Preparation method of hydrofining catalyst

Through the aging pH value swing and multiple health treatments, combined with vacuum filtration technology, the problems of the pore structure and active metal distribution of the hydrorefining catalyst have been solved, and the pore structure and activity of the catalyst have been improved, making it suitable for efficient hydrogenation reactions.

CN118767934AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310336358.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

The pore structure of existing hydrorefining catalysts is not ideal, resulting in low utilization of active metals and insufficient catalyst activity. Moreover, residual sodium ions affect the shape of the catalyst and the formation of the pore structure, affecting the efficiency of the hydrogenation reaction.

Method used

The aluminum-containing solution is added in batches during the aging pH value swing gel formation process, and the impurity sodium is removed by combining specific impurity removal methods to control the size and pore size distribution of the oxide particles. The pore structure and activity of the catalyst are improved through multiple curing and vacuum filtration. Metal dispersion.

Benefits of technology

The prepared catalyst has suitable pore size distribution and high mechanical strength, and the active metal is evenly dispersed, which significantly improves the performance of hydrodesulfurization, denitrification and aromatic hydrocarbon saturation reactions, and is suitable for hydrodesulfurization and ultra-deep hydrogenation of heavy distillate oil. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a hydrofining catalyst. The preparation method comprises the following steps: (1) preparing a mixed solution A containing an Al component and nickel salt; preparing a mixed solution B of sodium tungstate and sodium molybdate; preparing a solution C containing an Al component; (2) dropwise adding the mixed solution B and an alkaline precipitator into the mixed solution A to obtain slurry D; (3) aging the slurry D, and adding the solution C in batches in the aging process to obtain slurry E; (4) performing vacuum filtration on the slurry E, and performing primary curing on a filter cake; after curing is finished, deionized water with a certain proportion m is added into a filter cake, and a vacuum suction filtration process I is carried out; carrying out secondary maintenance on the filter cake, adding deionized water in a certain proportion n into the filter cake, and carrying out a suction filtration process II to obtain a filter cake F; and (5) drying the filter cake F, carrying out extrusion molding on the dried material, and roasting to obtain the hydrofining catalyst. The catalyst disclosed by the invention has relatively high hydrogenation saturation performance, and is particularly suitable for being applied to hydrogenation dearomatization, ultra-deep desulfurization and denitrification reactions of heavy distillate oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation, and in particular relates to a method for preparing a hydrorefining catalyst with high hydrodesulfurization, hydrodenitrogenation and aromatic saturation activities. Background Art

[0002] With the gradual improvement of oil quality requirements in my country, after the sulfur content of diesel is set to below 10μg / g, the requirements for aromatic content are becoming more stringent. The most effective means to meet the requirements for diesel quality upgrade is to use high hydrogenation activity catalysts. Therefore, as one of the catalysts with the highest hydrogenation activity in the current refining market, bulk catalysts are very suitable for diesel quality upgrades in refineries due to their excellent performance.

[0003] The preparation methods of hydrotreating catalysts are generally divided into impregnation, kneading, beating, ion exchange and coprecipitation. The preparation of bulk catalysts generally adopts kneading or coprecipitation. Due to the limitations of the preparation method, the kneading method can easily make it difficult to mix the components evenly, the active metals aggregate, and cannot promote the synergistic effect between the active metals, making it difficult for the catalyst to fully exert its activity; at the same time, because the preparation of bulk catalysts is greatly affected by the difficulty of molding, it is difficult to obtain high metal content catalysts using the kneading method.

[0004] Due to the characteristics of ionic reactions, the components of the coprecipitation method can be evenly mixed; and the coprecipitation method can use relatively low-priced sodium-containing raw materials to replace some high-priced or "ammonia nitrogen"-containing raw materials, which greatly reduces the cost of catalyst raw materials and the cost of nitrogen-containing wastewater treatment. However, the introduction of a large number of sodium ions makes it difficult to completely remove sodium ions from the bulk catalyst, and a large amount of impurity sodium exists in the coprecipitated material, resulting in poor material adhesion, difficulty in molding, or poor catalyst strength after molding; at the same time, the unremoved impurity sodium is not conducive to the formation of the catalyst pore structure, resulting in a small catalyst pore volume and pore size, affecting the diffusion efficiency during the catalytic reaction; in addition, bulk catalysts with too high sodium content will also cause active metal aggregation and reduce the hydrogenation activity of the catalyst.

[0005] In the distillate oil hydrotreating reaction, in order to improve the reaction efficiency of the catalyst active site, the catalyst needs to have a larger pore size when the raw material molecules and product molecules diffuse through the catalyst pores to facilitate the smooth passage of the raw material molecules and product molecules through the catalyst pores. Although the currently developed bulk catalyst has a high content of active metals, the catalyst pore size is small, which affects the diffusion efficiency of the catalytic reaction process; at the same time, high content of active metals is prone to excessive particle deposition, which affects the morphology of MoS2 / WS2 after sulfidation, reduces the amount of active phase formed, and reduces the utilization rate of the active metal of the catalyst, resulting in waste of active metals.

[0006] CN1339985A discloses a method for preparing a mixed metal catalyst composition, and CN101153228A discloses a multi-metal bulk catalyst for ultra-deep hydrodesulfurization of diesel. The above patents all adopt a co-precipitation method to prepare hydrogenation catalysts, but the pore structures of the prepared catalysts are not ideal, and the pore volumes and pore diameters are small.

[0007] CN114471593A and CN114471594A both disclose a method for preparing a hydrorefining catalyst. This method is also prepared by coprecipitation, and a sodium salt removal treatment is performed. This method selects to remove the sodium salt after the catalyst is extruded, but in the actual catalyst preparation process, when the sodium salt content is too high, the catalyst cannot be formed or the strength after forming is small, so when this method is used, there are certain requirements for the sodium content of the catalyst preparation raw material; at the same time, due to the presence of a large amount of sodium ions in the coprecipitation reaction product, this method will precipitate part of the sodium chloride crystals attached to its internal pores during the drying process of the coprecipitation reactant, which will also have an adverse effect on the formation of the catalyst pore structure. In addition, the sodium salt is removed after the catalyst is extruded, and the drying, extrusion and other treatments of the material in the middle increase the adsorption degree of sodium ions on the catalyst, making it more difficult to remove.

