Preparation method of glass-plastic composite laser radar window
By combining aluminosilicate glass with a black polycarbonate window and depositing an anti-reflective anti-reflection coating, the problem of insufficient scratch resistance and impact resistance of the lidar window is solved, achieving high hardness, low cost and high transmittance. High-efficiency lidar window, suitable for vehicle use environment.
Patent Information
- Application Number
- CN202410880020.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-15
AI Technical Summary
Existing LiDAR windows have deficiencies in scratch resistance, temperature resistance, and corrosion resistance. Especially in complex and changeable vehicle use environments, they are difficult to meet high requirements, are high in cost, and are fragile.
Using the preparation method of glass-plastic composite lidar window, the aluminosilicate glass window is combined with a black polycarbonate window, and an anti-reflection and anti-reflection film is deposited on the surface, which is fixed by ultrasonic cleaning, vacuum electron beam evaporation coating and optical glue. , forming a window structure with high hardness and impact resistance.
It improves the scratch and impact resistance of the lidar window, while reducing the cost, achieving high transmittance and black appearance, and is suitable for mass production.
Smart Images

Figure CN118769639A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of laser radar windows, and in particular to a method for preparing a glass-plastic composite laser radar window. Background Art
[0002] As an important component of laser radar, the laser radar window not only acts as an optical part to send and receive laser light, but also acts as an appearance part to protect the laser radar. Existing laser radar windows generally use special black glass or black polycarbonate materials that do not transmit visible light (380-700nm) but can transmit infrared rays of a specific band (700-1600nm). The glass material is divided into absorptive black glass that is doped with specific elements to filter out visible light and transparent glass that absorbs visible light through coating (hereinafter collectively referred to as black glass). The advantages of black glass laser radar windows are good scratch resistance, temperature resistance, and corrosion resistance, but the disadvantages are high cost, fragility, and difficulty in shaping. The advantages of polycarbonate laser radar windows are low cost, impact resistance, and easy shaping, but the disadvantages are poor scratch resistance, temperature resistance, and corrosion resistance. With the rapid expansion of laser radar applications, especially the gradual popularization of vehicle-mounted laser radars, the complex and changeable use environment has also put forward higher requirements on the performance of laser radar windows in all aspects. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing a glass-plastic composite laser radar window, which combines an aluminosilicate glass window with a black polycarbonate window to form a laser radar window, and can improve the impact resistance of the laser radar window while maintaining high hardness.
[0004] The present invention is implemented by the following technical scheme: a method for preparing a glass-plastic composite laser radar window, comprising an aluminosilicate glass window and a black polycarbonate window, wherein one side of the aluminosilicate glass window is fixed to one side of the black polycarbonate window; a first AR anti-reflection film is provided on the other side of the aluminosilicate glass window, and a second AR anti-reflection film is provided on the other side of the black polycarbonate window;
[0005] The method comprises the following steps:
[0006] Step 1, cleaning the aluminosilicate glass window using an ultrasonic cleaning machine;
[0007] Step 2, placing the aluminosilicate glass window into a vacuum electron beam evaporation coating machine, and depositing a first AR antireflection film on the surface of the aluminosilicate glass window;
[0008] Step 3, cleaning the black polycarbonate window using an ultrasonic cleaner, and then baking it;
[0009] Step 4, placing the black polycarbonate window into a vacuum electron beam evaporation coating machine, and depositing a second AR antireflection film on the surface of the black polycarbonate window;
[0010] Step 5: Clean the aluminosilicate glass window and the black polycarbonate window using an ultrasonic cleaner, and then glue and fix the aluminosilicate glass window and the black polycarbonate window using optical glue.
[0011] Preferably, in step 3, the baking temperature is 70±5° C. and the baking time is 1 hour.
[0012] Preferably, during the deposition of the first AR anti-reflection film and the second AR anti-reflection film, an ion source is used to generate ions to bombard the growing film layer.
[0013] Preferably, step 5 is further specified as follows: clean the aluminosilicate glass window and the black polycarbonate window using an ultrasonic cleaner, pour 3ml-5ml of optical glue on the bonding surface of the aluminosilicate glass window, fit the bonding surface of the black polycarbonate window thereto, press to make the optical glue evenly cover the bonding surface and wipe off excess optical glue overflowing around, align the positions of the two windows and irradiate them with ultraviolet light, and after irradiation, place them in a UV box for irradiation.
