MXene and silver co-coated copper conductive nano composite material and preparation method thereof
Through the reaction of MXene with silver salt and copper suspension, a conductive nanocomposite with silver coated copper was prepared, which solved the problems of uneven silver coating and environmental pollution in the prior art, achieved efficient conductivity and oxidation resistance, and reduced Production cost, suitable for industrial applications.
Patent Information
- Application Number
- CN202410750649.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
The prior art has problems such as uneven silver coating, unstable reduction reaction, environmental pollution, large consumption, and high cost when preparing silver-clad copper materials, making it difficult to achieve efficient conductivity and oxidation resistance.
By reacting MXene nanosheets with silver salt and copper suspension, a conductive nanocomposite with silver coated copper was prepared. The silver nanoparticles were fixed using MXene's active site and large specific surface area to inhibit their migration and by heating or Light source irradiation achieves efficient conductivity.
It significantly improves the conductivity and oxidation resistance of silver-clad copper powder, simplifies the preparation process, reduces the production cost of materials, and is suitable for industrial applications.
Smart Images

Figure CN118768568A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of nanocomposite materials, specifically a MXene two-dimensional material and silver co-coated copper conductive nanocomposite material and a preparation method thereof. Background Art
[0002] Silver and copper are widely used in the photovoltaic industry, electronics industry, sensors, and optical or biological devices due to their high conductivity. Common silver-coated copper preparation methods in industrial production include chemical plating, mechanical ball milling, melt atomization, etc. Among them, the direct replacement method can only obtain a dotted structure during the silver plating process, and the silver coating is uneven. The reduction method of silver plating will cause the silver plating solution to be unstable due to the fast reduction reaction rate, affecting the coating effect. In addition, the plating solution used in chemical plating has complex components, and the preparation process will produce waste gas and waste liquid, which is harmful to the environment. The mechanical ball milling method consumes a lot of silver, consumes a lot of energy, and has high costs. The melt atomization method has a complex preparation process and high equipment requirements, high production costs, and it is difficult to prepare micro-nano powders. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a MXene and silver-coated copper conductive nanocomposite material and a preparation method thereof, wherein ultrathin MXene nanosheets and silver-coated copper nanoparticles prepared after etching and peeling of MAX phase (such as Ti3AlC2) are formed into a conductive nanocomposite material, which inhibits silver migration under high temperature conditions, significantly improves the conductivity and antioxidant capacity of silver-coated copper powder, and solves the problem of easy migration of silver.
[0004] The present invention is achieved through the following technical solutions:
[0005] The invention relates to a method for preparing a MXene and silver-coated copper conductive nanocomposite material, comprising the steps of dispersing MXene in a dispersant, adding a silver salt or a silver salt solution to prepare a MXene / Ag suspension, further adding a nano copper suspension and a reducing agent, and washing a precipitate obtained through sufficient reaction to obtain a conductive nanocomposite material of MXene and silver-coated copper.
[0006] The MXene is prepared by etching and stripping the MAX phase, specifically: all the general formulas are M N+1 AX N Material, wherein: M is a pre-transition metal, A is an A group element, X is carbon or nitrogen, N=1,2,3..., preferably Ti3SiC2, Ti2GaC, Ti3GeC2 or Cr2AlC.
[0007] The dispersant is ethylene glycol, ethylenediamine, glycerol, isopropanol, n-propanol, acetone, N,N-dimethylformamide or a combination thereof.
[0008] The silver salt is silver nitrate, silver sulfate, silver acetate, silver perchlorate, silver periodate or silver perbromide.
[0009] The silver salt solution is a silver salt aqueous solution or a silver salt ethanol solution.
[0010] The copper powder is preferably pretreated to remove the surface oxide layer and oil stains, and is further preferably soaked and ultrasonically treated with acetone, NaOH, HCl, ammonia water or an amino mixed solution (such as ammonium sulfate / ammonia water mixture) and then centrifugally washed with deionized water and ethanol for three times respectively.
[0011] The nano copper suspension is: copper powder is dispersed in polyvinyl pyrrolidone, sodium citrate, sodium oleate, sodium ammonium polyacrylate, tetrabutylammonium bromide, polyvinyl alcohol or ethylenediaminetetraacetic acid.
