Ternary positive electrode material precursor and preparation method and application thereof

The ternary cathode material precursor is prepared under a pure oxygen atmosphere through solid-phase spray granulation technology, which solves the problems of long cycle time of the co-precipitation method and the pungent odor of ammonia, improves the density and electrochemical performance of the material, and achieves high efficiency. , safe production process.

CN118771479AActive Publication Date: 2024-10-15湖北金泉新材料有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410899281.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

In the existing ternary cathode material precursor preparation process, the co-precipitation method has a long cycle and low production efficiency, and the ammonia used has a pungent smell, which is harmful to the health of workers.

Method used

Solid-phase spray granulation technology is used to replace the co-precipitation process. Through spray granulation after wet grinding in a pure oxygen atmosphere, binders and defoaming agents are used to improve particle adhesion and bubble elimination, and improve the valence state of metal elements. and compactness.

Benefits of technology

Significantly improve the density and crystallinity of the ternary cathode material precursor, increase the tap density and bulk density, increase the subsequent sintering pot volume and the volume energy density of the cathode, and reduce the process complexity and equipment invest.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a ternary positive electrode material precursor and a preparation method and application thereof. The preparation method comprises the following steps: (1) performing wet grinding on metal salt, a binder, a defoaming agent and a solvent to obtain slurry; and (2) carrying out spray granulation on the slurry in a pure oxygen atmosphere to obtain the ternary positive electrode material precursor. The ternary positive electrode material precursor is prepared by adopting a solid-phase method spray granulation technology instead of a traditional coprecipitation process, the production efficiency is high, the period is short, a complexing agent with pungent smell does not need to be added, the process and equipment are simple, and the industrialization feasibility is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a ternary positive electrode material precursor and a preparation method and application thereof. Background Art

[0002] Ternary positive electrode materials generally use a co-precipitation process to prepare the precursor, which is then blended with the precursor and lithium salt and then subjected to high-temperature solid-phase sintering. However, the co-precipitation method has a long cycle for preparing precursors, usually 3 to 7 days or even longer, and the production efficiency is relatively low; at the same time, the co-precipitation process route is relatively long, and the investment in equipment and plant is large. In addition, in the co-precipitation process, due to the large differences in the solubility product constants of various metal elements (such as nickel, cobalt and manganese), the precipitation rates are different. Ammonia water is usually used as a chelating agent in industry to regulate the precipitation rate and ensure the uniformity of the product. Ammonia water has a pungent odor, which leads to a poor production environment and causes certain harm to the workers' bodies.

[0003] Therefore, there is an urgent need to provide a preparation process for a ternary positive electrode material precursor that can solve the above problems. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a ternary cathode material precursor and its preparation method and application. The present invention adopts solid phase spray granulation technology to replace the traditional coprecipitation process to prepare the ternary cathode material precursor, which has high production efficiency, short cycle, no need to add complexing agents with pungent odor, simple process and equipment, and high industrial feasibility.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a method for preparing a ternary cathode material precursor, the preparation method comprising:

[0007] (1) wet-grinding a metal salt, a binder, a defoamer, and a solvent to obtain a slurry;

[0008] (2) In a pure oxygen atmosphere, the slurry is sprayed and granulated to obtain the ternary positive electrode material precursor.

[0009] The invention provides a preparation method of a ternary cathode material precursor, which adopts a solid phase spray granulation technology to replace a traditional coprecipitation process, has high production efficiency, short cycle, does not need to add a complexing agent with irritating odor, and has simple process and equipment, and high industrial feasibility; the preparation raw materials of the invention include a binder and a defoamer in addition to a metal salt and a solvent, the binder helps to bond between primary particles, and the defoamer can eliminate bubbles generated during the spray granulation process; in addition, the spray granulation process of the invention is carried out under the condition of a pure oxygen atmosphere, and can be pre-oxidized to increase the comprehensive valence state of the metal elements in the ternary cathode material precursor, and can remove OH - (volatile in the form of water vapor), which is beneficial to improve the compactness of the ternary positive electrode material precursor, thereby increasing the tap density and loose density of the ternary positive electrode material precursor, and then increasing the filling amount of the subsequent sintering of the ternary positive electrode material precursor, and increasing production capacity; the corresponding compaction density of the ternary positive electrode material will also increase, and the contact between the particles will be close, so that the internal micropore size of the positive electrode is smaller, which can effectively increase the volume energy density of the positive electrode. In addition, through pre-oxidation, the ternary positive electrode material precursor can exist completely in the form of oxide, with good singleness, and can improve the crystallinity of the precursor, which is beneficial to improve the discharge capacity of the corresponding positive electrode material and improve the first effect.

