Excitant for high-volume slag cement and preparation method thereof

By using a specific combination of activators in large amounts of slag cement, including early strength, reinforcement, grinding aid and static elimination components, the problems of low grinding efficiency and insufficient compressive strength of slag cement are solved, and a more efficient process is achieved. Grinding and stronger compressive strength, superior to commercially available grinding aids.

CN118771771AActive Publication Date: 2024-10-15SHANDONG HONGYI TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410843506.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

The existing technology has low grinding efficiency and insufficient compressive strength in large-volume slag cement, making it difficult to effectively replace clinker, resulting in increased carbon dioxide emissions.

Method used

A large-amount activator for slag cement is used, including early strength components, reinforcing components, grinding aid components, static elimination components and stable solubilizing components, through aluminum sulfate, sodium thiocyanate, and sodium hydroxide. , sodium fluoroborate, magnesium hydroxide, glycol The combination of acid, triethanolamine, sodium alkyl succinate disulfonate, dodecyldimethyl tertiary amine and urea promotes the dissolution of slag glass, reduces the degree of silicon-oxygen tetrahedral polymerization, fills microstructure voids and pores, speeding up the grinding process.

Benefits of technology

Significantly improves the grinding efficiency and compressive strength of large-volume slag cement. The 45μm decreases by 3-3.5%, the 3d compressive strength increases by 4.1-5.4MPa, and the 28d compressive strength increases by 5.9-8.9MPa, which is better than commercially available grinding aids. agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004915051930000061
    Figure BDA0004915051930000061
  • Figure BDA0004915051930000071
    Figure BDA0004915051930000071
Patent Text Reader

Abstract

The invention discloses an activator for high-volume slag cement and a preparation method of the activator, and belongs to the technical field of cement admixtures. The activator comprises the following raw materials in parts by weight: 20-50 parts of an early strength component, 2-5 parts of a reinforcing component, 3-8 parts of a grinding aid component, 0.1-0.5 part of a static elimination component, 0.1-1 part of a stable solubilizing component and 30-70 parts of water. After the activator provided by the invention is added, the 45-micron compressive strength is reduced by 3-3.5%, the 3d compressive strength of cement mortar is increased by 4.1-5.4 MPa, the 28d compressive strength is increased by 5.9-8.9 MPa, and the grinding aiding and enhancing effects are obviously superior to those of a commercially available grinding aid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cement admixtures, and particularly relates to an activator for high-volume slag cement and a preparation method thereof. Background Art

[0002] Cement is an important component of concrete. Its production process can be summarized as "two grindings and one burning" (raw material grinding, clinker calcining, and clinker grinding). The main links that produce CO2 are coal combustion, limestone decomposition, and electricity and heat consumption. For every ton of clinker produced, about 0.8-1.0t of CO2 is produced.

[0003] Blast furnace slag is the molten silicate and aluminate minerals discharged from the steel industry when smelting pig iron in blast furnaces. The amount produced is usually 30-35% of the pig iron output. The chemical composition and mineral composition of slag are similar to those of silicate cement clinker. When used as a mixed material to produce cement, it only produces and emits CO2 during the power consumption in the grinding process (some processes include fuel combustion). Replacing clinker with slag in equal proportion can reduce CO2 emissions in the clinker production stage. If slag is used to replace clinker in cement production, carbon dioxide emissions can be greatly reduced.

[0004] However, slag is generally formed by water quenching and rapid cooling. During this process, the liquid phase does not have time to crystallize and forms a glassy body. It has problems such as poor abrasiveness and low early activity, which to a certain extent limits its use in cement.

[0005] At present, most of the activators for slag cement are used in the preparation of cement doped with a small amount of slag, and the effect is not good for slag cement with a large amount of slag. For example: Chinese patent application CN202010050676.7 discloses a slag cement activator and a preparation method thereof. The raw material components are calculated by mass fraction and include: polyethylene glycol 5%-10%, polyvinyl alcohol 2%-5%, polyvinyl pyrrolidone 2%-8%, diethanol monoisopropanolamine 10%-30%, water 15%-60%, and the pH value of the slag cement activator ranges from 5 to 12. Stir all the raw materials at 10°C-60°C for 20-120 minutes to obtain a slag cement activator.

[0006] Therefore, developing an activator for high-volume slag cement to improve the grinding efficiency of high-volume cement is a technical problem that needs to be solved urgently. Summary of the invention

[0007] In view of the above problems, the present invention provides an activator for high-volume slag cement, which can improve the grinding efficiency of high-volume slag cement and effectively improve its compressive strength. To achieve the above objectives, the present invention adopts the following technical solutions.