[0008] CN109692693B discloses a hydrorefining catalyst and a preparation method thereof, wherein the method adopts a two-cocurrent precipitation method to prepare a mixed precipitate containing tungsten, molybdenum and nickel as active metals, and the steps of aging, drying, molding and roasting are performed in the process to successfully prepare the hydrorefining catalyst. However, the method fails to effectively control the particle size of the product during the cocurrent coprecipitation reaction, especially in the second cocurrent coprecipitation, the previous product slurry is coprecipitated again, which will cause the final product particles to aggregate excessively or the particle size to be uneven, thereby affecting the active metal distribution of the catalyst and affecting the pore structure, thereby affecting the hydrogenation activity of the catalyst.

[0009] In the co-precipitation method for preparing bulk catalysts, the precipitation method and gelation conditions will affect the catalyst pore size and active metal distribution, resulting in a reduction in the active phase of MoS2 / WS2 after sulfidation, causing the hydrogenation activity to fail to reach an ideal state. Summary of the invention

[0010] In view of the problems existing in the prior art, the present invention provides a method for preparing a hydrorefining catalyst. The present invention adopts a low-cost and environmentally friendly sodium-containing raw material to prepare a bulk hydrorefining catalyst, and adds an aluminum-containing solution in batches during the gelling process by aging pH swing, and removes the impurity sodium in combination with a specific impurity removal method. The catalyst has a suitable pore size distribution and the active metal is well dispersed. The active metal particles are uniform and the particle size is suitable, and there will be no excessive aggregation of particles. At the same time, the catalyst molding problem and the catalyst activity inhibition problem when the sodium content is high are solved, and the catalyst strength and pore structure properties are greatly improved; the bulk catalyst prepared by the method of the present invention has a high hydrogenation saturation performance, and is particularly suitable for use in heavy distillate oil hydrodearomatization, ultra-deep hydrodesulfurization, and denitrogenation reactions.

[0011] The preparation method of the hydrotreating catalyst of the present invention comprises the following contents: (1) Prepare a mixed solution A containing Al component and nickel salt; prepare a mixed solution B containing sodium tungstate and sodium molybdate; prepare a solution C containing Al component; (2) Mixed solution A is used as the bottom water for the coprecipitation reaction. Under high-speed stirring conditions, mixed solution B and an alkaline precipitant are added dropwise to mixed solution A to obtain slurry D. (3) aging the slurry D, adding solution C in 2 to 8 times during the aging process to obtain slurry E; (4) The slurry E is vacuum filtered to obtain a filter cake, and the filter cake is cured once; after the curing, a certain proportion m of deionized water is added to the filter cake, and a vacuum filtration process I is performed; the filter cake is cured twice, and a certain proportion n of deionized water is added to the filter cake, and a filtration process II is performed to obtain a filter cake F; (5) The filter cake F is dried, the dried material is extruded into strips, and the strips are calcined to obtain a hydrogenation refining catalyst.

[0012] In the method of the present invention, the nickel salt in the mixed solution A of step (1) is a soluble nickel salt, such as nickel acetate and / or nickel chloride; Ni is calculated as NiO, and the molar concentration is 0.1-1.5 mol / L, preferably 0.4-0.8 mol / L.

[0013] In the method of the present invention, the aluminum source in the mixed solution A of step (1) is aluminum chloride, and the molar concentration of Al in terms of Al2O3 is 0.1-1 mol / L, preferably 0.2-0.8 mol / L.

[0014] In the method of the present invention, in the mixed solution B of step (1), the molar concentration of sodium molybdate is 0.01-1 mol / L, preferably 0.1-0.7 mol / L. The molar concentration of sodium tungstate is 0.05-1 mol / L, preferably 0.2-0.6 mol / L.

[0015] In the method of the present invention, in the solution C of step (1), the aluminum source is one or more of sodium aluminate, aluminum sulfate, aluminum chloride and aluminum acetate; Al is calculated as Al2O3, and the molar concentration is 0.05-0.5 mol / L, preferably 0.1-0.3 mol / L.

[0016] In the method of the present invention, in step (1), solution C is preferably divided into 2 to 8 portions of equal volume.

[0017] In the method of the present invention, the alkaline precipitant in step (2) is one or more of sodium hydroxide, sodium carbonate, and sodium bicarbonate. The pH value of the prepared alkaline precipitant is not less than 12.0, and preferably the pH value is 12.5-13.8.

[0018] In the method of the present invention, in the coprecipitation reaction of step (2), the pH of the reaction solution is measured online, and the pH of the reaction system is maintained in the range of 5.5 to 7.0, preferably 6.0 to 6.5, by controlling the dropping speed of the alkaline precipitant during the reaction.

[0019] In the method of the present invention, the coprecipitation reaction temperature in step (2) is 30-90° C., preferably 40-70° C.; the reaction time is controlled to be 30-120 minutes, preferably 40-80 minutes.

[0020] In the method of the present invention, the aging temperature in step (3) is 40 to 90°C, preferably 60 to 85°C.

[0021] In the method of the present invention, during the aging process of step (3), the pH value is first controlled to 11.8-13.8 using a sodium aluminate solution, and the aging time is 0.1-0.6 hours; then, after adding 1 portion of solution C, the aging pH value is controlled to 8.6-10.2, and the aging time is 0.1-0.6 hours; then, the aging pH value is controlled to 5.5-7.0, and the aging time is 0.1-0.6 hours; the above is the complete addition process of 1 portion of solution C, and the same process is repeated until solution C is completely added.

[0022] Among them, in the aging process, except for using sodium aluminate to control the pH value to 11.8~13.8, the other acids and alkalis used to adjust the pH value can be inorganic salts, inorganic acids and inorganic bases that do not contain aluminum elements, and can be one or more of hydrochloric acid and acetic acid, sodium hydroxide, sodium carbonate, and sodium bicarbonate. The concentration and dosage are adjusted according to actual needs.