[0014] Preferably, the ultraviolet lamp is used for irradiation for 30-60 seconds, and after the irradiation is completed, it is placed in a ultraviolet box with an illumination of 0.5mW / cm2 to 1.5mW / cm2 and irradiated for 2 hours to 4 hours.
[0015] Preferably, the vacuum degree when depositing the film layer in step 2 and step 4 is 3×10-3Pa; the environmental heating temperature of the coating vacuum chamber of the coating machine in step 2 is 100°C, and the environmental heating temperature of the coating vacuum chamber of the coating machine in step 4 is 150°C.
[0016] Preferably, the first AR antireflection film comprises:
[0017] a first titanium dioxide film layer, a first silicon dioxide film layer,
[0018] a second titanium dioxide film layer, a second silicon dioxide film layer,
[0019] a third titanium dioxide film layer, a third silicon dioxide film layer,
[0020] a fourth titanium dioxide film layer and a fourth silicon dioxide film layer;
[0021] The second AR antireflection film includes an aluminum oxide film layer, a fifth titanium dioxide film layer, and a fifth silicon dioxide film layer which are sequentially fixed on a black polycarbonate window.
[0022] Preferably, in step 2 and step 4, a crystal oscillator film thickness controller is used to control the thickness of each film layer.
[0023] The thickness of the first titanium dioxide film layer is 10.43±0.1nm, and the deposition rate is 0.4nm / sec;
[0024] The thickness of the first silicon dioxide film layer is 47.14±0.1nm, and the deposition rate is 0.8nm / sec;
[0025] The second titanium dioxide film has a thickness of 26.24±0.1nm and a deposition rate of 0.4nm / sec;
[0026] The thickness of the second silicon dioxide film layer is 21.49±0.1nm, and the deposition rate is 0.8nm / sec;
[0027] The thickness of the third titanium dioxide film layer is 121.89±0.1nm, and the deposition rate is 0.4nm / sec;
[0028] The thickness of the third silicon dioxide film layer is 26.38±0.1nm, and the deposition rate is 0.8nm / sec;
[0029] The thickness of the fourth titanium dioxide film layer is 17.15±0.1 nm, and the deposition rate is 0.4 nm / sec;
[0030] The fourth silicon dioxide film layer has a thickness of 126.46±0.1 nm and a deposition rate of 0.8 nm / sec;
[0031] The thickness of the aluminum oxide film is 30.00±0.1nm, and the deposition rate is 0.4nm / s;
[0032] The fifth titanium dioxide film layer has a thickness of 30.67±0.1 nm and a deposition rate of 0.4 nm / s;
[0033] The thickness of the fifth silicon dioxide film layer is 199.78±0.1 nm, and the deposition rate is 0.8 nm / sec.
[0034] Beneficial effects of the present invention:
[0035] (1) The hardness of the black polycarbonate window is 3B, and the hardness of the aluminosilicate glass window is 6.5H. The laser radar window formed by the combination of the two uses the aluminosilicate glass window surface as the outer surface of the laser radar, which can improve the scratch resistance of the laser radar window.
[0036] (2) One side of the aluminosilicate glass window is fixed to one side of the black polycarbonate window. The toughness of the polycarbonate material is better than that of the glass material. Combining the aluminosilicate glass window and the black polycarbonate window to form a lidar window can improve the impact resistance of the lidar window.
[0037] (3) Using aluminosilicate glass bonded to black polycarbonate windows can achieve a black appearance of the window and reduce costs. The market uses black colored glass as a lidar window to achieve a black appearance solution. Because colored glass is expensive, it cannot be mass-produced. The price of polycarbonate and aluminosilicate glass materials is relatively low, which is conducive to the mass production of such products.
[0038] The present invention combines an aluminosilicate glass window with a black polycarbonate window to form a laser radar window, which can improve the impact resistance of the laser radar window under the premise of high hardness. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic diagram of the structure of the glass-plastic composite lidar window.
[0040] Figure 2 Schematic diagram of the structure of the first AR antireflection film.
[0041] Figure 3 Schematic diagram of the structure of the second AR antireflection film.
[0042] Figure 4 It is the transmittance diagram of the lidar window in the 880-920 band. DETAILED DESCRIPTION
[0043] The present invention will be further described below in conjunction with the accompanying drawings.
