a ratio of water to agent = 10:1) and dried to obtain microspheres, which were recorded as DM-2.

[0082] Comparative Example 3 of Preparation of Anti-vanadium Additive

[0083] 1.6 kg of kaolin, 2.02 kg of pseudo-boehmite and 0.47 kg of aluminum sol were added to 10 kg of deionized water and stirred for 120 minutes. Hydrochloric acid was added to adjust the pH to 3.0, and stirring was continued for 60 minutes to obtain a first slurry.

[0084] 2.45 kg of the above-mentioned matrix DMA-3 and 0.55 kg of magnesium oxide were added to the first slurry, stirred for 30 minutes, spray-dried at an outlet temperature of 220°C, calcined at 450°C for 2 hours, washed twice (each washing was carried out at a ratio of water to agent = 10:1) and dried to obtain microspheres, which were recorded as DM-3.

[0085] The formulations and additive properties of comparative examples 1 to 4 of the preparation of anti-vanadium additives are shown in Table 2.

[0086] Table 1

[0087] Example 1 Example 2 Example 3 Example 4 Example 5 Additive No. M-1 M-2 M-3 M-4 M-5 Old soil 12 32 23 23 32 Aluminium 20 25 25 25 25 Aluminum sol 3 3 2 2 3 Matrix MA-1 65 40 40 Matrix MA-2 50 Matrix MA-3 50 Pore ​​volume, mL / g 0.48 0.42 0.44 0.45 0.44 Apparent bulk density, g / mL 0.66 0.71 0.67 0.68 0.68 Wear index, % / h 2.8 1.1 2.1 2.6 2.5

[0088] Table 2

[0089] Comparative Example 1 Comparative Example 2 Comparative Example 3 Additive No. DM-1 DM-2 DM-3 Old soil 32 23 23 Aluminium 25 25 25 Aluminum sol 3 2 2 Matrix DMA-1 40 Matrix DMA-2 41.4 Matrix DMA-3 39.3 Magnesium source 8.6 (Magnesium chloride) 10.7 (magnesium oxide) Pore ​​volume, mL / g 0.35 0.32 0.33 Apparent bulk density, g / mL 0.78 0.7 0.77 Wear index, % / h 5.1 3.9 6.7

[0090] In Tables 1 and 2, kaolin, diatomite, alumina sol, matrix MA-1 to MA-3, matrix DMA-1 to DMA-3 are the dry weight ratios.

[0091] Examples 1 to 5

[0092] The auxiliary agents prepared in Examples 1 to 5 were uniformly mixed with the main agent CAT-N (trade name CGP-1, produced by Sinopec Catalyst Co., Ltd.) at a weight ratio of 1:9, and then contaminated with 4000 ppm of vanadium.

[0093] Pollution method: After the catalyst mixture is introduced with heavy metal V by the Michel impregnation method, the catalyst after the introduction of heavy metal is loaded into the D-100 device (small fixed fluidized bed), and the treatment is carried out on the D-100 device according to the following steps:

[0094] (a) Heating to 600 °C at a heating rate of 20 °C / min under nitrogen atmosphere;

[0095] (b) heating to 780°C at a heating rate of 1.5°C / min, then maintaining the temperature at 780°C, and changing the treatment atmosphere during the temperature maintenance process as follows;

[0096] (i) treating the mixture for 10 minutes in an atmosphere containing 40% by volume of nitrogen (wherein the nitrogen contains 5% by volume of propylene) and 60% by volume of water vapor;

[0097] (ii) treating for 10 minutes in an atmosphere containing 40% by volume of nitrogen (pure nitrogen, propylene-free) and 60% by volume of water vapor,

[0098] (iii) treating for 10 minutes with an atmosphere containing 40% by volume of air (containing 4000 ppm SO2) and 60% by volume of water vapor,

[0099] (iv) treating with an atmosphere containing 40 volume % nitrogen and 60 volume % water vapor for 10 minutes; then repeating the cycle steps (i) to (iv) once each in the aforementioned order, and then repeating step (i) to end the cycle contamination step.

[0100] The aged catalysts were obtained by aging at 800° C. in a 100 volume % water vapor atmosphere for 4 hours, and were named CAT-M1, CAT-M2, CAT-M3, CAT-M4, and CAT-M5, respectively.

[0101] Comparative Example 1

[0102] No anti-metal additives are added to the main agent

[0103] The main agent CAT-N was contaminated with 4000 ppm of vanadium and then aged at 800° C. in a 100 volume % water vapor atmosphere for 4 hours. This was designated as CAT-NM.

[0104] Comparative Examples 2 to 4

[0105] The auxiliary agents prepared in comparative examples 1 to 3 were uniformly mixed with the main agent CAT-N in a weight ratio of 1:9, and then contaminated with 4000 ppm vanadium (the vanadium content after contamination was 4000 ppm by mass), and aged for 4 hours at 800°C and 100 volume % water vapor atmosphere to obtain aged CAT-DM1, CAT-DM2, and CAT-DM3.

[0106] Reaction evaluation

[0107] The aged vanadium-contaminated catalytic cracking catalyst and the mixture of the additive CAT-M1, CAT-M2, CAT-M3, CAT-M4, CAT-M5, CAT-DM1, CAT-DM2, CAT-DM3 and the contaminated main agent CAT-N were evaluated on the ACE device. The reaction conditions were: reaction temperature of 520 ° C, reaction weight hourly space velocity of 8h -1 , agent-oil ratio is 8 by weight, the properties of the raw oil are shown in Table 3, and the results are shown in Table 4.