[0012] The reducing agent is sodium borohydride, ascorbic acid, hydrazine hydrate, sodium hypophosphite, potassium borohydride, oxalic acid or ethylenediamine, and the molar ratio of the reducing agent to the silver salt is 1:10-1:20.
[0013] The sufficient reaction means: continuous magnetic stirring at room temperature, heating (20-80° C.) or light source irradiation energy supply conditions until a precipitate is obtained. Technical Effects
[0014] Compared with the prior art, the present invention realizes MXene and silver-coated copper through heating or light source irradiation function, significantly inhibits the migration and oxidation of silver nanoparticles, achieves efficient conductivity, simplifies the preparation process, reduces material production costs, and is suitable for industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is an electron microscope image of the product of Example 1;
[0016] Figure 2 This is an electron microscope image of the product of Example 2;
[0017] Figure 3 This is an electron microscope image of the product of Example 3;
[0018] Figure 4 This is an electron microscope image of the product of Example 4. DETAILED DESCRIPTION Example 1
[0019] This embodiment relates to a method for preparing a MXene and silver-coated copper conductive nanocomposite material, comprising:
[0020] Step 1) Preparation of MXene: Dilute concentrated hydrochloric acid to 6 mol / L with deionized water. Measure 20 mL of 6 mol / L HCl, add 0.8 g LiF, and stir magnetically for 30 min to make it evenly dispersed. Slowly add 1 g Ti3AlC2 to the mixture of HCl and LiF to avoid violent heat release. The mixture was then transferred to a polytetrafluoroethylene beaker and stirred continuously for 24 h at a stirring rate of 600 rpm. After stirring, the MXene was centrifuged and washed with deionized water to pH = 6, with a centrifugal speed of 3500 rpm and a centrifugal time of 15 min each time. The washed MXene was placed in a freeze dryer and dried for 12 h before being taken out to obtain a highly conductive, single-layer MXene.
[0021] Step 2) Preparation of MXene / Ag suspension: 0.2 g of MXene prepared in step 1) was added to 50 mL of ethylene glycol solution, and after being dispersed evenly by ultrasonication for 5 min, 0.4 g of AgNO3 was added and stirred for 30 min.
[0022] Step 3) Pretreatment of copper powder: Weigh 5g of nano copper powder (particle size 100-500nm) and add it to 100mL 0.1mol / LNaOH solution or 100mL acetone solution. After ultrasonic treatment for 1h, use deionized water and ethanol to centrifuge and wash 3 times respectively. The purpose of pretreatment is to remove impurities such as oxide layer and oil on the surface of copper powder, so as to reduce the resistivity of copper powder and better form a dense coating layer.
[0023] Step 4) Preparation of nano-copper suspension: Add the copper powder treated as above into 50 mL of ethylene glycol solution and stir for 1-2 h. Step 5) Preparation of MXene and silver-coated copper conductive nanocomposite: Mix the suspensions in step 2) and step 4), add 0.1g NaBH4, and stir magnetically for 0.5-1h at room temperature and under heating (20-80°C). Wash the precipitate after stirring by centrifugation 3 times with deionized water and ethanol respectively, and dry it in a vacuum drying oven to constant weight. The SEM image of the prepared MXene and silver-coated copper conductive nanocomposite is shown in Figure 2. Figure 1 As shown, the particle size is about 700-800nm. Example 2
[0024] This embodiment relates to a method for preparing a MXene and silver-coated copper conductive nanocomposite material, comprising:
[0025] Step 1) Preparation of MXene: Dilute concentrated hydrochloric acid to 8 mol / L with deionized water. Measure 15 mL of 8 mol / L HCl, add 1.0 g LiF, and stir magnetically for 20 min to disperse it evenly. Slowly add 1.5 g Ti3AlC2 to the mixture of HCl and LiF to avoid violent heat release. The mixture was then transferred to a polytetrafluoroethylene beaker and stirred continuously for 24 h at a stirring rate of 800 rpm. After stirring, the MXene was centrifuged and washed with deionized water to pH = 6, with a centrifugal speed of 3500 rpm and a centrifugal time of 15 min each time. The washed MXene was placed in a freeze dryer and dried for 12 h before being taken out to obtain a highly conductive, single-layer MXene.