[0008] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 20-50 parts of an early strength component, 2-5 parts of a reinforcing component, 3-8 parts of a grinding aid component, 0.1-0.5 parts of a static elimination component, 0.1-1 parts of a stabilizing solubilizing component, and 30-70 parts of water.

[0009] Furthermore, the early strength component includes aluminum sulfate, sodium thiocyanate and sodium hydroxide.

[0010] Furthermore, the weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is (30-60):(10-20):1.

[0011] Furthermore, the reinforcing component includes sodium fluoroborate, magnesium hydroxide and glycolic acid.

[0012] Furthermore, the weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is (4-8):(2-5):1.

[0013] Furthermore, the grinding aid component includes triethanolamine and sodium alkyl disulfonate succinate.

[0014] Furthermore, the weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is (5-10):1.

[0015] Furthermore, the static elimination component is dodecyl dimethyl tertiary amine.

[0016] Furthermore, the stable solubilizing component includes urea, dihydroxyaminoacetic acid aluminum, and carbomer, and the weight ratio of the three is (10-50): (2-5): 1.

[0017] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0018] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate to the reactor in proportion, and heat to 40°C.

[0019] Keep warm at -60℃ for 0.5-1h, wait until aluminum sulfate is completely dissolved, then add sodium hydroxide solution with a mass concentration of 30% and drip it in, add it in 0.5-1h, keep warm for 2-3h, and obtain the early strength component solution;

[0020] (2) adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches,

[0021] Stir evenly and cool to room temperature to obtain the activator.

[0022] Beneficial Effects

[0023] (1) In the activator of the present invention, the early strength component can introduce a large amount of AlO2 into the low carbon slag cement paste - 、SO4 2- and OH - , where OH - Can promote the dissolution of slag glass, AlO2 - 、SO4 2- Will and system Ca 2+ React to generate AFt and improve early strength;

[0024] (2) The magnesium hydroxide nuclei in the reinforcing component can reduce the nucleation barrier of CSH, promote the hydration of C3S, fill the microstructure voids and pores formed by rapid condensation, and glycolic acid can react with Ca in the slag powder particles. 2+ Mg 2+ reaction, promoting ion dissolution, F - Can replace O in Si-O bonds or Al-O bonds in slag glass 2- , respectively forming [SiO3F] 3- 、[AlO3F] 4- , reduce the number of oxygen bridges, reduce the degree of polymerization of silicon-oxygen tetrahedrons, and improve the reaction activity of slag powder;

[0025] (3) In the grinding aid component, triethanolamine and sodium alkyl disulfonate succinate are used at the same time. The combination of the two has a highly efficient adsorption effect, which not only penetrates into the cracks of the slag particles, fills the fine cracks, and makes it difficult for the cracks to heal by themselves, but also causes the existing cracks to form a "wedge splitting effect", accelerates the crack expansion, and thus promotes the refinement process of the slag particles. It can also more effectively reduce the surface energy of the slag powder, which is conducive to the formation and expansion of cracks in the slag particles during grinding;

[0026] (4) Adding dodecyl dimethyl tertiary amine as a static elimination component can form a conductive grid to allow static charges to move, part of which is dissipated into the surrounding air and carried away by the wind inside the mill, and part of which is neutralized with the surrounding opposite charges, thereby accelerating the dissipation of surface charges and preventing particle aggregation caused by static electricity;

[0027] (5) Adding stabilizing solubilizing components such as urea, dihydroxyaminoacetic acid aluminum, and carbomer can form a network structure in the slag cement system, greatly slowing down the sedimentation of solid particles and increasing the stability of the system;

[0028] (6) The composite early strength component, reinforcing component, grinding aid component, static elimination component, stabilizing solubilizing component, etc. of the present invention together constitute an activator for slag cement. The components work synergistically to improve the grinding efficiency of large-volume slag cement and effectively improve its compressive strength. After adding the activator of the present invention, 45μm decreases by 3-3.5%, the 3d compressive strength of cement mortar increases by 4.1-5.4MPa, and the 28d compressive strength increases by 5.9-8.9MPa. The grinding aid and reinforcing effects are significantly better than those of commercially available grinding aids. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.

[0030] Example 1

[0031] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 20 parts of an early strength component, 5 parts of a reinforcing component, 3 parts of a grinding aid component, 0.5 parts of a static elimination component, 0.1 parts of a stabilizing solubilizing component, and 70 parts of water.

[0032] The weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is 30:20:1.

[0033] The weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is 8:2:1.

[0034] The weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is 5:1.