[0108] Conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield

[0109] Total liquid yield = gasoline yield + liquefied gas yield + diesel yield

[0110] Table 3 Raw oil properties

[0111]

[0112] Table 4 Evaluation results

[0113]

[0114] It can be seen from the results in Table 4 that, compared with the comparative example, the catalysts mixed with the anti-vanadium additives of Examples 1 to 5 of the present invention have significantly improved conversion rates, high gasoline yields, and significantly reduced heavy oil yields.

[0115] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0116] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0117] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for utilizing catalytic cracking catalyst residue, comprising the following steps: (1) slurrying the catalytic cracking catalyst residue to obtain a slurry having a solid content of 5 to 15% by weight; (2) adding acid to the slurry obtained in step (1) to adjust the pH value of the slurry to 1-5, and reacting at above 30° C. to obtain an activated residue slurry; (3) mixing the activated residue slurry with an aluminum source and / or a magnesium source, aging at a temperature above 80° C., drying, and washing to obtain a mesoporous and macroporous matrix; (4) The medium- and macroporous matrix, binder, and clay are mixed and slurried, spray-dried, and washed to obtain a catalytic cracking anti-metal additive.

2. The method according to claim 1, wherein: The slurry obtained in step (1) has a particle size of D(V,0.5)≤8μm and D(V,0.9)≤20μm.

3. The method according to claim 1, wherein: In step (2), the pH value is 1.5-4.

4. The method according to claim 1, wherein: In step (2), the reaction temperature is 30°C to 90°C, and the reaction time is 1 to 8 hours.

5. The method according to claim 1, wherein: In step (2), the acid is an organic acid and / or an inorganic acid. The organic acid is, for example, one or more of formic acid, acetic acid, and oxalic acid. The inorganic acid is, for example, one or more of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.

6. The method according to claim 1, wherein: In step (3), the pH value of the mixture formed by mixing the activated residue slurry with the aluminum source and / or magnesium source is 8 to 11, for example, 9 to 11; the aging in step (3) has an aging temperature of 80°C to 120°C and an aging time of 2h to 12h.

7. The method according to claim 1, wherein: The aluminum source is one or more of Al(NO3)3, AlCl3, Al2(SO4)3, pseudo-boehmite, and aluminum sol; The magnesium source is one or more of magnesium oxide, magnesium hydroxide, metallic magnesium, magnesium chloride, magnesium carbonate, and magnesium nitrate; The clay is one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.

8. The method according to claim 1, wherein: Based on the dry weight of the slag, the slag contains 10 wt % to 50 wt % of Al2O3, 30 wt % to 70 wt % of SiO2, 2 wt % to 15 wt % of Na2O and 1 wt % to 15 wt % of RE2O3.

9. The method according to claim 1, wherein: The mesoporous and macroporous matrix contains 0.01 wt% to 3 wt% Na2O, 30 wt% to 60 wt%, such as 35 wt% to 55 wt% Al2O3, 25 wt% to 40 wt%, such as 25 wt% to 35 wt% SiO2, 2 wt% to 15 wt%, such as 4 wt% to 10 wt% RE2O3 and 5 wt% to 25 wt%, such as 10 wt% to 25 wt% MgO, The specific surface area of ​​the mesoporous matrix is ​​150 m 2 / g~300m 2 / gFor example 200m 2 / g~300m 2 / g, the water droplet pore volume of the meso-macroporous matrix is ​​0.5mL / g to 0.8mL / g; According to the low-temperature nitrogen adsorption capacity method, the pore volume of pores with a pore diameter greater than 10 nm in the meso-macroporous matrix accounts for no less than 40%, for example, 45-80% of the total pore volume. The pore volume of meso-macropores with a pore diameter greater than 10 nm refers to the pore volume of pores with a pore diameter greater than 10 nm and not exceeding 100 nm. The total pore volume refers to the pore volume of pores with a pore diameter greater than 0 and not exceeding 100 nm. The pore size distribution is calculated by the BJH method.

10. The method according to claim 1, wherein: Based on dry weight, the catalytic cracking anti-metal additive contains 10 wt% to 40 wt% clay, such as 15 wt% to 35 wt% clay, 20 wt% to 40 wt% binder, such as 22 wt% to 35 wt% binder and 40 wt% to 70 wt% of the meso-macroporous matrix.

11. The method according to claim 1, wherein: Step (4) comprises: mixing clay, a binder and water for slurrying, adding an inorganic acid to adjust the pH value to 2.5-4.0 to obtain a first slurry; mixing the first slurry and the mesoporous and macroporous matrix to obtain a second slurry, spray drying the second slurry, calcining and washing.

12. A meso-macroporous matrix material comprising 0.01 wt % to 3 wt % of Na2O, 30 wt % to 60 wt % of Al2O3, 25 wt % to 40 wt % of SiO2, 2 wt % to 15 wt % of RE2O3 and 5 wt % to 25 wt % of MgO; the specific surface area of ​​the meso-macroporous matrix material is 150 m 2 / g~300m 2 / g, the pore volume by water drop method is 0.5mL / g~0.8mL / g, and the pore size is greater than 10nm, and the proportion of macropores is more than 40%; one embodiment is prepared according to the method including steps (1) to (3) according to any one of claims 1 to 11.

13. Use of the meso-macroporous matrix material according to claim 12 in a vanadium-resistant additive for catalytic cracking.

Citation Information

Patent Citations

  • Preparation method of ZSM-5 molecular sieve

    CN102442686A

  • Method for preparing activated clay by harmless treatment on waste FCC(fluid catalytic cracking) catalysts

    CN106984264A

  • Catalytic cracking catalyst as well as preparation method and application thereof

    CN114425398A

  • Nano Y-type molecular sieve taking glue residue as raw material as well as preparation method and application of nano Y-type molecular sieve

    CN114620740A

  • AU2020101871A4