[0026] Step 2) Preparation of MXene / Ag suspension: Take 0.2 g of MXene prepared in step 1) and add it to 50 mL of ethylene glycol solution. After ultrasonic dispersion for 5 min, add 0.4 g of Ag2SO4 and stir for 30 min.
[0027] Step 3) Pretreatment of copper powder: Weigh 5g of nano copper powder (particle size 100-500nm) and add it to 100mL 0.1mol / LNaOH solution or 100mL acetone solution. After ultrasonic treatment for 1h, use deionized water and ethanol to centrifuge and wash 3 times respectively. The purpose of pretreatment is to remove impurities such as oxide layer and oil on the surface of copper powder, so as to reduce the resistivity of copper powder and better form a dense coating layer.
[0028] Step 4) Preparation of nano-copper suspension: Add the copper powder treated as above into 50 mL of ethylene glycol solution and stir for 1-2 h.
[0029] Step 5) Preparation of MXene and silver-coated copper conductive nanocomposite: Mix the suspensions in step 2) and step 4), add 0.1 g NaBH4, and stir magnetically for 0.5-1 h under heating (20-80° C.). Wash the stirred precipitate by centrifugation three times with deionized water and ethanol respectively, and dry it in a vacuum drying oven to constant weight.
[0030] The SEM image of the dense MXene and silver-coated copper conductive nanocomposite prepared in this example is shown in Figure 2. Figure 2 shown. Example 3
[0031] This embodiment relates to a method for preparing a MXene and silver-coated copper conductive nanocomposite material, comprising:
[0032] Step 1) Preparation of MXene: Dilute concentrated hydrochloric acid to 6 mol / L with deionized water. Measure 20 mL of 6 mol / L HCl, add 0.8 g LiF, and stir magnetically for 30 min to make it evenly dispersed. Slowly add 1 g Ti3AlC2 to the mixture of HCl and LiF to avoid violent heat release. The mixture was then transferred to a polytetrafluoroethylene beaker and stirred continuously for 24 h at a stirring rate of 600 rpm. After stirring, the MXene was centrifuged and washed with deionized water to pH = 6, with a centrifugal speed of 3500 rpm and a centrifugal time of 15 min each time. The washed MXene was placed in a freeze dryer and dried for 12 h before being taken out to obtain a highly conductive, single-layer MXene.
[0033] Step 2) Preparation of MXene / Ag suspension: 0.2 g of MXene prepared in step 1) was added to 50 mL of ethylene glycol solution, and after being dispersed evenly by ultrasonication for 5 min, 0.4 g of AgNO3 was added and stirred for 30 min.
[0034] Step 3) Pretreatment of copper powder: Weigh 5g of nano copper powder (particle size 100-500nm) and add it to 100mL 0.1mol / LNaOH solution or 100mL acetone solution. After ultrasonic treatment for 1h, use deionized water and ethanol to centrifuge and wash 3 times respectively. The purpose of pretreatment is to remove impurities such as oxide layer and oil on the surface of copper powder, so as to reduce the resistivity of copper powder and better form a dense coating layer.
[0035] Step 4) Preparation of nano-copper suspension: Add the copper powder treated as above into 50 mL of sodium citrate solution and stir for 1-2 h.
[0036] Step 5) Preparation of MXene and silver-coated copper conductive nanocomposite: Mix the suspensions in step 2) and step 4), add 0.1g NaBH4, and stir magnetically for 0.5-1h under the condition of irradiation with a light source (sunlight, halogen tungsten lamp, xenon lamp, medical LED, etc.). Wash the precipitate after stirring by centrifugation three times with deionized water and ethanol respectively, and dry it in a vacuum drying oven to constant weight.
[0037] The mass ratio of silver to copper in the MXene and silver-coated copper conductive nanomaterials prepared in this example is as follows: Figure 3 shown. Example 4
[0038] This embodiment relates to a method for preparing a MXene and silver-coated copper conductive nanocomposite material, comprising:
[0039] Step 1) Preparation of MXene: Dilute concentrated hydrochloric acid to 6 mol / L with deionized water. Measure 20 mL of 6 mol / L HCl, add 0.8 g LiF, and stir magnetically for 30 min to make it evenly dispersed. Slowly add 1.5 g Ti3AlC2 to the mixture of HCl and LiF. Then transfer the above mixture to a polytetrafluoroethylene beaker and stir continuously for 24 hours at a stirring rate of 600 rpm. After stirring, use deionized water to centrifuge and wash the MXene to pH = 6. The centrifugal speed is 3500 rpm each time and the centrifugal time is 15 min. Put the washed MXene into a freeze dryer and dry it for 24 hours before taking it out to obtain a highly conductive, single-layer MXene.