[0010] Preferably, the metal salt includes at least three of a divalent nickel salt, a divalent cobalt salt, a divalent manganese salt and a trivalent aluminum salt.

[0011] In the present invention, the metal salt can be a combination of a divalent nickel salt, a divalent cobalt salt and a divalent manganese salt, and the corresponding precursor is a nickel-cobalt-manganese ternary precursor; it can also be a combination of a divalent nickel salt, a divalent cobalt salt and a trivalent aluminum salt, and the corresponding precursor is a nickel-cobalt-aluminum ternary precursor.

[0012] In the present invention, the metal salt is preferably a combination of a divalent nickel salt, a divalent cobalt salt and a divalent manganese salt. 2+ , divalent cobalt salts include Co 2+ , divalent manganese salts include Mn 2+ The three elements Ni, Co and Mn in the metal salt are transition metal elements and all have a valence of +2; after wet grinding and spray granulation, the comprehensive valence state of the three elements Ni, Co and Mn in the ternary positive electrode material precursor is increased to +3.

[0013] Preferably, the anion of the metal salt includes at least one of carbonate, oxalate, acetate, nitrate and sulfate.

[0014] Optionally, the metal salt is a hydrated metal salt, that is, the metal salt contains bound water.

[0015] Preferably, the binder comprises at least one of hydroxypropyl cellulose, methyl cellulose, hydroxypropyl methyl cellulose, ethyl cellulose, povidone, copovidone and polyvinyl alcohol.

[0016] Preferably, based on the mass of the metal salt, the mass fraction of the binder is 0.5% to 2.5%, for example, it can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2% or 2.5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the defoaming agent includes at least one of polyether-modified silicone oil, polyurethane, silicones, alcohols, fatty acids, fatty acid esters, phosphates, mineral oils and amides.

[0018] Preferably, in the defoaming agent, the organosilicon includes polysiloxane.

[0019] Preferably, based on the mass of the metal salt, the mass fraction of the defoaming agent is 0.1‰ to 3‰, for example, it can be 0.1‰, 0.2‰, 0.5‰, 0.8‰, 1‰, 1.5‰, 1.8‰, 2‰, 2.5‰, 2.8‰ or 3‰, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the wet-milled raw material further comprises a lubricant, and the lubricant comprises at least one of silicone oil, glycerol, fatty acid amide, oleic acid, polyester, synthetic ester and carboxylic acid.

[0021] In the present invention, the lubricant can improve the fluidity of the slurry, and help the spherical particles formed by spray granulation to be more rounded, smooth, and have better sphericity.

[0022] Preferably, based on the mass of the metal salt, the mass fraction of the lubricant is 0.1‰ to 5‰, for example, it can be 0.1‰, 0.2‰, 0.5‰, 0.8‰, 1‰, 1.5‰, 1.8‰, 2‰, 2.5‰, 2.8‰, 3‰, 3.5‰, 4‰, 4.5‰, 4.8‰ or 5‰, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] In the present invention, if the mass fraction of the lubricant is too small, the improvement of the slurry fluidity is not obvious, the sphericity of the spray granulated particles is not good, the surface of the secondary spheres is not bumpy, and the finished positive electrode material inherits the morphology of the precursor, resulting in an increase in the specific surface area of ​​the material and an increase in the side reactions of the battery; if the mass fraction of the lubricant is too large, it may lead to an increase in the internal resistance of the material, an increase in the proportion of inertness in the positive electrode material, and a decrease in electrochemical properties such as specific capacity.

