High-flow, low-ash binder for metal injection molding and preparation method thereof
By using high-flow low-ash adhesive containing specific additives in metal injection molding, the problems of insufficient flowability and high ash content of traditional adhesives are solved, the compactness and mechanical properties of the molded parts are improved, and the defect rate and Highly efficient degreasing.
Patent Information
- Application Number
- CN202411240550.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Inadequate fluidity of traditional adhesives in metal injection molding leads to uneven filling and poor molding accuracy, high ash content leads to difficulty in post-processing and degradation of molded parts performance, limiting the expansion of MIM technology in high-precision and high-performance parts applications.
Using a high flow low ash binder, including wax, polymer matrix and specific structure additives, prepared by copolymerization and hydrolysis reaction, the additive contains an appropriate amount of carboxyl polar functional groups and oil-based functional groups to improve the binder's Flowability and adhesion, and quickly remove during degreasing to reduce defects.
The compactness and mechanical properties of the molded parts are significantly improved, defects and ash residues during degreasing are reduced, and low defect rate and efficient degreasing are achieved.
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of binders, and in particular to a high-flow, low-ash binder for metal injection molding and a preparation method thereof. Background Art
[0002] In the field of metal injection molding (MIM) technology, the role of binders is crucial. It not only determines the fluidity and formability of metal powders, but also directly affects the density, strength and microstructure of molded parts. Although traditional binders meet the basic requirements of the MIM process to a certain extent, there are still some problems that are difficult to overcome. Insufficient fluidity can lead to uneven distribution of metal powders in the mold, forming holes and defects, affecting the consistency and reliability of the product. In addition, binders with high ash content are difficult to completely remove during the degreasing process, and the residual ash will affect the mechanical properties and surface quality of the product, increasing the difficulty and cost of post-processing.
[0003] The existence of these problems limits the application of MIM technology in the manufacture of high-precision, high-performance parts. Especially in the fields of aerospace, medical equipment, precision instruments, etc., the precision and performance requirements of parts are extremely high, and the limitations of traditional adhesives have become a major bottleneck restricting the development of MIM technology. Therefore, developing new high-performance adhesives, improving the molding accuracy and product quality of the MIM process, and reducing the difficulty of post-processing have become an important research direction in this field. This can not only expand the application scope of MIM technology, but also enhance its competitiveness in modern manufacturing. Summary of the invention
[0004] In view of the shortcomings of the above-mentioned technologies, the present invention provides a high-flow, low-ash binder for metal injection molding, which aims to solve the problems of uneven filling and poor molding precision caused by insufficient fluidity of traditional binders, as well as difficulties in post-processing and decreased performance of molded parts caused by high ash content. The binder of the present invention not only significantly reduces the occurrence of defects such as cracks and blistering during the degreasing process, reduces internal stress, and improves degreasing efficiency, but also ensures that the molded parts have high density and excellent mechanical properties, achieving a low defect rate.
[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0006] A high-flow, low-ash binder for metal injection molding, the binder comprising wax, a polymer matrix, an auxiliary agent and an additive shown in structural formula I;
[0007] ;
[0008] In the formula, R1 is an alkane group having 4 to 7 carbon atoms, R2 is H or methyl, R3 is an alkane group having 17 to 32 carbon atoms, and a / b is 1 to 5:1.
[0009] As a preferred technical solution, the additive is first obtained by copolymerization of maleic anhydride, diene and long-chain acrylic ester, and then by hydrolysis under acidic conditions.
[0010] As a preferred technical solution, the diene is at least one of butadiene, isoprene and 3,3-dimethyl-1,4-pentadiene.
[0011] As a preferred technical solution, the long-chain acrylate is at least one of heptadecyl acrylate, 2-methylheptadecyl acrylate, 2-methylheptadecyl methacrylate, octadecyl methacrylate, 2-methyloctadecyl acrylate, 2-methyloctadecyl methacrylate, 2-methylnonadecyl methacrylate, eicosyl acrylate, heneicosyl acrylate, heneicosyl methacrylate, tetracosyl acrylate, hexacosyl methacrylate, hexacosyl acrylate, triacontyl acrylate, triacontyl acrylate, and triacontyl acrylate.
