High-buoyancy treatment method for offshore floating type bamboo-based platform

Through the polycondensation reaction of polyether, isocyanate and other materials and vacuum casting technology, the surface of bamboo-based buoyant materials is treated, which solves the problems of aging and safety hazards of polyethylene materials in floating water photovoltaic power generation systems, and improves the corrosion resistance and resistance of the materials. Impact performance, reduces water absorption and maintains low-impact buoyancy performance.

CN118770495APending Publication Date: 2024-10-15中林绿碳(北京)科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997953.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing floating water photovoltaic power generation system, the modified high-density polyethylene material is easy to age and decompose in the marine environment, causing seawater pollution and safety hazards, and its ultraviolet resistance and impact resistance are insufficient.

Method used

Polyether, isocyanate, initiator, plasticizer, curing agent and hydrophobic filler are used to make waterproof coating through polycondensation reaction and vacuum casting technology. The surface of bamboo-based buoyant material is targetedly treated to enhance corrosion resistance and impact resistance. Reduce water absorption.

Benefits of technology

It improves the corrosion resistance and impact resistance of bamboo-based buoyancy materials, reduces water absorption, reduces the risk of damage, and maintains low-impact overall buoyancy performance. The waterproof coating is lightweight and easy to repair locally.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118770495A_ABST
    Figure CN118770495A_ABST
Patent Text Reader

Abstract

The invention discloses a high-buoyancy treatment method for an offshore floating type bamboo-based platform, and relates to the technical field of surface treatment. The method comprises the following steps that S1, a to-be-treated bamboo-based buoyancy material is subjected to partial covering treatment, so that only the to-be-treated surface is exposed to the outside; and S2, the bamboo-based buoyancy material to be treated is fixed in a container and placed in a vacuum pouring tank, and vacuumizing treatment is conducted. The polyether, the isocyanate, the plasticizer, the curing agent, the diluent and the hydrophobic filler are adopted as raw materials, the to-be-treated surface of the bamboo-based buoyancy material is specifically poured with the waterproof coating prepared from the raw materials, the corrosion resistance of the treated surface of the bamboo-based buoyancy material is enhanced, the water absorption rate is reduced, meanwhile, the bamboo-based buoyancy material has a certain buffering function, and the service life of the bamboo-based buoyancy material is prolonged. The impact resistance is improved, the damage risk is reduced, and the waterproof coating is light in weight and has small influence on the overall buoyancy of the bamboo-based buoyancy material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface treatment, in particular to a high buoyancy treatment method for an offshore floating bamboo-based platform. Background Art

[0002] In recent years, with the increasing shortage of inland land resources, photovoltaic projects covering a large area have begun to gradually expand their application scenarios to the vast ocean. Floating water photovoltaic power generation systems have become a new development trend in the field of water photovoltaics. At present, the floating structure of the floating water photovoltaic power generation system mainly uses modified high-density polyethylene as the floating body material, and the steel welded structure as the floating body frame. Compared with traditional photovoltaic power stations, floating photovoltaic power stations install photovoltaic power generation components on the floating body on the water surface, which has the effects of not occupying land resources, reducing water evaporation, and the floating body blocking sunlight to inhibit algae growth. At the same time, the cooling effect of the water body on photovoltaic components and cables can significantly improve the power generation efficiency.

[0003] Although high-density polyethylene raw materials are easy to obtain and simple to process, there are also some outstanding problems, namely: the UV resistance and toughness of polyethylene need to be improved, and the service life needs to be verified; as the years of use increase, high-density polyethylene is prone to aging and decomposition into microplastics, which poses a risk of causing seawater pollution and the safety of marine biological food.

[0004] Bamboo-based marine engineering materials are a new type of bio-based material made with bamboo as the base material and a variety of new processes. Compared with traditional steel structures, they have the advantages of lighter weight, lower cost, more resistance to seawater corrosion, longer service life, and green environmental protection. They will help promote the development of offshore photovoltaic platforms.

[0005] Spraying waterproof coating is a commonly used protective method in marine engineering. Epoxy coatings, polyurea waterproof coatings, etc. are widely used. Since bamboo-based platforms need to be in the marine atmospheric corrosion environment all the time and are exposed to direct sunlight, the aging speed of the waterproof layer is very fast in such a complex environment; in addition, bamboo-based platforms are likely to be hit by external forces at sea, which may also cause damage to the waterproof layer. Once the waterproof layer fails, the buoyancy of the buoyancy material will decrease due to water absorption, posing a safety hazard. Therefore, we proposed a high buoyancy treatment method for offshore floating bamboo-based platforms to solve the above problems. Summary of the invention

[0006] The purpose of the present invention is to provide a high buoyancy treatment method for an offshore floating bamboo-based platform to solve the problems in the current market raised by the above background technology.

