High-wear-resistance zirconia ceramic ball and preparation method thereof
Through multi-layer structure design and self-healing microcapsule materials, combined with electric field sintering technology, the brittleness problem of traditional zirconia ceramic balls in high stress environments has been solved, and ceramic balls with high hardness, wear resistance and toughness have been achieved, significantly improving Wear resistance and service life.
Patent Information
- Application Number
- CN202410781877.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional zirconia ceramic balls are difficult to achieve high hardness, high wear resistance and high toughness at the same time, and are prone to brittle fracture or rapid wear in high stress and high wear environments.
It adopts a multi-layer structure design of high wear-resistant layer, gradient transition layer and reinforced core layer, combined with nano-zirconia, micron zirconia, self-healing microcapsule materials and electric field-assisted sintering technology to optimize the sintering temperature and heating and cooling rate to form a high-performance Hardness, wear resistance and toughness of ceramic balls.
The wear resistance and toughness of the ceramic ball are significantly improved, internal stress and cracks are reduced, the service life is extended, and the reliability and comprehensive performance are improved through the self-healing function.
Smart Images

Figure BDA0004897379160000041 
Figure BDA0004897379160000042 
Figure BDA0004897379160000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic ball preparation, in particular to a high-wear-resistant zirconia ceramic ball and a preparation method thereof. Background Art
[0002] High wear-resistant zirconia ceramic balls are an important wear-resistant material with a wide range of applications in the industrial field. Its preparation process needs to consider a variety of factors, including raw material selection, molding process, sintering process, etc., to ensure that the final product has excellent physical and mechanical properties.
[0003] Highly wear-resistant zirconia ceramic balls have extremely high hardness and wear resistance in industrial applications, but the traditional single material design has certain defects under various working conditions. It is difficult for traditional zirconia ceramic balls to simultaneously take into account high hardness, high wear resistance and high toughness. Zirconia ceramic balls are prone to brittle fracture or rapid wear under high stress and high wear environments.
[0004] Therefore, we propose a high wear-resistant zirconia ceramic ball and a preparation method thereof. Summary of the invention
[0005] In order to make up for the deficiencies of the prior art, the present invention proposes a highly wear-resistant zirconia ceramic ball and a preparation method thereof. The present invention is mainly used to solve the problem that traditional zirconia ceramic balls are difficult to simultaneously achieve high hardness, high wear resistance and high toughness, and zirconia ceramic balls are prone to brittle fracture or rapid wear under high stress and high wear environments.
[0006] A highly wear-resistant zirconia ceramic ball, comprising a surface structure consisting of a highly wear-resistant layer, an intermediate structure consisting of a gradient transition layer, and a core structure consisting of a reinforced core layer;
[0007] Every 100 parts by mass of the high wear-resistant layer components include: 85-90 parts by mass of ZrO2 nanopowder, 4-5 parts by mass of Y2O3 stabilizer, 1-3 parts by mass of CeO2 stabilizer, 0.5-1.5 parts by mass of carbon nanotubes, 1-10 parts by mass of self-repairing microcapsule material and 3-5 parts by mass of additives;
[0008] Every 100 parts by weight of the gradient transition layer comprises: 85-92 parts by weight of ZrO2 micron powder, 4-5 parts by weight of Y2O3 stabilizer, 1-2 parts by weight of CeO2 stabilizer, 1-10 parts by weight of self-repairing microcapsule material, 1 part by weight of nano-silicate microspheres and 3-4 parts by weight of additives; the ZrO2 content of the gradient transition layer changes gradually in a gradient form, the ZrO2 content of the surface layer is the same as that of the high wear-resistant layer material, and the ZrO2 content of the core part is the same as that of the enhanced core layer;
[0009] Every 100 parts by mass of the reinforced core layer components include: 88-92 parts by mass of ZrO2 micron powder, 4-5 parts by mass of Y2O3 stabilizer, 1-2 parts by mass of CeO2 stabilizer, 2-3 parts by mass of SiC micro powder and 3-5 parts by mass of additives;
[0010] The particle size of the ZrO2 nano powder is 20-50nm, and the particle size of the ZrO2 micro powder is 0.5-0.1um.
[0011] Furthermore, the outermost layer of the surface structure of the high wear-resistant zirconia ceramic ball is sprayed with a plasma sprayed layer, and the plasma sprayed layer is an Al2O3 coating of 50-100um.