[0024] Preferably, the wet-milled raw material further comprises a dopant, and the dopant comprises a metal oxide and / or an ammonium salt.

[0025] In the present invention, the introduction of dopants for bulk doping during the precursor preparation stage can ensure the uniformity of doping, achieve the orderliness of the arrangement of doping elements in the transition metal layer within the lattice, and help form a homogeneous solid solution.

[0026] Preferably, the metal oxide includes at least one of ZrO2, Al2O3, TiO2, MgO and WO3.

[0027] In the present invention, metal oxides are added to dope the precursor with metal elements, and the metal elements include at least one of Zr, Al, Ti, Mg and W elements.

[0028] Preferably, based on the theoretical mass of the ternary cathode material precursor being 100%, the mass content of the metal element in the dopant is 500 to 8000 ppm.

[0029] Preferably, the ammonium salt comprises NH4F and / or NH4H2PO4.

[0030] In the present invention, the precursor can be doped with non-metallic elements by adding ammonium salt. When NH4F is added, the doping ion is NH4 + and F - ; When doped with NH4H2PO4, the doping ion is NH4 + and PO4 3- .

[0031] Preferably, the solvent comprises water.

[0032] Preferably, the solid content of the mixture of the metal salt, binder, defoamer, lubricant, dopant and solvent is 10% to 25%, for example, it can be 10%, 12%, 15%, 18%, 20%, 22% or 25%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the wet grinding method includes ball milling and / or sand milling.

[0034] Preferably, the particle size D50 in the slurry is 0.5 μm to 2.5 μm, for example, it can be 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2 μm or 2.5 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] It should be noted that the particles in the slurry are wet-milled raw material particles that are not dissolved in the solvent after wet-milling. No chemical reaction occurs during the wet-milling process, only physical dispersion and mixing.

[0036] In the present invention, when the particle size D50 in the slurry is 0.5 μm to 2.5 μm, it is suitable for the subsequent spray granulation step. If the particle size D50 in the slurry is too small, it means that the wet grinding cycle is long, the efficiency is low, and the effect on improving product performance is small; if the particle size D50 in the slurry is too large, it leads to uneven material dispersion, local large particles lead to concentrated distribution of some elements, and at the same time, the primary particles on the surface of the secondary ball particles after spraying are larger, which is not conducive to the subsequent full mixing and infiltration with lithium salt.

[0037] Preferably, the inlet air temperature of the spray granulation is 450°C to 650°C, for example, it can be 450°C, 480°C, 500°C, 520°C, 550°C, 580°C, 600°C or 650°C, and the outlet air temperature is 100°C to 150°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] In the present invention, when the air inlet temperature of the spray granulation is 450°C to 650°C, sufficient pre-oxidation can be carried out under the condition of pure oxygen atmosphere, which can make the precursor uniform and improve the compactness of the precursor; at the same time, the solvent (such as water) can be removed within this temperature range, and when the metal salt contains bound water, the bound water can be removed within this temperature range, making the ternary positive electrode material precursor more compact. If the air inlet temperature of the spray granulation is too low, the precursor pre-oxidation reaction will be insufficient and the water removal will not be complete; if the air inlet temperature of the spray granulation is too high, the oxygen corrosion to the equipment will be greater, affecting the service life of the equipment.

[0039] Preferably, the spray granulation is performed using a spray dryer.

[0040] Preferably, the chemical formula of the ternary cathode material precursor is (Ni x Co y Y z)2O3, wherein 0<x<1, 0≤y<1, 0<z<1, x+y+z=1, and Y includes Mn and / or Al. The x can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc.; the y can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc.; the z can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] As a preferred technical solution of the present invention, the preparation method specifically comprises:

[0042] (I) wet-grinding a metal salt, a binder, a defoamer, a lubricant, a dopant and a solvent to obtain a slurry;