[0044] like Figures 1 to 3 The present invention provides an embodiment: a method for preparing a glass-plastic composite laser radar window, comprising an aluminosilicate glass window 1 and a black polycarbonate window 3, wherein the hardness of the black polycarbonate window 3 is 3B, and the hardness of the aluminosilicate glass window 1 is 6.5H. The laser radar window formed by the combination of the two uses the aluminosilicate glass window 1 as the outer surface of the laser radar, which can improve the scratch resistance of the laser radar window. One side of the aluminosilicate glass window 1 is fixed to one side of the black polycarbonate window 3; the toughness of the polycarbonate material is better than that of the glass material, and the combination of the aluminosilicate glass window 1 and the black polycarbonate window 3 can improve the impact resistance of the laser radar window. The other side of the aluminosilicate glass window 1 has a first AR anti-reflection film 2, and the other side of the black polycarbonate window 3 has a second AR anti-reflection film 4; the light transmittance of the window can be increased. The hardness of the black polycarbonate window 3 after being coated with the first AR antireflection film 2 is HB, and the hardness of the aluminosilicate glass window 1 after being coated is 7H, so that the laser radar window has the advantages of high hardness and scratch resistance.
[0045] The method comprises the following steps:
[0046] Step 1, cleaning the aluminosilicate glass window 1 using an ultrasonic cleaning machine;
[0047] Step 2, placing the aluminosilicate glass window 1 into a vacuum electron beam evaporation coating machine, and depositing a first AR antireflection film 2 on the surface of the aluminosilicate glass window 1;
[0048] Step 3, cleaning the black polycarbonate window 3 using an ultrasonic cleaning machine, and then performing a baking treatment;
[0049] Step 4, placing the black polycarbonate window 3 into a vacuum electron beam evaporation coating machine, and depositing a second AR antireflection film 4 on the surface of the black polycarbonate window 3;
[0050] Step 5: Clean the aluminosilicate glass window 1 and the black polycarbonate window 3 with an ultrasonic cleaner, and then glue the aluminosilicate glass window 1 and the black polycarbonate window 3 with optical glue. After gluing, the reflectivity of the gluing surface of the aluminosilicate glass window 1 and the black polycarbonate window 3 can be reduced, greatly improving the transmittance of the laser radar window.
[0051] In step 3, the baking temperature is 70±5° C. and the baking time is 1 hour, so that the water vapor can be removed.
[0052] During the deposition of the first AR antireflection film 2 and the second AR antireflection film 4, an ion source is used to generate ions to bombard the growing film layer. Ion beam assisted deposition improves the film layer stacking density and improves the film layer quality.
[0053] The step 5 is further specified as follows: the aluminosilicate glass window 1 and the black polycarbonate window 3 are cleaned using an ultrasonic cleaner, 3ml-5ml of Norland 61 optical glue is poured onto the bonding surface of the aluminosilicate glass window 1, the bonding surface of the black polycarbonate window 3 is fitted thereto, pressing to evenly cover the bonding surface with the optical glue and wiping off excess optical glue overflowing from all sides, aligning the two windows and irradiating them with an ultraviolet lamp, and after the irradiation is completed, placing them in an ultraviolet box for irradiation.
[0054] Use UV lamp to irradiate for 30-60 seconds. After irradiation, place it in a UV box with an illumination of 0.5mW / cm2 to 1.5mW / cm2 for 2 hours to 4 hours to cure the optical glue.
[0055] The vacuum degree when depositing the film layer in step 2 and step 4 is 3×10-3Pa; the environmental heating temperature of the coating vacuum chamber of the coating machine in step 2 is 100°C, and the environmental heating temperature of the coating vacuum chamber of the coating machine in step 4 is 150°C, which can improve the density and adhesion of the film layer.
[0056] The first AR antireflection film 2 includes a plurality of layers fixed in sequence on the aluminosilicate glass window 1.
[0057] a first titanium dioxide film layer 21, a first silicon dioxide film layer 22,
[0058] The second titanium dioxide film layer 23, the second silicon dioxide film layer 24,
[0059] The third titanium dioxide film layer 25, the third silicon dioxide film layer 26,
[0060] a fourth titanium dioxide film layer 27 and a fourth silicon dioxide film layer 28;
[0061] Titanium dioxide is used as a high refractive index film layer, silicon dioxide is used as a low refractive index film layer, and the combination of high and low refractive index film layers achieves an anti-reflection effect through thin film interference.