[0012] Furthermore, the surface structure thickness is 100-200um, accounting for 10-15% of the total thickness of the high wear-resistant zirconia ceramic ball; the intermediate structure thickness is 300-500um, accounting for 20-30% of the total thickness of the high wear-resistant zirconia ceramic ball; the core structure thickness is 800-1000um, accounting for 55-70% of the total thickness of the high wear-resistant zirconia ceramic ball.
[0013] Furthermore, for every 100 parts by mass of the high wear-resistant layer, the mass portion of the self-repairing microcapsule material is 3-5 parts.
[0014] Furthermore, for every 100 parts by mass of the high wear-resistant layer, the mass part of the self-repairing microcapsule material is 5 parts.
[0015] The preparation process of high wear-resistant zirconia ceramic balls includes the following preparation steps:
[0016] Step 1: Mix the surface structure, the middle structure and the raw materials of each layer in proportion, wherein the purity of ZrO2, Y2O3 and CeO2 is greater than 99%, and then use a ball mill to wet grind for 24 hours, using ethanol as the solvent and ZrO2 balls as the ball milling medium;
[0017] Step 2: Prepare several different mixture slurries with different composition ratios of zirconium oxide powder for different gradient layers, load the mixture slurry of the core layer into the mold, add the slurry of the middle structure layer layer by layer after preliminary molding, and finally add the slurry of the surface structure layer, perform cold isostatic pressing molding layer by layer, and maintain the pressure at 200-400MPa for 30min;
[0018] Step 3: pre-sinter the pressed sphere at 600-800°C with a heating rate of 2°C / min and keep warm for 2-4h;
[0019] Step 4: Use electric field to assist sintering, heating to 1400-1600°C at a rate of 100°C / min, keeping warm for 2-5h, and the electric field strength is 10-20V / cm;
[0020] Step 5: The surface of the sintered ceramic ball is subjected to high-temperature plasma spraying treatment, and a 50-100um Al2O3 coating is sprayed on the surface of the ceramic ball at a spraying rate of 100mm / min and a spraying temperature of more than 10000℃, and then gradually cooled to room temperature at a rate of 5-10℃ / min;
[0021] Step 6: Post-process the ceramic ball and polish it with diamond paste for 2 hours.
[0022] Furthermore, in step 4, an electric field is used for auxiliary sintering, heating to 1500° C. at a rate of 100° C. / min, and keeping warm for 3 hours, with an electric field strength of 10-20 V / cm.
[0023] Furthermore, in step five, the surface of the sintered ceramic ball is subjected to high-temperature plasma spraying treatment, and a 50-100um Al2O3 coating is sprayed on the surface of the ceramic ball at a spraying rate of 100mm / min and a spraying temperature of more than 10000°C, and then gradually cooled to room temperature at a rate of 7.5°C / min.
[0024] The present invention proposes a highly wear-resistant zirconia ceramic ball. Compared with the prior art:
[0025] Through gradient design, the ceramic ball is divided into surface structure, middle structure and core structure, and the material composition and performance indicators of each layer are different. The surface structure adopts nano zirconium oxide material with high hardness and high wear resistance, and increases the addition of yttrium stabilizer and cerium oxide to improve the hardness and wear resistance of the surface. The middle structure and core structure adopt micron zirconium oxide material with medium hardness and toughness, and increase yttrium stabilizer and cerium oxide to balance strength and toughness, and improve overall toughness and crack resistance.
[0026] By optimizing the sintering temperature, time and heating and cooling rates, the density and grain size of each layer of material are optimally controlled, significantly reducing internal stress and cracks.
[0027] At the same time, self-healing microcapsules are introduced in the preparation of ceramic balls. When microcracks appear on the surface of the ceramic balls, the microcapsules rupture and release repair agents to repair the cracks in time. The self-healing function significantly improves the service life and reliability of the ceramic balls. DETAILED DESCRIPTION
[0028] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0029] A highly wear-resistant zirconia ceramic ball comprises a surface structure composed of a highly wear-resistant layer, an intermediate structure composed of a gradient transition layer and a core structure composed of a reinforced core layer.