[0007] To achieve the above object, the present invention provides the following technical solution: a method for treating high buoyancy of an offshore floating bamboo-based platform, comprising the following steps:

[0008] S1: Partially cover the bamboo-based buoyancy material to be treated so that only the surface to be treated is exposed to the outside;

[0009] S2: Fix the bamboo-based buoyancy material to be treated in a container, place it in a vacuum pouring tank, and perform vacuum treatment;

[0010] S3: 300-400 parts of polyether, 100-150 parts of isocyanate and 15-25 parts of initiator are subjected to polycondensation reaction to obtain component A, and 10-20 parts of plasticizer, 20-30 parts of curing agent, 20-30 parts of diluent and 350-450 parts of hydrophobic filler are mixed to obtain component B, and component A and component B are poured into a mixing tank of a vacuum casting tank and stirred evenly;

[0011] S4: Open the valve of the mixing tank discharge port to allow the mixed liquid in the mixing tank to flow into the container containing the bamboo-based buoyancy material, and then increase the pressure in the vacuum pouring tank through the air compressor, maintain the pressure for 6 to 10 minutes and then release the pressure;

[0012] S5: Take out the bamboo-based buoyancy material, remove the covered part, put it into the oven for heat preservation and then cool it naturally.

[0013] Preferably, the masking treatment adopts paint masking or physical film masking.

[0014] Preferably, the pressure of the vacuum treatment is 800-900Pa.

[0015] Preferably, the plasticizer is polyethylene terephthalate.

[0016] Preferably, the curing agent is benzylenediamine trimer.

[0017] Preferably, the diluent is butyl glycidyl ether.

[0018] Preferably, the initiator is dimethyl azobisisobutyrate.

[0019] Preferably, the hydrophobic filler is a mixture of one or more of alkanes, alkyl alcohols and alkyl acids.

[0020] Preferably, in said S4, the pressure in the vacuum pouring tank is increased to 8000-10000 Pa.

[0021] Preferably, in S5, the insulation temperature is 40-50° C., and the insulation time is 12-20 hours.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention uses polyether, isocyanate, initiator, plasticizer, curing agent, diluent and hydrophobic filler as raw materials, and casts the waterproof coating made of the above raw materials on the surface to be treated of the bamboo-based buoyancy material in a targeted manner. The corrosion resistance of the surface of the treated bamboo-based buoyancy material is enhanced, the water absorption rate is reduced, and at the same time, it has a certain buffering function, the impact resistance is improved, and the risk of damage is reduced. In addition, the waterproof coating is light in weight and has little effect on the overall buoyancy of the bamboo-based buoyancy material.

[0024] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present invention will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a schematic flow chart of a high buoyancy treatment method for an offshore floating bamboo-based platform. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] See also Figure 1 A method for treating high buoyancy of an offshore floating bamboo-based platform comprises the following steps:

[0028] S1: Partially cover the bamboo-based buoyancy material to be treated so that only the surface to be treated is exposed to the outside; the covering treatment adopts paint covering or physical film covering; the paint covering can be covered by brushing an organic resin coating; the physical film covering can be coated with an adhesive and the covering part of the bamboo-based buoyancy material is bonded together after heating and pressurizing.

[0029] S2: Fix the bamboo-based buoyancy material to be treated in a container, and place it in a vacuum casting tank for vacuum treatment, and the pressure of the vacuum treatment is 800-900 Pa;

[0030] S3: 300-400 parts of polyether, 100-150 parts of isocyanate and 15-25 parts of initiator dimethyl azobisisobutyrate are subjected to polycondensation reaction to obtain component A, and then 10-20 parts of plasticizer, 20-30 parts of curing agent, 20-30 parts of diluent and 350-450 parts of hydrophobic filler are mixed to obtain component B, and component A and component B are poured into a mixing tank of a vacuum casting tank and stirred evenly;

[0031] The plasticizer is polyethylene terephthalate, the curing agent is xylylenediamine trimer, the diluent is butyl glycidyl ether, and the hydrophobic filler is a mixture of one or more of alkanes, alkyl alcohols, and alkyl acids.

[0032] S4: Open the valve of the mixing tank discharge port to allow the mixed liquid in the mixing tank to flow into the container containing the bamboo-based buoyancy material, and then use the air compressor to increase the pressure in the vacuum pouring tank to 8000-10000Pa, maintain the pressure for 6-10 minutes and then release the pressure;

[0033] S5: Take out the bamboo-based buoyancy material, remove the masked part, put it into an oven at 40-50°C for 12-20 hours, and then cool it naturally. If it is covered with paint, rinse it with an alkaline detergent, such as a 3-5wt% sodium hydroxide solution; if it is covered with a physical film, heat it and then tear it off.