[0023] In the method of the present invention, the aluminum added in step (3) is calculated as Al2O3, and the mass fraction of Al2O3 in the prepared hydrotreating catalyst is 5% to 50%, preferably 10% to 40%.

[0024] In the method of the present invention, the humidity of the filter cake curing environment in step (4) is greater than 80%; wherein the primary curing temperature is 28°C to 45°C, preferably 35°C to 40°C; the curing time is 0.4 to 1.5 hours, preferably 0.6 to 1.2 hours. The secondary curing temperature is 55°C to 75°C, preferably 60 to 68°C; the curing time is 0.4 to 1.5 hours, preferably 0.8 to 1.2 hours.

[0025] The curing process can be carried out in any environment that meets the above conditions, preferably directly in a vacuum filtration device without moving the filter cake to simplify the process.

[0026] In the method of the present invention, after the first curing in step (4), the filter cake base is 20wt%-25wt%; after the second curing, the filter cake base is 26wt%-29wt%.

[0027] In the method of the present invention, the certain proportion m of deionized water in step (4), calculated as the ratio of the mass of deionized water to the mass of the catalyst prepared, is m>2.5, preferably 3.5-4.5:1, and the temperature of the deionized water is 28°C-45°C, preferably consistent with the primary curing temperature; the certain proportion n of deionized water, calculated as the ratio of the mass of deionized water to the mass of the catalyst prepared, is n>0.6, preferably 0.8-2.5:1, and the temperature of the deionized water is 55°C-75°C, preferably consistent with the secondary curing temperature.

[0028] In the method of the present invention, in the filtration process I and II of step (4), deionized water cannot be stirred with the filter cake, and vacuum filtration is started within 3 minutes after adding deionized water, preferably within 1 minute.

[0029] In the method of the present invention, the drying temperature of the filter cake F in step (5) is 40-90° C., preferably 55-75° C.; the drying dry basis is controlled to be 43wt%-62wt%, preferably 46wt%-56wt%.

[0030] In the method of the present invention, the calcination treatment temperature in step (5) is 350-560° C., preferably 450-510° C.; and the calcination time is 2.5-7 hours.

[0031] The present invention provides a hydrorefining catalyst, wherein the catalyst components are oxides of tungsten, molybdenum, nickel and aluminum, the active components, namely, the oxides of tungsten, molybdenum and nickel account for 50wt% to 95wt%, preferably 60wt% to 90wt%; the aluminum oxide accounts for 5wt% to 50wt%, preferably 10wt% to 40wt%; and the sodium content in the catalyst is ≯0.1%.

[0032] The hydrotreating catalyst has a W / Mo molar ratio of 1:8-12:1, preferably 1:4-6:1, and a (Mo+W) / Ni molar ratio of 1:4-10:1, preferably 1:3-8:1.

[0033] The specific surface area of ​​the hydrotreating catalyst is 260-520 m 2 / g, pore volume 0.28~0.48mL / g, mechanical strength 16.0~24.0N·mm -1 .

[0034] The pore size distribution of the hydrotreating catalyst is as follows: the pore volume of pores with a pore size of less than 4 nm accounts for 1% to 9% of the total pore volume, the pore volume of pores with a pore size of 4 to 6 nm accounts for 5% to 15% of the total pore volume, the pore volume of pores with a pore size of 6 to 10 nm accounts for 52% to 68% of the total pore volume, the pore volume of pores with a pore size of 10 to 15 nm accounts for 16% to 30% of the total pore volume, and the pore volume of pores with a pore size of more than 15 nm accounts for 3% to 12% of the total pore volume.

[0035] Preferably, the pore size distribution of the catalyst is as follows: the pore volume of pores with a pore size of less than 4 nm accounts for 2% to 6% of the total pore volume, the pore volume of pores with a pore size of 4 to 6 nm accounts for 6% to 13% of the total pore volume, the pore volume of pores with a pore size of 6 to 10 nm accounts for 54% to 64% of the total pore volume, the pore volume of pores with a pore size of 10 to 15 nm accounts for 22% to 30% of the total pore volume, and the pore volume of pores with a pore size of more than 15 nm accounts for 3% to 8% of the total pore volume.

[0036] Compared with the prior art, the present invention has the following advantages: According to the method of the present invention, during the aging process, when the pH value fluctuates, the aluminum-containing solution is added in batches, and the amorphous oxide in the oxide particles formed by coprecipitation is dissolved by the pH value fluctuation. The addition of the aluminum-containing solution re-modifies the size of the oxide particles. After the pH value fluctuates n times, the growth of the oxide particles is controlled, and the oxide particles are made more uniform and of suitable size, thereby improving the dispersion of active metals in the bulk catalyst and increasing the proportion of pore sizes of 6-10 nm and 10-15 nm in the catalyst, so that macromolecular reactants and products can pass through the pores smoothly, which is beneficial to the hydrogenation activity of the catalyst.

[0037] The method of the present invention removes the sodium impurity from the product within a short time after the aging treatment. The sodium ion has a low degree of adsorption on the material, is easier to remove, and has a high efficiency in removing impurities. At the same time, compared with the traditional pulping washing, the two curing and vacuum filtration washing in the method can achieve a small amount of water to take away a large amount of sodium impurities in the filter cake, so as to meet the requirement that the sodium content in the filter cake is ≯0.1%, reduce the number of washing times, simplify the process and greatly reduce the amount of water used for preparation. The method is used to remove the sodium impurity, which solves the problem that the bulk catalyst is not easy to form when the sodium content is too high or the mechanical strength after forming is low.