[0012] As a preferred technical solution, the wax is at least one of paraffin wax, microcrystalline wax and synthetic wax.
[0013] As a preferred technical solution, the polymer matrix is composed of at least one of polypropylene, low-density polyethylene and medium-density polyethylene and metallocene polyethylene.
[0014] As a preferred technical solution, the auxiliary agent is at least one of a surfactant, a lubricant, and a stabilizer.
[0015] As a preferred technical solution, the mass ratio of the wax, polymer matrix, auxiliary agent and additive is 7-12:60-90:3-8:15-20.
[0016] Another aspect of the present invention is to provide a method for preparing the high-flow, low-ash binder for metal injection molding as described above, the preparation method comprising the following steps:
[0017] S1: copolymerizing maleic anhydride, diene and long-chain acrylate in a reactor containing a solvent to obtain a grafted anhydride and oil-based copolymer;
[0018] S2: dissolving the copolymer obtained in step S1 in a suitable solvent, then adding an acidic substance to adjust the pH value to 4.8-5.2, and performing a hydrolysis reaction to obtain the desired additive;
[0019] S3: The additive obtained in step S2 is stirred and mixed evenly with the wax, the polymer matrix and the auxiliary agent to obtain the high-flow and low-ash binder.
[0020] The compounded additive of the present invention enables the binder of the present invention to contain an appropriate amount of carboxyl polar functional groups, which not only enhances the adhesion with the metal powder, improves the density and mechanical properties of the molded part, but also improves the decomposition and volatility of the binder during the degreasing process, helps to reduce the residues during the degreasing process, thereby reducing the defect rate of the molded part. At the same time, the additive of the present invention contains a certain amount of C17-C35 wax base, which not only improves the lubricity and fluidity of the binder, ensures the uniform distribution of the metal powder during the injection molding process, but also helps to quickly remove it in the middle of the degreasing process due to its volatility during the degreasing process, thereby reducing the internal stress and defects of the molded part. The binder of the present invention, in which the additive is compounded with wax and polymer matrix, has the characteristic of being quickly removed during the degreasing process without forming defects in the injection-molded green parts; specifically, in the binder formula of the present invention, the wax, additive and polymer matrix are successively removed from the metal injection molding mold during different degreasing stages without causing defects in the metal green parts; because the wax can be first removed by solvent degreasing, and then the oil-based grafted additive degrades before the additive main chain and the polymer matrix in the solvent and at a certain temperature, and is removed from the metal green parts; in the final stage, a thermal degreasing operation is performed by heating to degrade the additive main chain and the polymer matrix; the present invention can combine the subsequent solvent degreasing and thermal degreasing methods through the compounding of additives, so that in the initial stage of thermal degreasing, the metal green parts have a small number of open holes, and then the degradation products generated in the subsequent thermal degreasing process escape from the open holes without forming defects such as cracks and bubbles, and at the same time, stress defects are not generated due to the high-temperature burning of the polymer matrix.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The high-flow, low-ash binder for metal injection molding of the present invention contains an appropriate amount of carboxyl polar functional groups and oil-based functional groups through its innovative additive molecular structure, which advantageously takes into account the high flowability of the binder and the adhesion to the metal powder. This structure not only ensures uniform filling during the injection molding process and improves the molding accuracy, but also effectively reduces the ash residue during the degreasing process through high decomposition volatility, reduces the occurrence of defects such as cracks and blistering, and reduces internal stress. In addition, the precise ratio of wax, additives and polymer matrix in the binder formula of the present invention optimizes the degreasing efficiency, realizes the efficient synergy of subsequent solvent degreasing and thermal degreasing, avoids the defects of metal green parts during the degreasing process, improves the density and mechanical properties of the molded parts, and realizes a low defect rate. DETAILED DESCRIPTION
[0023] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0024] Example 1
[0025] The method for preparing a high-flow, low-ash binder for metal injection molding in this embodiment comprises the following steps:
[0026] S1: maleic anhydride, butadiene and heptadecyl acrylate monomers in a molar ratio of 2:3:1 are added to a reactor containing xylene solvent to carry out copolymerization reaction; before the reaction starts, 0.5wt% of free radical initiator dibenzoyl peroxide is added to the reaction system, the reaction temperature is controlled to be 70°C, and the reaction time is 6h; during the reaction, nitrogen is introduced to exclude oxygen and prevent the occurrence of oxidation reaction. After the reaction is completed, the unreacted monomers, solvents and initiator residues are removed through post-treatment steps such as solvent evaporation, filtration, washing and drying, thereby obtaining the target product grafted anhydride and oil-based copolymer.