[0040] Step 2) Preparation of MXene / Ag suspension: Take 0.2 g of MXene prepared in step 1) and add it to 50 mL of ethylene glycol solution. After ultrasonic dispersion for 5 min, add 0.4 g of Ag2SO4 and stir for 30 min.
[0041] Step 3) Pretreatment of copper powder: Weigh 5g of nano copper powder (particle size 100-500nm) and add it to 100mL 0.1mol / LNaOH solution or 100mL acetone solution. After ultrasonic treatment for 1h, use deionized water and ethanol to centrifuge and wash 3 times respectively. The purpose of pretreatment is to remove impurities such as oxide layer and oil on the surface of copper powder, so as to reduce the resistivity of copper powder and better form a dense coating layer.
[0042] Step 4) Preparation of nano copper suspension: Add the copper powder treated as above into 50 mL of 0.5 mol / L ethylenediaminetetraacetic acid solution and stir for 1-2 h.
[0043] Step 5) Preparation of MXene and silver-coated copper conductive nanocomposite: Mix the suspensions in step 2) and step 4), add 0.5 mL of hydrazine hydrate, and stir magnetically for 1 hour at room temperature. Wash the precipitate after stirring by centrifugation three times with deionized water and ethanol respectively, and dry it in a vacuum drying oven to constant weight.
[0044] The mass ratio of silver to copper in the MXene and silver-coated copper conductive nanomaterials prepared in this example is as follows: Figure 4 shown.
[0045] Compared with the prior art, the present invention utilizes the abundant active sites and large specific surface area of MXene nanosheets to interconnect MXene, Ag, and Cu, effectively fix silver nanoparticles, and inhibit their migration. At the same time, a fast electron transmission channel is established inside the composite material formed by the three, achieving efficient conduction. In addition, the introduction of MXene can greatly reduce the use of precious metal silver, reduce the material production cost, and is conducive to industrial application.
[0046] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. A method for preparing a MXene and silver-coated copper conductive nanocomposite material, characterized in that: The method comprises dispersing MXene in a dispersant and then adding a silver salt or a silver salt solution to prepare a MXene / Ag suspension, further adding a nano copper suspension and a reducing agent, and washing the precipitate obtained after sufficient reaction to obtain a conductive nanocomposite material of MXene and silver-coated copper.
2. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, characterized in that: The general formula of the MXene is M N+1 AX N , wherein: M is a pre-transition metal, A is an A-group element, X is carbon or nitrogen, N=1,2,3…, and is obtained by etching and stripping based on the MAX phase.
3. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1 or 2, characterized in that: The MXene is made of Ti3SiC2, Ti2GaC, Ti3GeC2 or Cr2AlC.
4. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, characterized in that: The dispersant is ethylene glycol, ethylenediamine, glycerol, isopropanol, n-propanol, acetone, N,N-dimethylformamide or a combination thereof.
5. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, characterized in that: The silver salt is silver nitrate, silver sulfate, silver acetate, silver perchlorate, silver periodate or silver perbromide; The silver salt solution is a silver salt aqueous solution or a silver salt ethanol solution.
6. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, characterized in that: The copper powder is pre-treated to remove the surface oxide layer and oil stains.
7. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, characterized in that: The nano copper suspension is: copper powder is dispersed in polyvinyl pyrrolidone, sodium citrate, sodium oleate, sodium ammonium polyacrylate, tetrabutylammonium bromide, polyvinyl alcohol or ethylenediaminetetraacetic acid.
8. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, wherein: The reducing agent is sodium borohydride, ascorbic acid, hydrazine hydrate, sodium hypophosphite, potassium borohydride, oxalic acid or ethylenediamine, and the molar ratio of the reducing agent to the silver salt is 1:10-1:
20.
9. The method for preparing the MXene and silver-coated copper conductive nanocomposite material according to claim 1, wherein: The sufficient reaction means: continuous magnetic stirring at room temperature, heating or light source irradiation energy supply conditions until a precipitate is obtained.