[0038] In the method of the present invention, the primary curing precipitates most of the sodium ions in the filter cake from the material, so that the large pores formed in the pH swing gelation process are retained, and the pores of the material are prevented from being occupied by impurity sodium and causing the pores of the material to be reduced. In the secondary curing process of the method of the present invention, in addition to precipitating the remaining small part of the sodium ions, the vacancies formed by the sodium removal in the primary curing, under the higher temperature and humidity environment provided by the secondary curing, the water in the filter cake quickly diffuses outward in the form of water vapor, causing an impact on the pore structure, thereby producing a pore expansion effect on the material; when the filter cake F is temperature-controlled and dried in step (5), the material has the same pore expansion effect. In addition, during the secondary curing and temperature-controlled drying of the filter cake F, since the impurity sodium in the material is removed, no sodium chloride crystals will be precipitated and attached to its internal pores to affect the pore expansion, so the pore expansion effect of sodium removal before molding is more significant than that of sodium removal after the catalyst is molded.

[0039] The hydrorefining catalyst of the present invention has good pore structure, large pore volume and suitable pore size distribution, uniform dispersion of active metal, good mechanical strength, high hydrodesulfurization, hydrodenitrogenation and aromatic saturation reaction performance, and is particularly suitable for use in ultra-deep hydrodesulfurization, denitrogenation and dearomatization reactions of heavy distillate oil. DETAILED DESCRIPTION

[0040] The technical solution of the present invention will be described clearly and completely in conjunction with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. In the catalyst test characterization method of the embodiment, the specific surface area and pore size distribution of the carrier are measured on an American ASAP-2405 BET nitrogen adsorption instrument; the elemental analysis is performed using an Agilent inductively coupled plasma mass spectrometer (7700 ICP-MS); and the crushing strength of the catalyst is measured using a particle strength tester. Example 1

[0041] Prepare mixed solution A: nickel chloride has a molar concentration of 0.60 mol / L based on NiO, and aluminum chloride has a molar concentration of 0.38 mol / L based on Al2O3. Prepare mixed solution B: sodium tungstate has a molar concentration of 0.30 mol / L, and sodium molybdate has a molar concentration of 0.75 mol / L. Prepare solution C: sodium aluminate has a molar concentration of 0.10 mol / L based on Al2O3, and divide solution C into 4 equal parts.

[0042] Solution A was heated to 70°C as reaction bottom water, and solution B and sodium hydroxide solution (pH=13.8) were added to the reaction bottom water in parallel to carry out a co-precipitation reaction. The reaction pH was controlled at 6.2-6.3, the reaction temperature was 70°C, and the reaction time was 60 min.

[0043] An aging treatment was carried out at an aging temperature of 83°C. The pH value was first adjusted to 13.5 with a sodium aluminate solution, and the aging time was 0.3 hour. Then, after adding 1 portion of solution C, the aging pH value was adjusted to 10.0, and the aging time was 0.4 hour. Then, the aging pH value was adjusted to 6.4, and the aging time was 0.2 hour. The above is the complete addition process of 1 portion of solution C. The above process was repeated 4 times to completely add solution C. The amount of Al added during the aging process, calculated as Al2O3, accounted for 25.0% of the Al2O3 component of the final catalyst, and slurry D was finally obtained.

[0044] Vacuum filter slurry D to obtain material filter cake; perform curing on the filter cake once, curing is directly performed in a vacuum filter, maintain curing environment humidity of 85%, curing temperature of 37°C, time of 1.0h, and the base of the filter cake after the first curing is 22%; add deionized water with a mass ratio of 4:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 37°C, and vacuum filter is performed after 20S until the filter cake is completely free of filtrate dripping. Continue to perform secondary curing on the filter cake, maintain curing environment humidity of 82%, curing temperature of 65°C, time of 1.2h, and the base of the filter cake after the second curing is 28%; add deionized water with a mass ratio of 2:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 65°C, and vacuum filter is performed after 30S until the filter cake is completely free of filtrate dripping, and filter cake F is obtained after washing.

[0045] The filter cake F was dried at 72°C to control the dry basis to 48%; it was extruded into clover-shaped strips and calcined at 510°C for 4 hours to obtain the final catalyst a. The main properties are shown in Table 1. Example 2

[0046] Prepare mixed solution A: nickel chloride has a molar concentration of 0.80 mol / L based on NiO, and aluminum chloride has a molar concentration of 0.15 mol / L based on Al2O3. Prepare mixed solution B: sodium tungstate has a molar concentration of 0.55 mol / L, and sodium molybdate has a molar concentration of 0.70 mol / L. Prepare solution C: aluminum chloride has a molar concentration of 0.15 mol / L based on Al2O3, and divide solution C into 6 equal parts.

[0047] Solution A was heated to 60°C as reaction bottom water, and solution B and sodium carbonate solution (pH=13.0) were added to the reaction bottom water in parallel to carry out co-precipitation reaction. The reaction pH was controlled at 5.7-5.8, the reaction temperature was 60°C, and the reaction time was 80 min.

[0048] An aging treatment was carried out at an aging temperature of 75°C. The pH value was first adjusted to 13.0 with a sodium aluminate solution, and the aging time was 0.5 hour. Then, after adding 1 portion of solution C, the aging pH value was adjusted to 9.6, and the aging time was 0.6 hour. Then, the aging pH value was adjusted to 6.0, and the aging time was 0.5 hour. The above is the complete addition process of 1 portion of solution C. The above process was repeated 6 times to completely add solution C. The amount of Al added during the aging process, calculated as Al2O3, accounted for 35.0% of the Al2O3 component of the final catalyst, and slurry D was finally obtained.

[0049] Vacuum filter slurry D to obtain material filter cake; perform curing on the filter cake once, curing is directly performed in a vacuum filter, maintain curing environment humidity of 87%, curing temperature of 31°C, time of 1.2h, and the base of the filter cake after the first curing is 23%; add deionized water with a mass ratio of 3.5:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 36°C, and vacuum filter is performed after 40S until the filter cake is completely free of filtrate dripping. Continue to perform secondary curing on the filter cake, maintain curing environment humidity of 90%, curing temperature of 60°C, time of 0.9h, and the base of the filter cake after the second curing is 26%; add deionized water with a mass ratio of 1.5:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 55°C, and vacuum filter is performed after 50S until the filter cake is completely free of filtrate dripping, and filter cake F is obtained after washing.