[0043] The metal salt comprises at least three of divalent nickel salt, divalent cobalt salt, divalent manganese salt and trivalent aluminum salt; the binder comprises at least one of hydroxypropyl cellulose, methyl cellulose, hydroxypropyl methyl cellulose, ethyl cellulose, povidone, copovidone and polyvinyl alcohol; the defoamer comprises at least one of polyether modified silicone oil, polyurethane, silicone, alcohol, fatty acid, fatty acid ester, phosphate ester, mineral oil and amide; the lubricant comprises at least one of silicone oil, glycerol, fatty acid amide, oleic acid, polyester, synthetic ester and carboxylic acid; the solvent comprises water; the particle size D50 of the particles in the slurry is 0.5 μm to 2.5 μm;

[0044] (II) stirring the slurry at a rate of 150 r / min to 500 r / min (e.g., 150 r / min, 180 r / min, 200 r / min, 300 r / min, 400 r / min or 500 r / min, etc.), and spray granulating the slurry as a raw material in a pure oxygen atmosphere to obtain the ternary cathode material precursor;

[0045] The inlet air temperature of the spray granulation is 450°C to 650°C, and the outlet air temperature is 100°C to 150°C; the chemical formula of the ternary cathode material precursor is (Ni x Co y Y z )2O3, wherein 0<x<1, 0≤y<1, 0<z<1, x+y+z=1, and Y includes Mn and / or Al.

[0046] In the present invention, the slurry is stirred at a rate of 150 r / min to 500 r / min in order to prevent the slurry from segregating.

[0047] In a second aspect, the present invention provides a ternary cathode material precursor, which is prepared by the preparation method described in the first aspect.

[0048] Preferably, the particle size D50 of the ternary positive electrode material precursor is 5 μm to 15 μm, for example, it can be 5 μm, 6 μm, 7 μm, 10 μm, 12 μm, 14 μm or 15 μm.

[0049] In a third aspect, the present invention provides a ternary positive electrode material, which is obtained by mixing and sintering the ternary positive electrode material precursor described in the second aspect with a lithium source.

[0050] Preferably, the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium nitrate, lithium oxalate and lithium acetate.

[0051] Preferably, the molar ratio of the lithium element in the lithium source to the transition metal element in the ternary positive electrode material precursor is 1.00 to 1.08, for example, it can be 1.00, 1.02, 1.05, 1.06 or 1.08, but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0052] Preferably, the sintering temperature is 800°C to 950°C, for example, it can be 800°C, 820°C, 850°C, 880°C, 900°C, 920°C or 950°C, and the sintering holding time is 10h to 24h, for example, it can be 10h, 12h, 15h, 18h, 20h, 22h or 24h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] Preferably, when the lithium source is lithium hydroxide, the sintering atmosphere is a pure oxygen atmosphere or an atmosphere with an oxygen volume content of ≥90%; when the lithium source is lithium carbonate, lithium nitrate, lithium oxalate or lithium acetate, the sintering atmosphere is dry compressed air with a dew point ≤-40°C.

[0054] Preferably, after the sintering, the sintered product is subjected to jaw crushing, rolling, pulverization and 200-350 mesh screening to obtain the ternary positive electrode material.

[0055] Preferably, the pulverization includes mechanical pulverization and / or air flow pulverization.

[0056] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the positive electrode of the lithium-ion battery includes the ternary positive electrode material described in the second aspect.

[0057] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0058] Compared with the prior art, the present invention has the following beneficial effects:

[0059] The invention provides a preparation method of a ternary cathode material precursor, which adopts a solid phase spray granulation technology to replace a traditional coprecipitation process, has high production efficiency, short cycle, does not need to add a complexing agent with irritating odor, and has simple process and equipment, and high industrial feasibility; the preparation raw materials of the invention include a binder and a defoamer in addition to a metal salt and a solvent, the binder helps to bond between primary particles, and the defoamer can eliminate bubbles generated during the spray granulation process; in addition, the spray granulation process of the invention is carried out under the condition of a pure oxygen atmosphere, and can be pre-oxidized to increase the comprehensive valence state of the metal elements in the ternary cathode material precursor, and can remove OH - (volatile in the form of water vapor), which is beneficial to improve the compactness of the ternary positive electrode material precursor, thereby increasing the tap density and loose density of the ternary positive electrode material precursor, and then increasing the filling amount of the subsequent sintering of the ternary positive electrode material precursor, and increasing production capacity; the corresponding compaction density of the ternary positive electrode material will also increase, and the contact between the particles will be close, so that the internal micropore size of the positive electrode is smaller, which can effectively increase the volume energy density of the positive electrode. In addition, through pre-oxidation, the ternary positive electrode material precursor can exist completely in the form of oxide, with good singleness, and can improve the crystallinity of the precursor, which is beneficial to improve the discharge capacity of the corresponding positive electrode material and improve the first effect. DETAILED DESCRIPTION