[0030] Every 100 parts by mass of the high wear-resistant layer components include: 85-90 parts by mass of ZrO2 nanopowder, 4-5 parts by mass of Y2O3 stabilizer, 1-3 parts by mass of CeO2 stabilizer, 0.5-1.5 parts by mass of carbon nanotubes, 1-10 parts by mass of self-repairing materials and 3-5 parts by mass of additives. The specific ingredients are as follows:
[0031]
[0032] Every 100 parts by mass of the gradient transition layer comprises: 85-92 parts by mass of ZrO2 micron powder, 4-5 parts by mass of Y2O3 stabilizer, 1-2 parts by mass of CeO2 stabilizer, 1-10 parts by mass of self-repairing microcapsule material, 1 part by mass of nano-silicate microspheres and 3-5 parts by mass of additives; the ZrO2 content of the gradient transition layer changes gradually in a gradient form, the ZrO2 content of the surface layer is the same as that of the high wear-resistant layer material, and the ZrO2 content of the core part is the same as that of the enhanced core layer ZrO2, and the specific composition is as follows;
[0033] Intermediate structural materials
[0034] Material purity Particle size / tube diameter (um) Specific surface area (m2 / g)
[0035] Zirconia>99.5% 0.5-1 2-5
[0036] Yttrium oxide>99.9% 50-100 5-10
[0037] Cerium oxide>99.9% 50-100 5-10
[0038] Silicate microspheres>99% 0.05-0.2 -
[0039] Additives>99% Nano-grade
[0040] Every 100 parts by mass of the reinforced core layer component includes: 88-92 parts by mass of ZrO2 micron powder, 4-5 parts by mass of Y2O3 stabilizer, 1-2 parts by mass of CeO2 stabilizer, 2-3 parts by mass of SiC micro powder and 3-5 parts by mass of additives, and the specific ingredients are as follows;
[0041]
[0042] In the present application, Y2O3 and CeO2 are used as stabilizers. Adding yttrium oxide to zirconia can stabilize its tetragonal phase structure and prevent it from transforming into a monoclinic phase at room temperature. This stable tetragonal phase has high strength and toughness. Furthermore, by stabilizing the tetragonal phase, the fracture toughness and flexural strength of zirconia ceramics can be significantly improved. Cerium oxide has good oxidation stability, which can improve the oxidation resistance of zirconia ceramics in high temperature environments, maintain the stability of zirconia at higher temperatures, and improve the toughness and wear resistance of the material.
[0043] The outermost layer of the surface structure of the high wear-resistant zirconia ceramic ball is sprayed with Al2O3 plasma spray layer, which can further increase the wear resistance of the ceramic ball.
[0044] In the present application, the thickness of the surface structure is 100-200um, accounting for 10-15% of the total thickness of the high wear-resistant zirconia ceramic ball; the thickness of the intermediate structure is 300-500um, accounting for 20-30% of the total thickness of the high wear-resistant zirconia ceramic ball; the thickness of the core structure is 800-1000um, accounting for 55-70% of the total thickness of the high wear-resistant zirconia ceramic ball.
[0045] The surface structure is the part that is most directly in contact with the external interface. The surface mainly bears friction and wear. Therefore, the selection of high-hardness materials such as nano-scale zirconium oxide powder, yttrium oxide and cerium oxide, as well as nano-carbon tubes or graphene can significantly improve the hardness and wear resistance of the surface. The introduction of self-healing microcapsule materials can automatically repair microcracks when they appear on the surface, further improving the durability of the material.
[0046] In the present application, the self-repairing microcapsule material is a polymer composite material composed of polyurethane and urea-formaldehyde resin, with polyurethane as the core material and urea-formaldehyde resin as the shell material. During the use of the ceramic ball, microcracks may be generated on the surface or inside of the ceramic ball due to external force or fatigue. When the microcracks expand, they encounter the self-repairing microcapsules embedded in the ceramic matrix, causing the microcapsules to rupture. After the microcapsules rupture, the internal repair agent flows out and fills the cracks. Since the surface of the ceramic ball usually has a microporous structure, the repair agent can fully penetrate into the cracks, and the repair agent solidifies in the cracks to form a solid filler, thereby restoring the integrity and mechanical properties of the material.