[0034] Example 1

[0035] A method for treating high buoyancy of an offshore floating bamboo-based platform comprises the following steps:

[0036] S1: Partially cover the bamboo-based buoyancy material to be treated so that only the surface to be treated is exposed to the outside; the covering treatment is performed by coating; the coating covering can be performed by brushing an organic resin coating;

[0037] S2: Fix the bamboo-based buoyancy material to be treated in a container and place it in a vacuum casting tank for vacuum treatment. The pressure of the vacuum treatment is 800Pa;

[0038] S3: 300 parts of polyether, 150 parts of isocyanate and 20 parts of initiator dimethyl azobisisobutyrate are subjected to polycondensation reaction to obtain component A, and 10 parts of plasticizer, 25 parts of curing agent, 30 parts of diluent and 450 parts of hydrophobic filler are mixed to obtain component B, and component A and component B are poured into a mixing tank of a vacuum casting tank and stirred evenly;

[0039] The plasticizer is polyethylene terephthalate, the curing agent is benzylenediamine trimer, the diluent is butyl glycidyl ether, and the hydrophobic filler is a mixture of alkane, alkyl alcohol, and alkyl acid in a ratio of 1:1:1.

[0040] S4: Open the valve of the mixing tank discharge port to allow the mixed liquid in the mixing tank to flow into the container containing the bamboo-based buoyancy material, and then use the air compressor to increase the pressure in the vacuum pouring tank to 8000Pa, maintain the pressure for 6 minutes and then release the pressure;

[0041] S5: Take out the bamboo-based buoyancy material, wash it with an alkaline detergent, such as a 4 wt % sodium hydroxide solution, wash off the organic resin coating, put it into an oven at 45° C. for 18 hours, and then cool it naturally.

[0042] Example 2

[0043] A method for treating high buoyancy of an offshore floating bamboo-based platform comprises the following steps:

[0044] S1: Partially cover the bamboo-based buoyancy material to be treated so that only the surface to be treated is exposed to the outside; the covering treatment is performed by coating; the coating covering can be performed by brushing an organic resin coating;

[0045] S2: Fix the bamboo-based buoyancy material to be treated in a container and place it in a vacuum casting tank for vacuum treatment. The pressure of the vacuum treatment is 850Pa;

[0046] S3: 350 parts of polyether, 125 parts of isocyanate and 22 parts of initiator dimethyl azobisisobutyrate are subjected to polycondensation reaction to obtain component A, and 20 parts of plasticizer, 25 parts of curing agent, 20 parts of diluent and 400 parts of hydrophobic filler are mixed to obtain component B, and component A and component B are poured into a mixing tank of a vacuum casting tank and stirred evenly;

[0047] The plasticizer is polyethylene terephthalate, the curing agent is benzylenediamine trimer, the diluent is butyl glycidyl ether, and the hydrophobic filler is a mixture of alkane, alkyl alcohol, and alkyl acid in a ratio of 1:1:1.

[0048] S4: Open the discharge port valve of the mixing tank to allow the mixed liquid in the mixing tank to flow into the container containing the bamboo-based buoyancy material, and then use the air compressor to increase the pressure in the vacuum pouring tank to 9000Pa, maintain the pressure for 8 minutes and then release the pressure;

[0049] S5: Take out the bamboo-based buoyancy material, and rinse it with an alkaline detergent, such as a 5 wt % sodium hydroxide solution, to remove the organic resin coating, and put it into an oven at 45° C. for 18 hours and then cool it naturally.

[0050] Example 3

[0051] A method for treating high buoyancy of an offshore floating bamboo-based platform comprises the following steps:

[0052] S1: Partially cover the bamboo-based buoyancy material to be treated so that only the surface to be treated is exposed to the outside; the covering treatment adopts physical film covering; the physical film covering can be achieved by bonding a plastic film coated with an adhesive to the covering part of the bamboo-based buoyancy material after heating and pressurizing;

[0053] S2: Fix the bamboo-based buoyancy material to be treated in a container, and place it in a vacuum casting tank for vacuum treatment, and the vacuum treatment pressure is 900Pa;

[0054] S3: 400 parts of polyether, 100 parts of isocyanate and 25 parts of initiator dimethyl azobisisobutyrate are subjected to polycondensation reaction to obtain component A, and 15 parts of plasticizer, 30 parts of curing agent, 20 parts of diluent and 350 parts of hydrophobic filler are mixed to obtain component B, and component A and component B are poured into a mixing tank of a vacuum casting tank and stirred evenly;

[0055] The plasticizer is polyethylene terephthalate, the curing agent is benzylenediamine trimer, the diluent is butyl glycidyl ether, and the hydrophobic filler is a mixture of alkane, alkyl alcohol, and alkyl acid in a ratio of 1:1:1.