[0060] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0061] Example 1

[0062] This embodiment provides a method for preparing a ternary positive electrode material precursor, the preparation method comprising:

[0063] (1) Wet-grinding a metal salt, a binder, a defoamer, a lubricant, a dopant and a solvent to obtain a slurry, wherein the metal salt is a mixture of NiSO4·6H2O, CoSO4·7H2O and MnSO4·H2O, the binder is polyvinyl alcohol, the defoamer is polyether-modified silicone oil, the lubricant is silicone oil, the dopant is ZrO2, and the solvent is deionized water; based on the mass of the metal salt, the mass fraction of the binder is 1%, the mass fraction of the defoamer is 1‰, the mass fraction of the lubricant is 2‰, and the mass fraction of the dopant is 0.2%; the solid content of the mixture of the metal salt, the binder, the defoamer, the lubricant, the dopant and the solvent is 18%; and the particle size D50 of the particles in the slurry is 1 μm;

[0064] (2) discharging the slurry, stirring the slurry with an electric stirrer at a rate of 400 r / min, and introducing the slurry into a spray dryer for spray granulation under a pure oxygen atmosphere, wherein the inlet air temperature of the spray granulation is 450° C. and the outlet air temperature is 110° C., to obtain the ternary positive electrode material precursor, wherein the chemical formula of the ternary positive electrode material precursor is (Ni 0.83 Co 0.12 Mn 0.05 )2O3, particle size D50 is 15μm.

[0065] This embodiment also provides a method for preparing a ternary positive electrode material using the above-mentioned ternary positive electrode material precursor, the method comprising:

[0066] The ternary positive electrode material precursor and lithium carbonate are mixed, with the molar ratio of lithium element in lithium carbonate to transition metal element in the ternary positive electrode material precursor being 1.04. Then, the mixture is sintered at 910°C for 20 hours in a dry compressed air atmosphere. After the sintering temperature drops below 100°C, the furnace is opened, the material is collected, and then jaw crushing, double-roll crushing, mechanical crushing and 200-mesh screening are performed to obtain the nickel-cobalt-manganese-oxide lithium ternary positive electrode material.

[0067] Example 2

[0068] This embodiment provides a method for preparing a ternary positive electrode material precursor, the preparation method comprising:

[0069] (1) Wet-grinding a metal salt, a binder, a defoamer, a lubricant, a dopant and a solvent to obtain a slurry, wherein the metal salt is a mixture of Ni(NO3)2·6H2O, Co(NO3)2·7H2O and Mn(NO3)2·H2O, the binder is polyvinyl alcohol, the defoamer is polyether-modified silicone oil, the lubricant is silicone oil, the dopant is ZrO2, and the solvent is deionized water; based on the mass of the metal salt, the mass fraction of the binder is 2.5%, the mass fraction of the defoamer is 2‰, the mass fraction of the lubricant is 3‰, the mass fraction of the dopant is 0.3%, and the solid content of the mixture of the metal salt, the binder, the defoamer, the lubricant, the dopant and the solvent is 21%; and the particle size D50 of the particles in the slurry is 0.6 μm;

[0070] (2) discharging the slurry, stirring the slurry with an electric stirrer at a rate of 500 r / min, and introducing the slurry into a spray dryer for spray granulation under a pure oxygen atmosphere, wherein the inlet air temperature of the spray granulation is 600° C. and the outlet air temperature is 120° C., to obtain the ternary positive electrode material precursor, wherein the chemical formula of the ternary positive electrode material precursor is (Ni 0.6 Co 0.2 Mn 0.2 )2O3, particle size D50 is 10μm.