[0047] The preparation process of self-healing microcapsules is as follows:
[0048] Step 1: Preparation of core materials: prepare 100 parts by mass of Epon 828, 10 parts by mass of curing agent and 2 parts by mass of silane coupling agent raw materials; weigh 100 parts by mass of Epon 828 epoxy resin, add 10 parts by mass of DMP-30 curing agent, stir evenly, add 2 parts by mass of silane coupling agent, and continue stirring until completely mixed;
[0049] Step 2: Preparation of core materials: prepare 5 parts by mass of urea, 10 parts by mass of 37% formaldehyde solution, 70 parts by mass of deionized water raw material and 2 parts by mass of polyvinyl alcohol; add 50 parts by mass of deionized water and 5 parts by mass of urea to a mixing container, stir to dissolve, add 10 parts by mass of formaldehyde solution, continue stirring, in another mixing container, add 2 parts by mass of PVA to 20 parts by mass of deionized water, stir and heat until completely dissolved, slowly add the PVA solution to the urea-formaldehyde solution, and stir evenly;
[0050] Step 3: preparing microcapsules by in-situ polymerization;
[0051] Slowly add the repair agent core material to the shell material solution, and stir with a high-speed stirrer to form an emulsion. The stirring speed is controlled at 1000rpm, and the stirring time is 30min to ensure the formation of a uniform emulsion. Heat the emulsion to 55°C, and slowly add a small amount of hydrochloric acid or sulfuric acid under continuous stirring to adjust the pH value of the solution to 2-3. React for 2h to ensure that the urea-formaldehyde resin forms a uniform shell on the surface of the repair agent core material;
[0052] After the reaction, the reaction system was cooled to room temperature, and the microcapsules were separated using a centrifuge at a speed of 3000 rpm for 10 min, and washed three times with deionized water to remove residual reactants and solvents;
[0053] The washed microcapsules were placed in an oven and dried at 60°C for 12 h. After drying, they were sieved using a sieve to obtain self-healing microcapsules.
[0054] By adding self-repairing microcapsules into ceramic balls, the self-repairing microcapsules can continuously repair microcracks during the use of the ceramic balls, thereby extending the service life of the material. In actual applications, the self-repairing function of the ceramic balls reduces the frequency of replacement and maintenance, reduces maintenance costs, and reduces the risks caused by material failure.
[0055] According to the ceramic ball preparation scheme of this application, the self-healing microcapsules were mixed into the ceramic ball samples according to different addition ratios, and the following tests were performed:
[0056] Wear resistance test: The sintered ceramic balls were subjected to friction tests, and the wear volume and wear rate of each group of samples were recorded;
[0057] Mechanical properties test: Conduct a three-point bending test and record the bending strength of each group of samples;
[0058] Self-healing ability test: Artificially generate micro cracks on the surface of the ceramic ball, heat it to the curing temperature of the repair agent, and observe the repair of the cracks.
[0059] ① According to ISO 6339-2:1987, the wear resistance test method of ceramic materials, the friction tester load is 20N, the speed is 200pmp, and the test time is 60min. The test results are as follows:
[0060]
[0061] The above test results show that the addition of self-repairing microcapsules can significantly improve the wear resistance of ceramic balls, and the optimal addition ratio is 3-5wt%.
[0062] ② According to ISO 6872:2015, physical and chemical properties of dental ceramics were tested using a three-point bending tester with a loading speed of 0.5 mm / min and the bending strength was recorded. The results are as follows:
[0063]
[0064] The addition of self-healing microcapsules has a certain effect on the mechanical properties. The appropriate amount of addition can improve wear resistance while maintaining high mechanical properties. Among them, the sample without microcapsules has the highest bending strength. After adding microcapsules, the bending strength gradually decreases, especially when the addition ratio reaches 10wt%, the strength decreases significantly. The appropriate amount of microcapsules (1-5wt%) has little effect on the strength, but 10wt% significantly affects the mechanical properties of the material.
[0065] ③ According to ASTM E1820-21, the crack opening displacement measurement method was used for measurement. The test results are as follows:
[0066]
[0067] The addition of self-healing microcapsules significantly improves the wear resistance and self-healing ability of high wear-resistant zirconia ceramic balls. 3-5wt% of microcapsules can provide optimal wear resistance and self-healing ability while maintaining high mechanical properties. Although too many microcapsules have significant repair effects, they will lead to uneven material structure and reduce mechanical properties.
[0068] Through the prediction and analysis of the test results, the following conclusions can be drawn: the introduction of self-healing microcapsules significantly improves the wear resistance and self-healing ability of zirconia ceramic balls. The appropriate addition of capsules provides optimal wear resistance and self-healing ability while maintaining high mechanical properties.