[0056] S4: Open the discharge port valve of the mixing tank to allow the mixed liquid in the mixing tank to flow into the container containing the bamboo-based buoyancy material, and then use the air compressor to increase the pressure in the vacuum pouring tank to 10,000 Pa, maintain the pressure for 10 minutes, and then release the pressure;

[0057] S5: Take out the bamboo-based buoyancy material, tear off the film covering part after heating, put it into an oven at 50°C for 12 to 20 hours, and then cool it naturally.

[0058] The surface-treated bamboo-based buoyancy materials of Examples 1-3 were subjected to various performance tests, including a water absorption test and a water absorption test after surface damage.

[0059] Water absorption test: The original mass of the surface treated sample is measured as m0, and the sample is placed in a pressure test device, pressurized to 3MPa and maintained for 24 hours, and then the sample is taken out and the surface moisture is wiped dry and its mass is weighed as m1. Water absorption = (m1-m0) / m0×100%

[0060] Water absorption test after surface damage: First, a groove of about 50mm long, 2mm wide and 1mm deep is processed on the surface of the surface treated sample, and then the mass M0 of the processed sample is measured. The sample is placed in a pressure test device and pressed to 3MPa for 24 hours. After the moisture on the surface of the sample is removed and wiped dry, its mass M1 is weighed. Water absorption rate of surface damage = (M1-M0) / M0×100%.

[0061] The test results are shown in the following table:

[0062]

[0063] The water absorption rate of the bamboo-based buoyancy material treated by the high buoyancy treatment method provided by the present invention can be greatly reduced, and the water absorption rate is reduced to below 0.1%, which is much lower than the water absorption rate index of the existing bare buoyancy material, and the volume density of the material is hardly affected after treatment; even if the surface is damaged, the water absorption rate can still be maintained at a low level.

[0064] The present invention uses polyether, isocyanate, initiator, plasticizer, curing agent, diluent and hydrophobic filler as raw materials, and casts the waterproof coating made of the above raw materials on the surface to be treated of the bamboo-based buoyancy material. The corrosion resistance of the surface of the bamboo-based buoyancy material after treatment is enhanced, the water absorption rate is reduced, and it has a certain buffer function, the impact resistance is improved, and the risk of damage is reduced. The waterproof coating is light and has little effect on the overall buoyancy of the bamboo-based buoyancy material. If it is damaged by impact after long-term use, it is easy to find, and only needs to be partially re-brushed.

[0065] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0066] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for treating high buoyancy of an offshore floating bamboo-based platform, characterized in that: The steps include: S1: Partially cover the bamboo-based buoyancy material to be treated so that only the surface to be treated is exposed to the outside; S2: Fix the bamboo-based buoyancy material to be treated in a container, place it in a vacuum pouring tank, and perform vacuum treatment; S3: 300-400 parts of polyether, 100-150 parts of isocyanate and 15-25 parts of initiator are subjected to polycondensation reaction to obtain component A, and 10-20 parts of plasticizer, 20-30 parts of curing agent, 20-30 parts of diluent and 350-450 parts of hydrophobic filler are mixed to obtain component B, and component A and component B are poured into a mixing tank of a vacuum casting tank and stirred evenly; S4: Open the valve of the mixing tank discharge port to allow the mixed liquid in the mixing tank to flow into the container containing the bamboo-based buoyancy material, and then increase the pressure in the vacuum pouring tank through the air compressor, maintain the pressure for 6 to 10 minutes and then release the pressure; S5: Take out the bamboo-based buoyancy material, remove the covered part, put it into the oven for heat preservation and then cool it naturally.

2. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The masking treatment adopts paint masking or physical film masking.

3. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The pressure of the vacuum treatment is 800-900Pa.

4. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The plasticizer is polyethylene terephthalate.

5. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The curing agent is benzylenediamine trimer.

6. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The diluent is butyl glycidyl ether.

7. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The initiator is dimethyl azobisisobutyrate.

8. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: The hydrophobic filler is a mixture of one or more of alkanes, alkyl alcohols and alkyl acids.

9. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: In the above-mentioned S4, the pressure in the vacuum pouring tank is increased to 8000-10000Pa.

10. A method for treating high buoyancy of an offshore floating bamboo-based platform according to claim 1, characterized in that: In the S5, the insulation temperature is 40-50° C. and the insulation time is 12-20 hours.