[0050] The filter cake F was dried at 64°C to control the dry basis to 44%; it was extruded into clover-shaped strips and calcined at 490°C for 4.5 hours to obtain the final catalyst b. The main properties are shown in Table 1. Example 3

[0051] Prepare mixed solution A: nickel chloride is calculated as 0.40 mol / L in terms of molar concentration of NiO, and aluminum chloride is calculated as 0.29 mol / L in terms of molar concentration of Al2O3. Prepare mixed solution B: sodium tungstate is calculated as 0.40 mol / L in terms of molar concentration of sodium molybdate, and sodium molybdate is calculated as 0.50 mol / L. Prepare solution C: aluminum acetate is calculated as 0.20 mol / L in terms of molar concentration of Al2O3, and divide solution C into two equal parts.

[0052] Solution A was heated to 85°C as reaction bottom water, and solution B and a mixed solution of sodium bicarbonate and sodium hydroxide (pH=12.5) were added to the reaction bottom water in parallel to carry out a co-precipitation reaction. The reaction pH was controlled at 6.4-6.5, the reaction temperature was 85°C, and the reaction time was 100 min.

[0053] An aging treatment was carried out at an aging temperature of 64°C. The pH value was first adjusted to 12.5 with a sodium aluminate solution, and the aging time was 0.6 hour. Then, after adding 1 portion of solution C, the aging pH value was adjusted to 9.2, and the aging time was 0.4 hour. Then, the aging pH value was adjusted to 6.9, and the aging time was 0.3 hour. The above is the complete addition process of 1 portion of solution C. The above process was repeated twice to completely add solution C. The amount of Al added during the aging process, calculated as Al2O3, accounted for 18.0% of the Al2O3 component of the final catalyst, and slurry D was finally obtained.

[0054] Vacuum filter slurry D to obtain material filter cake; cure the filter cake once, directly in the vacuum filter, maintain the curing environment humidity of 81%, curing temperature of 40℃, time 0.8h, the filter cake base is 25% after the first curing; add deionized water with a mass ratio of 2.6:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 40℃, and vacuum filter is performed after 80S until the filter cake is completely free of filtrate dripping. Continue to cure the filter cake twice, maintain the curing environment humidity of 92%, curing temperature of 69℃, time 0.6h, the filter cake base is 27% after the second curing; add deionized water with a mass ratio of 1.0:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 70℃, and vacuum filter is performed after 70S until the filter cake is completely free of filtrate dripping, and filter cake F is obtained after washing.

[0055] The filter cake F was dried at 58°C to control the dry basis to 53%; it was extruded into clover-shaped strips and calcined at 470°C for 6.0 h to obtain the final catalyst c. The main properties are shown in Table 1. Example 4

[0056] Prepare mixed solution A: nickel chloride is calculated as 0.3 mol / L in terms of molar concentration of NiO, and aluminum chloride is calculated as 0.23 mol / L in terms of molar concentration of Al2O3. Prepare mixed solution B: sodium tungstate is calculated as 0.25 mol / L in terms of molar concentration of sodium molybdate, and 0.61 mol / L in terms of molar concentration of sodium molybdate. Prepare solution C: sodium metaaluminate is calculated as 0.25 mol / L in terms of molar concentration of Al2O3, and divide solution C into 8 equal portions.

[0057] Solution A was heated to 40°C as reaction bottom water, and solution B and a mixture of sodium carbonate and sodium hydroxide (pH=13.4) were added to the reaction bottom water in parallel to carry out a co-precipitation reaction. The reaction pH was controlled at 6.7-6.8, the reaction temperature was 40°C, and the reaction time was 40 min.

[0058] An aging treatment was carried out at an aging temperature of 45°C. The pH value was first adjusted to 12.0 with a sodium aluminate solution, and the aging time was 0.4 hour. Then, after adding 1 portion of solution C, the aging pH value was adjusted to 8.7, and the aging time was 0.3 hour. Then, the aging pH value was adjusted to 5.7, and the aging time was 0.2 hour. The above is the complete addition process of 1 portion of solution C. The above process was repeated 8 times to completely add solution C. The amount of Al added during the aging process, calculated as Al2O3, accounted for 48.0% of the Al2O3 component of the final catalyst, and slurry D was finally obtained.

[0059] Vacuum filter slurry D to obtain material filter cake; perform curing on the filter cake once, curing is directly performed in a vacuum filter, maintain curing environment humidity at 92%, curing temperature at 43°C, time 0.6h, and filter cake base is 24% after one curing; add deionized water with a mass ratio of 5:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 30°C, and vacuum filter is performed after 120S until the filter cake is completely free of filtrate dripping. Continue to perform secondary curing on the filter cake, maintain curing environment humidity at 86%, curing temperature at 72°C, time 0.5h, and filter cake base is 28% after the secondary curing; add deionized water with a mass ratio of 2.8:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 75°C, and vacuum filter is performed after 90S until the filter cake is completely free of filtrate dripping, and filter cake F is obtained after washing.

[0060] The filter cake F was dried at 85°C to control the dry basis to 60%; it was extruded into clover-shaped strips and calcined at 500°C for 2.5 h to obtain the final catalyst d. The main properties are shown in Table 1. Example 5

[0061] Prepare mixed solution A: nickel chloride has a molar concentration of 0.50 mol / L based on NiO, and aluminum chloride has a molar concentration of 0.36 mol / L based on Al2O3. Prepare mixed solution B: sodium tungstate has a molar concentration of 0.19 mol / L, and sodium molybdate has a molar concentration of 0.35 mol / L. Prepare solution C: aluminum sulfate has a molar concentration of 0.30 mol / L based on Al2O3, and divide solution C into 5 equal portions.

[0062] Solution A was heated to 50°C as reaction bottom water, and solution B and sodium hydroxide solution (pH=12.8) were added to the reaction bottom water in parallel to carry out co-precipitation reaction. The reaction pH was controlled at 6.3-6.4, the reaction temperature was 50°C, and the reaction time was 70 min.