[0035] The static elimination component is dodecyl dimethyl tertiary amine.

[0036] The stable solubilizing component comprises urea, dihydroxyaminoacetic acid aluminum and carbomer, and the weight ratio of the three is 10:5:1.

[0037] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0038] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate to the reactor in proportion, and heat to

[0039] Keep warm at 40℃ for 1 hour. After aluminum sulfate is completely dissolved, prepare sodium hydroxide into a sodium hydroxide solution with a mass concentration of 30% and drip it. The addition is completed in 0.5 hour. Keep warm for 3 hours to obtain an early strength component solution.

[0040] (2) Adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches, stirring evenly, and cooling to room temperature to obtain the activator.

[0041] Example 2

[0042] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 50 parts of an early strength component, 2 parts of a reinforcing component, 8 parts of a grinding aid component, 0.1 parts of a static elimination component, 1 part of a stabilizing solubilizing component, and 30 parts of water.

[0043] The weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is 60:10:1.

[0044] The weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is 4:5:1.

[0045] The weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is 10:1.

[0046] The static elimination component is dodecyl dimethyl tertiary amine.

[0047] The stable solubilizing component comprises urea, dihydroxyaminoacetic acid aluminum and carbomer, and the weight ratio of the three is 50:2:1.

[0048] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0049] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate in proportion to the reactor, heat to 60° C. and keep warm for 0.5 h. After the aluminum sulfate is completely dissolved, prepare sodium hydroxide to a sodium hydroxide solution with a mass concentration of 30% and then drop it in. The addition is completed within 1 h, and the temperature is kept warm for 2 h to obtain an early strength component solution;

[0050] (2) Adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches, stirring evenly, and cooling to room temperature to obtain the activator.

[0051] Example 3

[0052] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 30 parts of an early strength component, 4 parts of a reinforcing component, 6 parts of a grinding aid component, 0.3 parts of a static elimination component, 0.5 parts of a stabilizing solubilizing component, and 54 parts of water.

[0053] The weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is 50:10:1.

[0054] The weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is 5:3:1.

[0055] The weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is 8:1.

[0056] The static elimination component is dodecyl dimethyl tertiary amine.

[0057] The stable solubilizing component comprises urea, dihydroxyaminoacetic acid aluminum and carbomer, and the weight ratio of the three is 20:3:1.

[0058] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0059] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate in proportion to the reactor, heat to 50° C. and keep warm for 40 minutes, wait for the aluminum sulfate to be completely dissolved, then add sodium hydroxide to a sodium hydroxide solution with a mass concentration of 30% and drip it in, add it in 0.8 hours, keep warm for 2.5 hours, and obtain an early strength component solution;

[0060] (2) Adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches, stirring evenly, and cooling to room temperature to obtain the activator.

[0061] Example 4

[0062] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 40 parts of an early strength component, 3 parts of a reinforcing component, 5 parts of a grinding aid component, 0.2 parts of a static elimination component, 0.7 parts of a stabilizing solubilizing component, and 49 parts of water.

[0063] Furthermore, the weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is 55:15:1.

[0064] Furthermore, the weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is 6:4:1.

[0065] Furthermore, the weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is 6:1.

[0066] Furthermore, the static elimination component is dodecyl dimethyl tertiary amine.

[0067] Furthermore, the stable solubilizing component includes urea, dihydroxyaminoacetic acid aluminum, and carbomer, and the weight ratio of the three is 30:4:1.

[0068] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0069] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate to the reactor in proportion, and heat to

[0070] Keep warm at 45℃ for 1 hour. After aluminum sulfate is completely dissolved, prepare sodium hydroxide into a sodium hydroxide solution with a mass concentration of 30% and drip it. Add it in 1 hour and keep warm for 3 hours to obtain an early strength component solution.

[0071] (2) Adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches, stirring evenly, and cooling to room temperature to obtain the activator.

[0072] Comparative Example 1

[0073] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 30 parts of an early strength component, 4 parts of a reinforcing component, 6 parts of a grinding aid component, 0.5 parts of a stabilizing solubilizing component, and 54 parts of water.

[0074] The weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is 50:10:1.

[0075] The weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is 5:3:1.

[0076] The weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is 8:1.

[0077] The stable solubilizing component comprises urea, dihydroxyaminoacetic acid aluminum and carbomer, and the weight ratio of the three is 20:3:1.