[0071] This embodiment also provides a method for preparing a ternary positive electrode material using the above-mentioned ternary positive electrode material precursor, the method comprising:

[0072] The ternary positive electrode material precursor and lithium carbonate are mixed, with the molar ratio of lithium element in lithium carbonate to transition metal element in the ternary positive electrode material precursor being 1.06, and then sintered at 880°C for 24 hours in a dry compressed air atmosphere. After sintering, the furnace is opened when the temperature drops below 100°C, the material is collected, and then jaw crushing, double roller crushing, mechanical crushing and 200 mesh screening are performed to obtain the nickel cobalt manganese oxide lithium ternary positive electrode material.

[0073] Example 3

[0074] The difference between this embodiment and embodiment 1 is that the mass fraction of the lubricant in step (1) is adjusted to 0.05‰.

[0075] The remaining parameters remain the same as those in Example 1.

[0076] Example 4

[0077] The difference between this embodiment and embodiment 1 is that the mass fraction of the lubricant in step (1) is adjusted to 5.2‰.

[0078] The remaining parameters remain the same as those in Example 1.

[0079] Example 5

[0080] The difference between this embodiment and embodiment 1 is that in step (1), the particle size D50 of the particles in the slurry is 0.3 μm.

[0081] The remaining parameters remain the same as those in Example 1.

[0082] Example 6

[0083] The difference between this embodiment and embodiment 1 is that in step (1), the particle size D50 of the particles in the slurry is 2.8 μm.

[0084] The remaining parameters remain the same as those in Example 1.

[0085] Example 7

[0086] The difference between this embodiment and embodiment 1 is that the inlet air temperature of the spray granulation in step (2) is adjusted to 420°C.

[0087] The remaining parameters remain the same as those in Example 1.

[0088] Example 8

[0089] The difference between this embodiment and embodiment 1 is that the air inlet temperature of the spray granulation in step (2) is adjusted to 680°C.

[0090] The remaining parameters remain the same as those in Example 1.

[0091] Example 9

[0092] This embodiment provides a method for preparing a ternary positive electrode material precursor, the preparation method comprising:

[0093] (1) Wet-grinding a metal salt, a binder, a defoamer, a lubricant, a dopant and a solvent to obtain a slurry, wherein the metal salt is a mixture of Ni(NO3)2·6H2O, Co(NO3)2·7H2O and Al(NO3)3·9H2O, the binder is polyvinyl alcohol, the defoamer is polyether-modified silicone oil, the lubricant is silicone oil, the dopant is ZrO2, and the solvent is deionized water; based on the mass of the metal salt, the mass fraction of the binder is 2.5%, the mass fraction of the defoamer is 2‰, the mass fraction of the lubricant is 3‰, the mass fraction of the dopant is 0.3%, and the solid content of the mixture of the metal salt, the binder, the defoamer, the lubricant, the dopant and the solvent is 21%; and the particle size D50 of the particles in the slurry is 0.6 μm;

[0094] (2) discharging the slurry, stirring the slurry with an electric stirrer at a rate of 500 r / min, and introducing the slurry into a spray dryer for spray granulation under a pure oxygen atmosphere, wherein the inlet air temperature of the spray granulation is 600° C. and the outlet air temperature is 120° C., to obtain the ternary positive electrode material precursor, wherein the chemical formula of the ternary positive electrode material precursor is (Ni 0.8 Co 0.15 Al 0.05 )2O3, particle size D50 is 10μm.

[0095] This embodiment also provides a method for preparing a ternary positive electrode material using the above-mentioned ternary positive electrode material precursor, the method comprising:

[0096] The ternary positive electrode material precursor and lithium carbonate are mixed, with the molar ratio of lithium element in lithium carbonate to transition metal element in the ternary positive electrode material precursor being 1.06, and then sintered at 880°C for 24 hours in a dry compressed air atmosphere. After sintering, the furnace is opened when the temperature drops below 100°C, the material is collected, and then jaw crushing, double roller crushing, mechanical crushing and 200 mesh screening are performed to obtain nickel cobalt aluminum oxide lithium ternary positive electrode material.