[0063] An aging treatment was carried out at an aging temperature of 55°C. The pH value was first adjusted to 13.2 with a sodium aluminate solution, and the aging time was 0.2 hours. Then, after adding 1 portion of solution C, the aging pH value was adjusted to 9.0, and the aging time was 0.5 hours. Then, the aging pH value was adjusted to 6.6, and the aging time was 0.6 hours. The above is the complete addition process of 1 portion of solution C. The above process was repeated 5 times to completely add solution C. The amount of Al added during the aging process, calculated as Al2O3, accounted for 33.0% of the Al2O3 component of the final catalyst, and slurry D was finally obtained.

[0064] Vacuum filter slurry D to obtain material filter cake; perform curing on the filter cake once, the curing process is carried out in an incubator, maintain the curing environment humidity at 95%, curing temperature at 34°C, time for 0.5h, and the base of the filter cake after the first curing is 21%; place the filter cake flat and seamless on the filter cloth of the vacuum filter, add deionized water with a mass ratio of 4.5:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 45°C, and vacuum filter after 160S until the filter cake is completely free of filtrate dripping. Continue to perform secondary curing on the filter cake, maintain the curing environment humidity at 96%, curing temperature at 58°C, time for 0.7h, and the base of the filter cake after the second curing is 26%; add deionized water with a mass ratio of 3.0:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 60°C, and vacuum filter after 40S until the filter cake is completely free of filtrate dripping, and filter cake F is obtained after washing.

[0065] The filter cake F was dried at 45°C to control the dry basis to 56%; it was extruded into clover-shaped strips and calcined at 480°C for 5.0 h to obtain the final catalyst e. The main properties are shown in Table 1.

[0066] Comparative Example 1 Prepare mixed solution A: the molar concentration of nickel chloride as NiO is 0.60 mol / L, and the molar concentration of aluminum chloride as Al2O3 is 0.51 mol / L. Prepare mixed solution B: the molar concentration of sodium tungstate is 0.30 mol / L, and the molar concentration of sodium molybdate is 0.75 mol / L.

[0067] Solution A was heated to 70°C as reaction bottom water, and solution B and sodium hydroxide solution (pH=13.8) were added to the reaction bottom water in parallel to carry out a co-precipitation reaction. The reaction pH was controlled at 6.2-6.3, the reaction temperature was 70°C, and the reaction time was 60 min.

[0068] An aging treatment was performed at an aging temperature of 83° C., a pH value of 6.2-6.3 during aging, and an aging time of 0.9 hour, to finally obtain slurry D.

[0069] Vacuum filter slurry D to obtain material filter cake; perform curing on the filter cake once, curing is directly performed in a vacuum filter, maintain curing environment humidity of 85%, curing temperature of 37°C, time of 1.0h, and the base of the filter cake after the first curing is 22%; add deionized water with a mass ratio of 4:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 37°C, and vacuum filter is performed after 20S until the filter cake is completely free of filtrate dripping. Continue to perform secondary curing on the filter cake, maintain curing environment humidity of 82%, curing temperature of 65°C, time of 1.2h, and the base of the filter cake after the second curing is 28%; add deionized water with a mass ratio of 2:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 65°C, and vacuum filter is performed after 30S until the filter cake is completely free of filtrate dripping, and filter cake F is obtained after washing.

[0070] The filter cake F was dried at 72°C and the dry basis was controlled to be 48%; it was extruded into clover-shaped strips and calcined at a temperature of 510°C for 4 hours to obtain the final catalyst f. The main properties are shown in Table 1.

[0071] Comparative Example 2 The other steps of this example are the same as those of Example 1, except that the impurity removal process of step (4) is not performed after the aging treatment in this comparative example.

[0072] Finally, catalyst g was obtained, and its main properties are shown in Table 1.

[0073] Comparative Example 3 The other steps of this example are the same as those of Example 1, except that in the impurity removal process of step (4) of this comparative example, the first and second curing are not performed, and the deionized water filtration processes I and II are directly performed twice.

[0074] Finally, catalyst h was obtained, and its main properties are shown in Table 1.

[0075] Comparative Example 4 The other steps of this example are the same as those of Example 1, except that in the impurity removal process of step (4) of this comparative example, the humidity of the secondary curing environment is 50% and the curing temperature is 30°C.

[0076] The final catalyst i was obtained, and its main properties are shown in Table 1.

[0077] Comparative Example 5 According to the method disclosed in CN114471594A, the catalyst composition is referred to Example 1, and the catalyst j is prepared. The specific process is as follows: a mixed solution P containing nickel chloride, aluminum chloride solution, citric acid and propylene glycol is prepared, wherein the mass concentration of Ni in the mixed solution is 26 g / L as NiO, the mass concentration of Al in Al2O3 is 30 g / L, the molar ratio of citric acid to propylene glycol is 1.0, and the molar ratio of the total number of moles of citric acid and propylene glycol to Ni is 1.2. 500 mL of deionized water is added to the reaction tank as the reaction bottom water, and 12 wt% sodium hydroxide solution, sodium tungstate and sodium molybdate solution (the mass concentration of W in WO3 is 20 g / L, and the mass concentration of Mo in MoO3 is 30 g / L) and the mixed solution P are added to the reaction tank in parallel, the gelling reaction temperature is 60°C, the reaction pH is 7.6, and the gelling time is 60 minutes to obtain a precipitate slurry.

[0078] The slurry was aged at 72°C, 7.8 pH value and 2 hours. The slurry was filtered, and the obtained filter cake was dried at 80°C for 10 hours, rolled and extruded.

[0079] The impurity sodium was removed from the molded strips: the molded strips were cured at 85°C for 48 hours, then cooled to 28°C, and continued to be cured for 30 hours, washed twice with deionized water, the ratio of deionized water to catalyst preparation mass was 5:1, and then dried and calcined. The main properties of catalyst j are shown in Table 1. Example 6

[0080] This example is an activity evaluation experiment of catalysts prepared in different embodiments and comparative examples of the present invention. Catalysts a, b, c of the present invention and catalysts f, h, i, j of comparative examples were used. The catalyst of comparative example g was not tested for activity evaluation because its mechanical strength was too low and it was not within the catalyst performance index range. The evaluation test was conducted on a 200mL small hydrogenation device.