[0078] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0079] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate in proportion to the reactor, heat to 50° C. and keep warm for 40 minutes, wait for the aluminum sulfate to be completely dissolved, then add sodium hydroxide to a sodium hydroxide solution with a mass concentration of 30% and drip it in, add it in 0.8 hours, keep warm for 2.5 hours, and obtain an early strength component solution;

[0080] (2) Adding the stabilizing solubilizing component, the grinding aid component and the strengthening component to the early strength component solution in batches, stirring evenly, and cooling to room temperature to obtain the activator.

[0081] In this comparative example, except that no static elimination component is added to the raw material composition, the other raw materials and preparation method are the same as those in Example 3.

[0082] Comparative Example 2

[0083] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 30 parts of an early strength component, 6 parts of a grinding aid component, 0.3 parts of a static elimination component, 0.5 parts of a stabilizing solubilizing component, and 54 parts of water.

[0084] In this comparative example, except that no reinforcing component is added to the raw material composition, the other raw materials and preparation method are the same as those in Example 3.

[0085] Comparative Example 3

[0086] An activator for high-volume slag cement comprises the following raw materials in parts by weight: 30 parts of an early strength component, 4 parts of a reinforcing component, 6 parts of a grinding aid component, 0.3 parts of a static elimination component, 0.5 parts of a stabilizing solubilizing component, and 54 parts of water.

[0087] The weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is 50:10:1.

[0088] The weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is 5:3:1.

[0089] The grinding aid component is triethanolamine.

[0090] The static elimination component is dodecyl dimethyl tertiary amine.

[0091] The stable solubilizing component comprises urea, dihydroxyaminoacetic acid aluminum and carbomer, and the weight ratio of the three is 20:3:1.

[0092] A method for preparing an activator for high-volume slag cement comprises the following preparation steps:

[0093] (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate in proportion to the reactor, heat to 50° C. and keep warm for 40 minutes, wait for the aluminum sulfate to be completely dissolved, then add sodium hydroxide to a sodium hydroxide solution with a mass concentration of 30% and drip it in, add it in 0.8 hours, keep warm for 2.5 hours, and obtain an early strength component solution;

[0094] (2) adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches,

[0095] Stir evenly and cool to room temperature to obtain the activator.

[0096] In this comparative example, except that only conventional triethanolamine is used in the grinding aid component, the remaining raw materials and preparation method are the same as those in Example 3.

[0097] Performance Testing

[0098] In order to further verify the effect of the activator of the present invention, the above-mentioned Examples 1-4, Comparative Examples 1-3, and the commercially available grinding aid HLA-GO10 were mixed into cement, and the mixing amount was 0.1% of the total weight of cement, and a blank comparative example was set, that is, no admixture was added; a total of 9 experimental groups were set, each experimental group was repeated 5 times, and the various properties were statistically compared, and the experimental results were averaged:

[0099] Cement raw material mix ratio: clinker 25wt%, slag 70wt%, gypsum 5wt%.

[0100] Test operation: The moisture content of all raw materials is controlled below 1%, and the raw material particles crushed to 1mm to 7mm are mixed evenly and set aside. One part is used to prepare a blank sample without activator (grinding aid), and the other part is used to prepare a comparative sample with activator (grinding aid).

[0101] 1) Preparation of blank samples

[0102] 5 kg of cement clinker, slag and gypsum were prepared in a mass ratio of 25:70:5 and ground in a small test mill that met the requirements to a specific surface area of ​​370 m 2 / kg±10m 2 / kg, record the grinding time T s , the 45μm sieve residue of cement is determined according to GB / T1345. Then the ground cement is tested for cement strength according to the national standard GB / T17671-2021 "Test method for cement mortar strength", and the setting time and other properties are tested according to the national standard GB / T1346-2011.

[0103] 2) Preparation of comparative samples

[0104] According to the preparation method of blank sample, two portions of 5 kg cement clinker, slag and gypsum were prepared, and the grinding aid (activator) was evenly added to the clinker according to the recommended dosage (internal addition), and the powder was ground. s Time (T. time described in A.4.2), grind twice. Discard the first grind sample added with grinding aid (activator), and measure the 45μm sieve residue of the second grind sample. Then test the cement strength according to the national standard GB / T17671-2021 cement mortar strength test method, and test the setting time and other properties according to the national standard GB / T1346-2011.

[0105] The performance test results are shown in Table 1 below.

[0106] Table 1 Cement performance test results

[0107]

[0108]

[0109] As can be seen from Table 1, after adding the activator of the present invention, 45μm decreased by 3-3.5%, the 3d compressive strength of cement mortar increased by 4.1-5.4MPa, and the 28d compressive strength increased by 5.9-8.9MPa, and the grinding aid and enhancement effects were significantly better than those of commercial grinding aids. However, when the key components 1-3 were changed, the various properties of the cement samples obtained showed a downward trend.