[0027] S2: Dissolve 25 g of the grafted anhydride and oil-based copolymer obtained in step S1 in 250 mL of ethyl acetate, then add an acid solution consisting of acetic acid and water in a volume ratio of 2:1, adjust the pH value to 5, and carry out a hydrolysis reaction at room temperature. Maintain a stirring speed of 500 rpm for 3 hours. After the reaction is completed, filter, wash, and dry to obtain the desired additive.
[0028] S3: Stir and mix the additive obtained in step S2 with paraffin wax, low-density polyethylene, metallocene polyethylene and auxiliary agent to obtain the high-flow low-ash binder. The mass ratio of the paraffin wax, low-density polyethylene, metallocene polyethylene, auxiliary agent and additive is 12:20:40:8:20. The auxiliary agent is composed of a surfactant polyvinyl pyrrolidone, a lubricant calcium stearate and a stabilizer bis(2,4-di-tert-butylphenyl) phosphate in a mass ratio of 3:1:2.
[0029] The test results show that the adhesive of this embodiment has a melt index of 20 g / 10 min measured by a melt index tester at a test temperature of 150° C. and a test pressure according to ASTM D1238. After being heated to constant weight in a high-temperature furnace at 600° C., the ash content of the adhesive is less than 0.5%.
[0030] In the degreasing test, n-hexane was first used as the solvent for solvent degreasing at room temperature for 60 minutes, then thermal degreasing was performed at a thermal degreasing temperature of 150°C for 60 minutes, and finally thermal degreasing was performed at a thermal degreasing temperature of 180°C for 120 minutes, with a degreasing efficiency of 96.2%. At the same time, 20 molded parts were visually and dimensionally inspected, and no appearance defects were found.
[0031] Example 2
[0032] The method for preparing a high-flow, low-ash binder for metal injection molding in this embodiment comprises the following steps:
[0033] S1: maleic anhydride, isoprene and 2-methylheptadecyl acrylate monomers in a molar ratio of 1:2:1 are added to a reactor containing xylene solvent to carry out copolymerization reaction; before the reaction starts, 0.5wt% of free radical initiator dibenzoyl peroxide is added to the reaction system, the reaction temperature is controlled to be 80°C, and the reaction time is 4h; during the reaction, nitrogen is introduced to exclude oxygen and prevent the occurrence of oxidation reaction. After the reaction is completed, the unreacted monomers, solvents and initiator residues are removed through post-treatment steps such as solvent evaporation, filtration, washing and drying, thereby obtaining the target product grafted anhydride and oil-based copolymer.
[0034] S2: Dissolve 25 g of the grafted anhydride and oil-based copolymer obtained in step S1 in 250 mL of ethyl acetate, then add an acid solution consisting of acetic acid and water in a volume ratio of 2:1, adjust the pH value to 4.8, and carry out a hydrolysis reaction at room temperature. Maintain a stirring speed of 500 rpm for 2 hours. After the reaction is completed, filter, wash, and dry to obtain the desired additive.
[0035] S3: The additive obtained in step S2 is stirred and mixed evenly with microcrystalline wax, polypropylene, metallocene polyethylene and auxiliary agent to obtain the high-flow low-ash binder. The mass ratio of the microcrystalline wax, polypropylene, metallocene polyethylene, auxiliary agent and additive is 7:25:50:3:15. The auxiliary agent is the same as that in Example 1.
[0036] The test results show that the adhesive of this embodiment has a melt index of 21 g / 10 min measured by a melt index tester at a test temperature of 150° C. and a test pressure according to ASTM D1238. After being heated to constant weight in a high-temperature furnace at 600° C., the ash content of the adhesive is less than 0.5%.