[0081] Evaluation conditions: total reaction pressure 6.8MPa, hydrogen-oil volume ratio 500:1, volumetric space velocity 1.5h -1 , reaction temperature 365°C, main properties of raw materials used for evaluation are shown in Table 2, and Table 3 lists the catalyst evaluation results.

[0082] Evaluation results in Table 3 show that the hydrodesulfurization, hydrodenitrogenation, and aromatic saturation performances of catalysts a and b prepared by the present invention are better than those of comparative example j. The pore structure of the bulk catalyst prepared by the method of the present invention is significantly improved, the pore volume and specific surface area are larger, the pore distribution moves toward the macropore direction, and the catalyst pore distribution is good, so the catalyst hydrogenation activity is significantly improved. The hydrogenation activity of catalyst a is better than that of comparative example f, indicating that the pH swing gelation in the aging process of the method of the present invention has a good effect on adjusting the pore structure of the catalyst, and the movement of the pore distribution toward the macropore direction promotes the hydrogenation activity of the catalyst. The hydrogenation activity of catalyst a is better than that of comparative examples h and i, indicating that the subsequent sodium removal treatment in the method of the present invention not only has a good sodium removal effect on the catalyst, but also the pore expansion effect of the secondary health care promotes the hydrogenation activity of the catalyst.

[0083] Table 1 Composition and properties of catalysts prepared in Examples and Comparative Examples Catalyst No. a b c d e f g h i j Catalyst composition <![CDATA[MoO3,wt%]]> 42 32 24 28 14 42 42 42 42 42 <![CDATA[WO3,wt%]]> 28 40 30 18 12 28 28 28 28 28 NiO,wt% 14 20 21 18 30 14 14 14 14 14 <![CDATA[Al2O3,wt%]]> margin margin margin margin margin margin margin margin margin margin Na, ppm 144 253 421 219 376 169 86463 2312 635 1577 <![CDATA[Specific surface area, m 2 / g]]> 407 392 412 417 431 401 115 396 402 382 Pore ​​volume, mL / g 0.458 0.426 0.440 0.432 0.469 0.423 0.122 0.439 0.453 0.405 Pore ​​distribution, % <4nm 4.23 8.20 6.14 6.28 3.17 7.31 25.59 6.17 6.16 8.64 4nm~6nm 10.62 14.92 12.83 14.48 8.25 16.59 53.87 13.31 12.29 18.72 6nm~10nm 57.58 52.76 54.60 53.39 55.32 52.72 10.43 53.89 55.61 49.34 10nm~15nm 22.32 20.48 22.19 21.70 25.90 18.24 8.91 21.62 21.89 17.88 >15nm 5.25 3.64 4.24 4.15 7.36 5.14 1.20 5.01 4.05 5.42 Mechanical strength, N / mm 19.4 17.7 21.4 21.9 20.3 19.8 3.7 19.0 20.2 13.5 Table 2 Raw oil properties Crude oil Diesel Fuel Straight firewood / coke firewood / catalyzed firewood, % 32 / 37 / 31 Secondary processed diesel, % 68 <![CDATA[Density (20 °C) / g•cm -3 > 0.8763 Distillation range / ℃ (IBP~FBP) 149~372 Sulfur / µg•g-1 14203 Nitrogen µg•g-1 846 Aromatics, % 45.9 PAHs, % 24.1 Cetane Index 32.5 Table 3 Catalyst evaluation test results Catalyst No. a b f h i j <![CDATA[Generated oil density (20 °C), g / cm 3 > 0.8535 0.8514 0.8546 0.8553 0.8540 0.8559 S, µg / g 7.9 5.2 10.7 13.2 9.6 14.1 N, µg / g 5.7 3.4 6.8 7.4 6.1 7.8 Aromatics, wt% 27.5 27.0 28.1 28.5 27.7 28.8 PAHs, wt% 4.9 4.4 5.6 6.3 5.1 6.5 Cetane number 41.5 42.1 40.8 40.6 41.2 40.2

Claims

1. A method for preparing a hydrotreating catalyst, characterized in that The method comprises the following contents: (1) preparing a mixed solution A containing an Al component and a nickel salt; preparing a mixed solution B containing sodium tungstate and sodium molybdate; preparing a solution C containing an Al component; (2) using the mixed solution A as the bottom water for the coprecipitation reaction, and adding the mixed solution B and an alkaline precipitant to the mixed solution A in parallel under high-speed stirring conditions to obtain a slurry D; (3) aging the slurry D, and adding the solution C in 2 to 8 times during the aging process to obtain a slurry E; (4) vacuum filtering the slurry E to obtain a filter cake, and performing a curing process on the filter cake; after the curing process, adding a certain proportion m of deionized water to the filter cake to perform a vacuum filtration process I; continuing to perform a secondary curing on the filter cake, adding a certain proportion n of deionized water to the filter cake to perform a filtration process II to obtain a filter cake F; (5) drying the filter cake F, extruding the dried material into strips, and calcining the formed material to obtain a hydrogenation refining catalyst.

2. The method according to claim 1, characterized in that: The nickel salt in the mixed solution A of step (1) is a soluble nickel salt, Ni is calculated as NiO, and the molar concentration is 0.1-1.5 mol / L.

3. The method according to claim 1, characterized in that: The aluminum source in the mixed solution A of step (1) is aluminum chloride, Al is calculated as Al2O3, and the molar concentration is 0.1-1 mol / L.

4. The method according to claim 1, characterized in that: In the mixed solution B of step (1), the molar concentration of sodium molybdate is 0.01-1 mol / L, and the molar concentration of sodium tungstate is 0.05-1 mol / L.

5. The method according to claim 1, characterized in that: In the solution C of step (1), the aluminum source is one or more of sodium aluminate, aluminum sulfate, aluminum chloride and aluminum acetate; Al is calculated as Al2O3 and the molar concentration is 0.05-0.5 mol / L.

6. The method according to claim 1, characterized in that: Step (2) According to the number of additions during the aging process, solution C is divided into 2 to 8 portions, preferably divided into 2 to 8 portions of equal volume.