[0097] Comparative Example 1

[0098] The difference between this comparative example and Example 1 is that the atmosphere of the spray granulation was adjusted to air atmosphere.

[0099] The remaining parameters remain the same as those in Example 1.

[0100] Performance Testing

[0101] The tap density and bulk density of the ternary cathode material precursors provided in the above embodiments and comparative examples were tested; the first effect test of the provided ternary cathode material was performed:

[0102] Tap density: Refer to GB / T 31057.2 Part 2: Measurement of tap density.

[0103] Bulk density: Refer to GB / T 31057.1 Part 1: Measurement of bulk density.

[0104] First effect: Refer to GB / T 23365-2023 lithium cobalt oxide electrochemical performance test first discharge specific capacity and first charge and discharge efficiency test method.

[0105] The test results are shown in Table 1.

[0106] Table 1

[0107] <![CDATA[Tap density (g / cm 3 )]]> <![CDATA[Bulk density (g / cm 3 )]]> First effect (%) Example 1 2.31 1.18 88 Example 2 2.29 1.15 87 Example 3 2.28 1.13 85 Example 4 2.24 1.10 81 Example 5 2.26 1.09 84 Example 6 2.29 1.14 81 Example 7 2.29 1.15 82 Example 8 2.31 1.18 84 Example 9 2.28 1.14 88 Comparative Example 1 2.26 1.12 80

[0108] analyze:

[0109] It can be seen from Examples 1-2 and Example 9 that the ternary precursor material prepared by the method of the present invention is dense, has small particle gaps, and has a high loading capacity in subsequent sintering, which can improve production capacity and has high production efficiency; the corresponding ternary positive electrode material has a higher initial efficiency.

[0110] It can be seen from Example 1 and Examples 3-4 that in the wet-ground raw materials, if the mass fraction of the lubricant is too small, the surface of the precursor material particles will be rough, the specific surface area will be large, and the density will be reduced; if the mass fraction of the lubricant is too large, the particle size will be smaller, the tap density will be reduced, and the initial efficiency of the positive electrode material will be reduced.

[0111] It can be seen from Example 1 and Examples 5-6 that after wet grinding, if the particle size D50 in the slurry is too small, the secondary spherical particles will be smaller in size, and the tapped and loose density will be smaller; if the particle size D50 in the slurry is too large, the primary particles on the surface of the secondary spherical particles will be larger, the gaps between the primary particles will be larger, the specific surface area will increase, and the electrochemical performance of the material will decrease (the first effect will decrease).

[0112] It can be seen from Example 1 and Examples 7-8 that if the inlet air temperature of the spray granulation is too low, it will lead to insufficient pre-oxidation of the precursor, poor material uniformity, and reduced overall performance; if the inlet air temperature of the spray granulation is too high, it will lead to excessive pre-oxidation of the precursor, resulting in larger primary particles on the surface of the secondary spherical particles, reduced primary efficiency, and greater oxygen corrosion to the spray equipment.

[0113] It can be seen from Example 1 and Comparative Example 1 that when the atmosphere of the spray granulation is adjusted to an air atmosphere, the precursor pre-oxidation is insufficient, the material uniformity is poor, and the overall performance is reduced.

[0114] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a ternary cathode material precursor, characterized in that: The preparation method comprises: (1) wet-grinding a metal salt, a binder, a defoamer, and a solvent to obtain a slurry; (2) In a pure oxygen atmosphere, the slurry is sprayed and granulated to obtain the ternary positive electrode material precursor.

2. The preparation method according to claim 1, characterized in that: The metal salt includes at least three of a divalent nickel salt, a divalent cobalt salt, a divalent manganese salt and a trivalent aluminum salt.

3. The preparation method according to claim 1 or 2, characterized in that: The binder comprises at least one of hydroxypropyl cellulose, methyl cellulose, hypromellose, ethyl cellulose, povidone, copovidone and polyvinyl alcohol; Preferably, based on the mass of the metal salt, the mass fraction of the binder is 0.5% to 2.5%; Preferably, the defoaming agent includes at least one of polyether-modified silicone oil, polyurethane, silicone, alcohol, fatty acid, fatty acid ester, phosphate ester, mineral oil and amide; Preferably, based on the mass of the metal salt, the mass fraction of the defoaming agent is 0.1‰ to 3‰.