[0062] The second AR antireflection film 4 comprises an aluminum oxide film layer 41, a fifth titanium dioxide film layer 42, and a fifth silicon dioxide film layer 43 which are sequentially fixed on the black polycarbonate window 3. Aluminum oxide is used to improve the bonding strength between the black polycarbonate and the film layer.
[0063] In step 2 and step 4, a crystal oscillator film thickness controller is used to control the thickness of each film layer, so that the film layer can be dense and uniform in thickness.
[0064] The thickness of the first titanium dioxide film layer 21 is 10.43.00±0.1 nm, and the deposition rate is 0.4 nm / sec;
[0065] The first silicon dioxide film layer 22 has a thickness of 47.14±0.1 nm and a deposition rate of 0.8 nm / sec;
[0066] The thickness of the second titanium dioxide film layer 23 is 26.24±0.1nm and the deposition rate is 0.4nm / sec;
[0067] The second silicon dioxide film layer 24 has a thickness of 21.49±0.1 nm and a deposition rate of 0.8 nm / sec;
[0068] The thickness of the third titanium dioxide film layer 25 is 121.89.67±0.1 nm, and the deposition rate is 0.4 nm / sec;
[0069] The thickness of the third silicon dioxide film layer 26 is 26.38±0.1 nm and the deposition rate is 0.8 nm / sec;
[0070] The fourth titanium dioxide film layer 27 has a thickness of 17.15±0.1 nm and a deposition rate of 0.4 nm / sec;
[0071] The fourth silicon dioxide film layer 28 has a thickness of 126.46±0.1 nm and a deposition rate of 0.8 nm / sec;
[0072] Through the above-mentioned nanometer-level thickness optical film design, the anti-reflection effect can be better achieved.
[0073] The thickness of the aluminum oxide film 41 is 30.00±0.1 nm, and the deposition rate is 0.4 nm / s;
[0074] The fifth titanium dioxide film layer 42 has a thickness of 30.67±0.1 nm and a deposition rate of 0.4 nm / sec;
[0075] The fifth silicon dioxide film layer 43 has a thickness of 199.78±0.1 nm and a deposition rate of 0.8 nm / sec.
[0076] Through the above-mentioned design of the optical film with nanometer-level thickness, the bonding strength between the black polycarbonate and the film layer can be better improved.
[0077] The hardness of polycarbonate after coating is HB, and the hardness of aluminosilicate glass after coating is 7H.
[0078] Aluminosilicate glass can pass the scratch resistance test after coating. (Use 0000# steel wool, apply a load of 200g, and rub back and forth on the sample surface 10 times.)
[0079] By gluing the aluminosilicate glass window 1 and the black polycarbonate window 3, the light energy loss can be greatly reduced and the laser transmittance can be increased. Figure 4 The transmittance of the glass-plastic composite laser radar window can reach 99.5% in the laser radar working band of 880-920nm, greatly improving the optical performance of the laser radar.
[0080] The hardness values in the present invention are all obtained by pencil hardness test method with a load of 750g.
[0081] The above description is only a preferred embodiment of the present invention and should not be construed as limiting the present application. All equivalent changes and modifications made within the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing a glass-plastic composite laser radar window, characterized in that: It comprises an aluminosilicate glass window and a black polycarbonate window, wherein one side of the aluminosilicate glass window is fixed to one side of the black polycarbonate window; the other side of the aluminosilicate glass window has a first AR anti-reflection film, and the other side of the black polycarbonate window has a second AR anti-reflection film; The method comprises the following steps: Step 1, cleaning the aluminosilicate glass window using an ultrasonic cleaning machine; Step 2, placing the aluminosilicate glass window into a vacuum electron beam evaporation coating machine, and depositing a first AR antireflection film on the surface of the aluminosilicate glass window; Step 3, cleaning the black polycarbonate window using an ultrasonic cleaner, and then baking it; Step 4, placing the black polycarbonate window into a vacuum electron beam evaporation coating machine, and depositing a second AR antireflection film on the surface of the black polycarbonate window; Step 5: Clean the aluminosilicate glass window and the black polycarbonate window using an ultrasonic cleaner, and then glue and fix the aluminosilicate glass window and the black polycarbonate window using optical glue.