[0037] In the degreasing test, n-hexane was first used as the solvent for solvent degreasing at room temperature for 60 minutes, then thermal degreasing was performed at a thermal degreasing temperature of 150°C for 60 minutes, and finally thermal degreasing was performed at a thermal degreasing temperature of 180°C for 120 minutes, with a degreasing efficiency of 95.8%. At the same time, 20 molded parts were visually and dimensionally inspected, and no appearance defects were found.
[0038] Example 3
[0039] The method for preparing a high-flow, low-ash binder for metal injection molding in this embodiment comprises the following steps:
[0040] S1: maleic anhydride, 3,3-dimethyl-1,4-pentadiene and 2-methyloctadecyl methacrylate monomers in a molar ratio of 3:4:1 are added to a reactor containing xylene solvent to carry out copolymerization reaction; before the reaction starts, 0.5wt% of free radical initiator dibenzoyl peroxide is added to the reaction system, the reaction temperature is controlled to be 90°C, and the reaction time is 4h; during the reaction, nitrogen is introduced to exclude oxygen and prevent the occurrence of oxidation reaction. After the reaction is completed, the unreacted monomers, solvents and initiator residues are removed through post-treatment steps such as solvent evaporation, filtration, washing and drying, thereby obtaining the target product grafted anhydride and oil-based copolymer.
[0041] S2: Dissolve 25 g of the grafted anhydride and oil-based copolymer obtained in step S1 in 250 mL of ethyl acetate, then add an acid solution consisting of acetic acid and water in a volume ratio of 2:1, adjust the pH value to 5.2, and carry out a hydrolysis reaction at room temperature. Maintain a stirring speed of 500 rpm for 4 hours. After the reaction is completed, filter, wash, and dry to obtain the desired additive.
[0042] S3: The additive obtained in step S2 is stirred and mixed evenly with synthetic wax, medium density polyethylene, metallocene polyethylene and auxiliary agent to obtain the high flow and low ash binder. The mass ratio of the synthetic wax, medium density polyethylene, metallocene polyethylene, auxiliary agent and additive is 10:30:40:5:15. The auxiliary agent is the same as that in Example 1.
[0043] The test results show that the binder of this embodiment has a melt index of 22 g / 10 min measured by a melt index tester at a test temperature of 150° C. and a test pressure according to ASTM D1238. After being heated to constant weight in a high-temperature furnace at 600° C., the ash content of the binder is less than 0.5%.
[0044] In the degreasing test, n-hexane was first used as the solvent for solvent degreasing at room temperature for 60 minutes, then thermal degreasing was performed at a thermal degreasing temperature of 150°C for 60 minutes, and finally thermal degreasing was performed at a thermal degreasing temperature of 180°C for 120 minutes, with a degreasing efficiency of 93.7%. At the same time, 20 molded parts were visually and dimensionally inspected, and no appearance defects were found.
[0045] Example 4
[0046] The method for preparing a high-flow, low-ash binder for metal injection molding in this embodiment comprises the following steps:
[0047] S1: maleic anhydride, butadiene and eicosyl acrylate monomers in a molar ratio of 4:5:1 are added to a reactor containing xylene solvent to carry out copolymerization; before the reaction begins, 0.5wt% of free radical initiator dibenzoyl peroxide is added to the reaction system, the reaction temperature is controlled to be 70°C, and the reaction time is 8h; during the reaction, nitrogen is introduced to exclude oxygen and prevent the occurrence of oxidation reaction. After the reaction is completed, the unreacted monomers, solvents and initiator residues are removed through post-treatment steps such as solvent evaporation, filtration, washing and drying, thereby obtaining the target product grafted anhydride and oil-based copolymer.
[0048] S2: Dissolve 25 g of the grafted anhydride and oil-based copolymer obtained in step S1 in 250 mL of ethyl acetate, then add an acid solution consisting of acetic acid and water in a volume ratio of 2:1, adjust the pH value to 4.8, and carry out a hydrolysis reaction at room temperature. Maintain a stirring speed of 500 rpm for 3 hours. After the reaction is completed, filter, wash, and dry to obtain the desired additive.