7. The method according to claim 1, characterized in that: The alkaline precipitant in step (2) is one or more of sodium hydroxide, sodium carbonate, and sodium bicarbonate. The pH value of the prepared alkaline precipitant is not less than 12.0, and the preferred pH value is 12.5-13.

8.

8. The method according to claim 1, characterized in that: In the coprecipitation reaction of step (2), the pH of the reaction solution is measured online, and the pH of the reaction system is maintained in the range of 5.5 to 7.0 by controlling the dropping speed of the alkaline precipitant during the reaction.

9. The method according to claim 1, characterized in that: The coprecipitation reaction temperature in step (2) is 30-90° C., and the reaction time is controlled at 30-120 minutes.

10. The method according to claim 1, characterized in that: The aging temperature in step (3) is 40 to 90°C.

11. The method according to claim 1, characterized in that: During the aging process of step (3), the pH value is first controlled to 11.8-13.8 with sodium aluminate solution, and the aging time is 0.1-0.6 hours; then, after adding 1 portion of solution C, the aging pH value is controlled to 8.6-10.2, and the aging time is 0.1-0.6 hours; then, the aging pH value is controlled to 5.5-7.0, and the aging time is 0.1-0.6 hours; the above process is repeated until all portions of solution C are completely added.

12. The method according to claim 1, characterized in that: During the aging process, except for using sodium aluminate to control the pH value to 11.8-13.8, the other acids and alkalis used to adjust the pH value are inorganic salts, inorganic acids and inorganic alkalis that do not contain aluminum elements.

13. The method according to claim 1, characterized in that: The aluminum added in step (3) is calculated as Al2O3, and the mass fraction of Al2O3 in the prepared hydrotreating catalyst is 5% to 50%.

14. The method according to claim 1, characterized in that: The humidity of the filter cake curing environment in step (4) is greater than 80%; wherein the primary curing temperature is 28°C to 45°C, preferably 35°C to 40°C; the curing time is 0.4 to 1.5 hours, preferably 0.6 to 1.2 hours; the secondary curing temperature is 55°C to 75°C, preferably 60 to 68°C; the curing time is 0.4 to 1.5 hours, preferably 0.8 to 1.2 hours.

15. The method according to claim 1, characterized in that: After the first curing in step (4), the filter cake base is 20wt%~25wt%; after the second curing, the filter cake base is 26wt%~29wt%.

16. The method according to claim 1, characterized in that: In step (4), the deionized water in a certain proportion m is calculated by the ratio of the mass of deionized water to the mass of the catalyst preparation, m>2.5, preferably 3.5-4.5:1, and the deionized water temperature is 28°C-45°C, preferably consistent with the primary curing temperature; the deionized water in a certain proportion n is calculated by the ratio of the mass of deionized water to the mass of the catalyst preparation, n>0.6, preferably 0.8-2.5:1, and the deionized water temperature is 55°C-75°C, preferably consistent with the secondary curing temperature.

17. The method according to claim 1, characterized in that: In the filtration process I and II of step (4), the deionized water is not stirred with the filter cake, and vacuum filtration is started within 3 minutes after the deionized water is added, preferably within 1 minute.

18. The method according to claim 1, characterized in that: The drying temperature of the filter cake F in step (5) is 40-90° C., preferably 55-75° C.; the dry basis is controlled to be 43wt%-62wt%, preferably 46wt%-56wt%.

19. The method according to claim 1, characterized in that: The calcination temperature in step (5) is 350-560° C. and the calcination time is 2.5-7 hours.

20. A hydrotreating catalyst prepared by the method according to any one of claims 1 to 19, characterized in that: The catalyst components are oxides of tungsten, molybdenum, nickel and aluminum, wherein the oxides of active components tungsten, molybdenum and nickel account for 50wt%~95wt%, preferably 60wt%~90wt%; aluminum oxide accounts for 5wt%~50wt%, preferably 10wt%~40wt%; and the sodium content in the catalyst is ≯0.1%.

21. The hydrotreating catalyst according to claim 20, characterized in that: The molar ratio of W / Mo is 1:8-12:1, preferably 1:4-6:1, and the molar ratio of (Mo+W) / Ni is 1:4-10:1, preferably 1:3-8:

1.

22. The hydrotreating catalyst according to claim 20, characterized in that: The specific surface area of ​​the hydrotreating catalyst is 260-520 m 2 / g, pore volume 0.28~0.48mL / g, mechanical strength 16.0~24.0N·mm -1 .

23. The hydrotreating catalyst according to claim 20, characterized in that: The pore size distribution of the hydrotreating catalyst is as follows: the pore volume of pores with a pore size of less than 4 nm accounts for 1% to 9% of the total pore volume, the pore volume of pores with a pore size of 4 to 6 nm accounts for 5% to 15% of the total pore volume, the pore volume of pores with a pore size of 6 to 10 nm accounts for 52% to 68% of the total pore volume, the pore volume of pores with a pore size of 10 to 15 nm accounts for 16% to 30% of the total pore volume, and the pore volume of pores with a pore size of more than 15 nm accounts for 3% to 12% of the total pore volume.

24. The hydrotreating catalyst according to claim 20 or 23, characterized in that: The pore size distribution of the catalyst is as follows: the pore volume with a pore size below 4nm accounts for 2%~6% of the total pore volume, the pore volume with a pore size of 4~6nm accounts for 6%~13% of the total pore volume, the pore volume with a pore size of 6~10nm accounts for 54%~64% of the total pore volume, the pore volume with a pore size of 10~15nm accounts for 22%~30% of the total pore volume, and the pore volume with a pore size above 15nm accounts for 3%~8% of the total pore volume.

Citation Information

Patent Citations

  • Hydrotreatment catalyst and preparation method thereof

    CN102319572A

  • Preparation method of residual oil hydro-treatment catalyst

    CN103769179A

  • Preparation method of hydrofining catalyst

    CN114433116A

  • Preparation method of heavy diesel oil fraction hydrofining catalyst

    CN114433117A

  • Preparation method of hydrofining catalyst

    CN114471595A