2. The method for preparing a glass-plastic composite laser radar window according to claim 1, characterized in that: In step 3, the baking temperature is 70±5° C. and the baking time is 1 hour.
3. The method for preparing a glass-plastic composite laser radar window according to claim 1, characterized in that: During the deposition of the first AR antireflection film and the second AR antireflection film, an ion source is used to generate ions to bombard the growing film layer.
4. The method for preparing a glass-plastic composite laser radar window according to claim 1, characterized in that: The step 5 is further specified as follows: the aluminosilicate glass window and the black polycarbonate window are cleaned with an ultrasonic cleaner, 3ml-5ml of optical glue is poured on the bonding surface of the aluminosilicate glass window, the bonding surface of the black polycarbonate window is fitted thereto, pressing to make the optical glue evenly cover the bonding surface and wiping off excess optical glue overflowing around, aligning the two windows and irradiating them with a UV lamp, and after irradiation is completed, placing them in a UV box for irradiation.
5. The method for preparing a glass-plastic composite laser radar window according to claim 4, characterized in that: Use UV lamp to irradiate for 30-60 seconds. After irradiation, place it in a UV box with an illumination of 0.5mW / cm2 to 1.5mW / cm2 for 2 hours to 4 hours.
6. The method for preparing a glass-plastic composite laser radar window according to claim 1, characterized in that: The vacuum degree when depositing the film layer in step 2 and step 4 is 3×10-3Pa; the environmental heating temperature of the coating vacuum chamber of the coating machine in step 2 is 100°C, and the environmental heating temperature of the coating vacuum chamber of the coating machine in step 4 is 150°C.
7. The method for preparing a glass-plastic composite laser radar window according to claim 1, characterized in that: The first AR antireflection film includes a plurality of layers fixed in sequence on the aluminosilicate glass window. a first titanium dioxide film layer, a first silicon dioxide film layer, a second titanium dioxide film layer, a second silicon dioxide film layer, a third titanium dioxide film layer, a third silicon dioxide film layer, a fourth titanium dioxide film layer and a fourth silicon dioxide film layer; The second AR antireflection film includes an aluminum oxide film layer, a fifth titanium dioxide film layer, and a fifth silicon dioxide film layer which are sequentially fixed on a black polycarbonate window.
8. The method for preparing a glass-plastic composite laser radar window according to claim 7, characterized in that: In step 2 and step 4, a crystal oscillator film thickness controller is used to control the thickness of each film layer. The thickness of the first titanium dioxide film layer is 10.43±0.1nm, and the deposition rate is 0.4nm / sec; The thickness of the first silicon dioxide film layer is 47.14±0.1nm, and the deposition rate is 0.8nm / sec; The second titanium dioxide film has a thickness of 26.24±0.1nm and a deposition rate of 0.4nm / sec; The thickness of the second silicon dioxide film layer is 21.49±0.1nm, and the deposition rate is 0.8nm / sec; The thickness of the third titanium dioxide film layer is 121.89±0.1nm, and the deposition rate is 0.4nm / sec; The thickness of the third silicon dioxide film layer is 26.38±0.1nm, and the deposition rate is 0.8nm / sec; The thickness of the fourth titanium dioxide film layer is 17.15±0.1 nm, and the deposition rate is 0.4 nm / sec; The fourth silicon dioxide film layer has a thickness of 126.46±0.1 nm and a deposition rate of 0.8 nm / sec; The thickness of the aluminum oxide film is 30.00±0.1nm, and the deposition rate is 0.4nm / s; The fifth titanium dioxide film layer has a thickness of 30.67±0.1 nm and a deposition rate of 0.4 nm / s; The thickness of the fifth silicon dioxide film layer is 199.78±0.1 nm, and the deposition rate is 0.8 nm / sec.
Citation Information
Patent Citations
Photovoltaic glass antireflection film
CN108424007A
Laminated glazing, associated apparatus with near-infrared vision system
CN115226396A
Laminated glass and vehicle
CN117183496A
Large-incidence-angle anti-reflection film for laser radar window and preparation method of large-incidence-angle anti-reflection film
CN117590496A
High-precision laser radar window structure
CN218470965U