[0049] S3: Stir and mix the additive obtained in step S2 with paraffin wax, medium density polyethylene, metallocene polyethylene and auxiliary agent to obtain the high fluidity low ash binder. The mass ratio of the paraffin wax, medium density polyethylene, metallocene polyethylene, auxiliary agent and additive is 12:25:45:3:15. The auxiliary agent is the same as that in Example 1.
[0050] The test results show that the adhesive of this embodiment has a melt index of 21 g / 10 min measured by a melt index tester at a test temperature of 150° C. and a test pressure according to ASTM D1238. After being heated to constant weight in a high-temperature furnace at 600° C., the ash content of the adhesive is less than 0.5%.
[0051] In the degreasing test, n-hexane was first used as the solvent for solvent degreasing at room temperature for 60 minutes, then thermal degreasing was performed at a thermal degreasing temperature of 150°C for 60 minutes, and finally thermal degreasing was performed at a thermal degreasing temperature of 180°C for 120 minutes, with a degreasing efficiency of 95.1%. At the same time, 20 molded parts were visually and dimensionally inspected, and no appearance defects were found.
[0052] Example 5
[0053] The method for preparing a high-flow, low-ash binder for metal injection molding in this embodiment comprises the following steps:
[0054] S1: maleic anhydride, isoprene and tetracosyl acrylate monomers in a molar ratio of 5:6:1 are added to a reactor containing xylene solvent to carry out copolymerization reaction; before the reaction starts, 0.5wt% of free radical initiator dibenzoyl peroxide is added to the reaction system, the reaction temperature is controlled to be 80°C, and the reaction time is 6h; during the reaction, nitrogen is introduced to exclude oxygen and prevent the occurrence of oxidation reaction. After the reaction is completed, the unreacted monomers, solvents and initiator residues are removed through post-treatment steps such as solvent evaporation, filtration, washing and drying, thereby obtaining the target product grafted anhydride and oil-based copolymer.
[0055] S2: Dissolve 25 g of the grafted anhydride and oil-based copolymer obtained in step S1 in 250 mL of ethyl acetate, then add an acid solution consisting of acetic acid and water in a volume ratio of 2:1, adjust the pH value to 5.0, and carry out a hydrolysis reaction at room temperature. Maintain a stirring speed of 500 rpm for 4 hours. After the reaction is completed, filter, wash, and dry to obtain the desired additive.
[0056] S3: The additive obtained in step S2 is stirred and mixed evenly with microcrystalline wax, low-density polyethylene, metallocene polyethylene and auxiliary agent to obtain the high-flow low-ash binder. The mass ratio of the microcrystalline wax, low-density polyethylene, metallocene polyethylene, auxiliary agent and additive is 8:22:45:7:18. The auxiliary agent is the same as that in Example 1.
[0057] The test results show that the binder of this embodiment has a melt index of 22 g / 10 min measured by a melt index tester at a test temperature of 150° C. and a test pressure according to ASTM D1238. After being heated to constant weight in a high-temperature furnace at 600° C., the ash content of the binder is less than 0.5%.
[0058] In the degreasing test, n-hexane was first used as the solvent for solvent degreasing at room temperature for 60 minutes, then thermal degreasing was performed at a thermal degreasing temperature of 150°C for 60 minutes, and finally thermal degreasing was performed at a thermal degreasing temperature of 180°C for 120 minutes, with a degreasing efficiency of 93.7%. At the same time, 20 molded parts were visually and dimensionally inspected, and no appearance defects were found.
[0059] Example 6
[0060] The method for preparing a high-flow, low-ash binder for metal injection molding in this embodiment comprises the following steps:
[0061] S1: maleic anhydride, butadiene and tridecyl acrylate monomers in a molar ratio of 5:6:1 are added to a reactor containing xylene solvent to carry out copolymerization reaction; before the reaction starts, 0.5wt% of free radical initiator dibenzoyl peroxide is added to the reaction system, the reaction temperature is controlled to be 90°C, and the reaction time is 5h; during the reaction, nitrogen is introduced to exclude oxygen and prevent the occurrence of oxidation reaction. After the reaction is completed, the unreacted monomers, solvents and initiator residues are removed through post-treatment steps such as solvent evaporation, filtration, washing and drying, thereby obtaining the target product grafted anhydride and oil-based copolymer.