[0110] This is because cement will cut off the internal covalent bonds of the particles during the crushing process, resulting in changes in electron density, so staggered active points of calcium ions and oxygen ions appear on both sides of the cross section. When there is no foreign substance to shield these active points, they will attract each other, causing the broken interface to tend to heal, resulting in the phenomenon of material aggregation during the grinding process. The role of the static elimination component is that it can quickly adsorb on the surface of the particles to form an adsorption layer to reduce the surface energy, and provide foreign ions or molecules to neutralize the free charge and unsaturated valence bonds on the cross section, eliminate the tendency of accumulation, and prevent the fracture surface of the material particles from recombining. Compared with Example 3, the 45μm reduction in Comparative Example 1 without adding the static elimination component is significantly reduced, the particles are coarser, and the grinding aid effect is worse. At the same time, the cement fineness becomes coarser, which affects the strength development. Comparative Example 3 using conventional grinding aid components does not have the synergistic grinding aid effect of sodium succinate alkyl disulfonate, the grinding aid effect is reduced, and the particles are also coarser. Comparative Example 2 lacks the reinforcing component, and its overall performance also shows a decline to varying degrees, and the decline in strength performance is more obvious. It can be seen that the addition of the reinforcing component, the static eliminating component and the sodium alkyl disulfonate of succinate is crucial to improving the performance of high-volume slag cement, and the effect will be weak if any one of them is missing.

[0111] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. An activator for high-volume slag cement, It is characterized in that The invention comprises the following raw materials in parts by weight: 20-50 parts of early strength component, 2-5 parts of reinforcing component, 3-8 parts of grinding aid component, 0.1-0.5 parts of static elimination component, 0.1-1 parts of stabilizing solubilizing component and 30-70 parts of water.

2. The activator for high-volume slag cement according to claim 1, It is characterized in that The early strength component includes aluminum sulfate, sodium thiocyanate and sodium hydroxide.

3. The activator for high-volume slag cement according to claim 2, It is characterized in that The weight ratio of aluminum sulfate, sodium thiocyanate and sodium hydroxide in the early strength component is (30-60):(10-20):

1.

4. The activator for high-volume slag cement according to claim 1, It is characterized in that The reinforcing component includes sodium fluoroborate, magnesium hydroxide and glycolic acid.

5. The activator for high-volume slag cement according to claim 4, It is characterized in that The weight ratio of sodium fluoroborate, magnesium hydroxide and glycolic acid in the reinforcing component is (4-8):(2-5):

1.

6. The activator for high-volume slag cement according to claim 1, It is characterized in that The grinding aid component comprises triethanolamine and sodium alkyl disulfosuccinate.

7. The activator for high-volume slag cement according to claim 6, It is characterized in that The weight ratio of triethanolamine to sodium alkyl succinate disulfonate in the grinding aid component is (5-10):

1.

8. The activator for high-volume slag cement according to claim 1, It is characterized in that The static elimination component is dodecyl dimethyl tertiary amine.

9. The activator for high-volume slag cement according to claim 1, It is characterized in that The stable solubilizing component comprises urea, dihydroxyaminoacetic acid aluminum and carbomer, and the weight ratio of the three is (10-50): (2-5):

1.

10. A method for preparing the activator for high-volume slag cement according to any one of claims 1 to 9, It is characterized in that Bag The preparation steps include: (1) Add water to the reactor, start stirring, add aluminum sulfate and sodium thiocyanate to the reactor in proportion, heat to 40°C-60°C and keep warm for 0.5-1h, wait until the aluminum sulfate is completely dissolved, and then add sodium hydroxide to a mass concentration of 30% sodium thiocyanate. Then, add the sodium solution dropwise, and the addition will be completed in 0.5-1h. Keep warm for 2-3h to obtain the early strength component solution. (2) Adding the stabilizing solubilizing component, the grinding aid component, the strengthening component and the static eliminating component to the early strength component solution in batches, stirring evenly, and cooling to room temperature to obtain the activator.

Citation Information

Patent Citations

  • Reinforced cement grinding aid and preparation method thereof

    CN103274632A

  • Granulated blast furnace slag exciting agent as well as preparation method and application thereof

    CN108083671A

  • High-strength anti-fatigue load steel-concrete connection grouting material and preparation method thereof

    CN115925350A

  • Cement regeneration technique by activating discarded concrete

    CN1990410A

  • Activator for high volume slag cement, high volume slag cement composition containing the activator and process of the cement

    KR1020130087240A