4. The preparation method according to any one of claims 1 to 3, characterized in that The wet-milled raw material also includes a lubricant, and the lubricant includes at least one of silicone oil, glycerol, fatty acid amide, oleic acid, polyester, synthetic ester and carboxylic acid; Preferably, based on the mass of the metal salt, the mass fraction of the lubricant is 0.1‰ to 5‰; Preferably, the wet-milled raw material further comprises a dopant, and the dopant comprises a metal oxide and / or an ammonium salt; Preferably, the metal oxide includes at least one of ZrO2, Al2O3, TiO2, MgO and WO3; Preferably, the ammonium salt comprises NH4F and / or NH4H2PO4; Preferably, the solvent comprises water; Preferably, the solid content of the mixture of the metal salt, the binder, the defoamer, the lubricant, the dopant and the solvent is 10% to 25%.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The wet grinding method includes ball milling and / or sand milling; Preferably, the particle size D50 of the particles in the slurry is 0.5 μm to 2.5 μm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The inlet air temperature of the spray granulation is 450°C to 650°C, and the outlet air temperature is 100°C to 150°C; Preferably, the chemical formula of the ternary cathode material precursor is (Ni x Co y Y z )2O3, wherein 0<x<1, 0≤y<1, 0<z<1, x+y+z=1, and Y includes Mn and / or Al.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method specifically comprises: (I) wet-grinding a metal salt, a binder, a defoamer, a lubricant, a dopant and a solvent to obtain a slurry; The metal salt comprises at least three of divalent nickel salt, divalent cobalt salt, divalent manganese salt and trivalent aluminum salt; the binder comprises at least one of hydroxypropyl cellulose, methyl cellulose, hydroxypropyl methyl cellulose, ethyl cellulose, povidone, copovidone and polyvinyl alcohol; the defoamer comprises at least one of polyether modified silicone oil, polyurethane, silicone, alcohol, fatty acid, fatty acid ester, phosphate ester, mineral oil and amide; the lubricant comprises at least one of silicone oil, glycerol, fatty acid amide, oleic acid, polyester, synthetic ester and carboxylic acid; the solvent comprises water; the particle size D50 of the particles in the slurry is 0.5 μm to 2.5 μm; (II) stirring the slurry at a rate of 150 r / min to 500 r / min, and spray granulating the slurry as a raw material in a pure oxygen atmosphere to obtain the ternary cathode material precursor; The inlet air temperature of the spray granulation is 450°C to 650°C, and the outlet air temperature is 100°C to 150°C; the chemical formula of the ternary cathode material precursor is (Ni x Co y Y z )2O3, wherein 0<x<1, 0≤y<1, 0<z<1, x+y+z=1, and Y includes Mn and / or Al.

8. A ternary cathode material precursor, characterized in that: The ternary cathode material precursor is prepared by the preparation method according to any one of claims 1 to 7; Preferably, the particle size D50 of the ternary cathode material precursor is 5 μm to 15 μm.

9. A ternary positive electrode material, characterized in that: The ternary positive electrode material is obtained by mixing and sintering the ternary positive electrode material precursor described in claim 8 with a lithium source.

10. A lithium ion battery, characterized in that: The positive electrode of the lithium-ion battery includes the ternary positive electrode material according to claim 9.

Citation Information

Patent Citations

  • Novel method for preparing lithium ion battery anode ternary material LiCoxNiyMn2O2

    CN101369651A

  • Nickel cobalt lithium aluminate positive material and preparation method thereof

    CN103985856A

  • Ternary positive electrode material and preparation method thereof

    CN115215388A

  • Na &lt; + &gt;-doped ternary lithium ion battery positive electrode material and spray drying preparation method

    CN116553629A

  • Preparation method of ternary precursor in oxygen-containing atmosphere

    CN118183875A