[0062] S2: Dissolve 25 g of the grafted anhydride and oil-based copolymer obtained in step S1 in 250 mL of ethyl acetate, then add an acid solution consisting of acetic acid and water in a volume ratio of 2:1, adjust the pH value to 4.8, and carry out a hydrolysis reaction at room temperature. Maintain a stirring speed of 500 rpm for 4 hours. After the reaction is completed, filter, wash, and dry to obtain the desired additive.
[0063] S3: The additive obtained in step S2 is stirred and mixed evenly with synthetic wax, polypropylene, metallocene polyethylene and auxiliary agent to obtain the high-flow low-ash binder. The mass ratio of the synthetic wax, polypropylene, metallocene polyethylene, auxiliary agent and additive is 12:28:42:3:15. The auxiliary agent is the same as that in Example 1.
[0064] The test results show that the adhesive of this embodiment has a melt index of 23 g / 10 min measured by a melt index tester at a test temperature of 150° C. and a test pressure according to ASTM D1238. After being heated to constant weight in a high-temperature furnace at 600° C., the ash content of the adhesive is less than 0.5%.
[0065] In the degreasing test, n-hexane was first used as the solvent for solvent degreasing at room temperature for 60 minutes, then thermal degreasing was performed at a thermal degreasing temperature of 150°C for 60 minutes, and finally thermal degreasing was performed at a thermal degreasing temperature of 180°C for 120 minutes, with a degreasing efficiency of 94.1%. At the same time, 20 molded parts were visually and dimensionally inspected, and no appearance defects were found.
[0066] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention claimed.
Claims
1. A high-flow, low-ash binder for metal injection molding, characterized in that: The binder comprises wax, a polymer matrix, an auxiliary agent and an additive shown in structural formula I; ; In the formula, R1 is an alkane group of 4 to 7 carbon atoms, R2 is H or methyl, R3 is an alkane group of 17 to 32 carbon atoms, and a / b is 1 to 5:1; The additive is first obtained by copolymerization of maleic anhydride, diene and long-chain acrylate, and then by hydrolysis under acidic conditions; the polymer matrix is composed of at least one of polypropylene, low-density polyethylene and medium-density polyethylene and metallocene polyethylene; the auxiliary agent is at least one of a surfactant, a lubricant and a stabilizer; the mass ratio of the wax, polymer matrix, auxiliary agent and additive is 7-12:60-90:3-8:15-20.
2. The high-flow, low-ash binder for metal injection molding according to claim 1, characterized in that: The diene is at least one of butadiene, isoprene, and 3,3-dimethyl-1,4-pentadiene.
3. The high-flow, low-ash binder for metal injection molding according to claim 1, wherein: The long-chain acrylate is at least one of heptadecyl acrylate, 2-methylheptadecyl acrylate, 2-methylheptadecyl methacrylate, octadecyl methacrylate, 2-methyloctadecyl acrylate, 2-methyloctadecyl methacrylate, 2-methylnonadecyl methacrylate, eicosyl acrylate, heneicosyl acrylate, heneicosyl methacrylate, tetracosyl acrylate, octacosyl methacrylate, octacosyl acrylate, triacontyl acrylate, triacontyl acrylate, and triacontyl acrylate.
4. The high-flow, low-ash binder for metal injection molding according to claim 1, wherein: The wax is at least one of paraffin wax, microcrystalline wax and synthetic wax.
5. A method for preparing a high-flow, low-ash binder for metal injection molding according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1: Copolymerizing maleic anhydride, diene and long-chain acrylate in a reactor containing a solvent to obtain a grafted anhydride and oil-based copolymer; S2: dissolving the copolymer obtained in step S1 in a suitable solvent, then adding an acidic substance to adjust the pH value to 4.8-5.2, and performing a hydrolysis reaction to obtain the desired additive; S3: The additive obtained in step S2 is stirred and mixed evenly with the wax, polymer matrix and auxiliary agent to obtain the high-flow low-ash binder.