[0069] Taking wear resistance, mechanical properties and self-repairing ability into consideration, the optimal addition ratio is 5wt%, which can achieve a balance in all aspects and provide excellent comprehensive performance.
[0070] The preparation process of high wear-resistant zirconia ceramic balls includes the following preparation steps:
[0071] Step 1: Mix the surface structure, the middle structure and the raw materials of each layer in proportion, and then use a ball mill to wet grind for 24 hours. The solvent used is ethanol and the ball milling medium is ZrO2 ball. It should be noted that the particle size distribution during the grinding process needs to be checked regularly to ensure that a uniform particle distribution of nanometer or micrometer level is achieved.
[0072] Step 2: Prepare several different mixture slurries with different composition ratios of zirconium oxide powder for different gradient layers, load the mixture slurry of the innermost layer (core layer) into the mold, and after preliminary molding, add the slurry of the middle structure layer layer by layer, and finally add the slurry of the surface structure, and perform cold isostatic pressing layer by layer, and maintain the pressure at 200-400MPa for 30min;
[0073] Step 3: pre-sinter the pressed sphere at 600-800°C with a heating rate of 2°C / min and keep warm for 2-4h;
[0074] Step 4: Use electric field to assist sintering, heating to 1400-1600°C at a rate of 100°C / min, keeping warm for 2-5h, and the electric field strength is 10-20V / cm;
[0075] Step 5: The surface of the sintered ceramic ball is subjected to high-temperature plasma spraying treatment, and a 50-100um Al2O3 coating is sprayed on the surface of the ceramic ball at a spraying rate of 100mm / min and a spraying temperature of more than 10000℃, and then gradually cooled to room temperature at a rate of 5-10℃ / min;
[0076] Step 6: Post-process the ceramic ball and polish it with diamond paste for 2 hours.
[0077] In this application, the sintering process is the key point that needs to be controlled. The temperature and time will directly affect the porosity and mechanical properties of the ceramic ball. Multiple sintering groups are set up to explore the temperature control during the sintering process.
[0078] Set three groups of 1400℃, 1500℃, and 1600℃, marked as A, B, and C respectively. The specific parameter settings are as follows:
[0079]
[0080] The test results are as follows:
[0081]
[0082]
[0083] Based on the above analysis, the best sintering conditions are sintering temperature of 1500℃, sintering time of 3 hours, and heating and cooling rate of 7.5℃ / min. These conditions can obtain high wear-resistant zirconia ceramic balls with high density, low porosity, good mechanical properties and wear resistance.
[0084] The above-mentioned specific implementations are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can make many forms without departing from the scope of protection of the present invention and the claims, all of which are protected by the present invention.
Claims
1. A highly wear-resistant zirconia ceramic ball, characterized in that: The highly wear-resistant zirconia ceramic ball comprises a surface structure consisting of a highly wear-resistant layer, an intermediate structure consisting of a gradient transition layer, and a core structure consisting of a reinforced core layer; Every 100 parts by mass of the high wear-resistant layer components include: 85-90 parts by mass of ZrO2 nanopowder, 4-5 parts by mass of Y2O3 stabilizer, 1-3 parts by mass of CeO2 stabilizer, 0.5-1.5 parts by mass of carbon nanotubes, 1-10 parts by mass of self-repairing microcapsule material and 3-5 parts by mass of additives; Every 100 parts by weight of the gradient transition layer comprises: 85-92 parts by weight of ZrO2 micron powder, 4-5 parts by weight of Y2O3 stabilizer, 1-2 parts by weight of CeO2 stabilizer, 1-10 parts by weight of self-repairing microcapsule material, 1 part by weight of nano-silicate microspheres and 3-4 parts by weight of additives; the ZrO2 content of the gradient transition layer changes gradually in a gradient form, the ZrO2 content of the surface layer is the same as that of the high wear-resistant layer material, and the ZrO2 content of the core part is the same as that of the enhanced core layer; Every 100 parts by mass of the reinforced core layer components include: 88-92 parts by mass of ZrO2 micron powder, 4-5 parts by mass of Y2O3 stabilizer, 1-2 parts by mass of CeO2 stabilizer, 2-3 parts by mass of SiC micro powder and 3-5 parts by mass of additives; The particle size of the ZrO2 nano powder is 20-50nm, and the particle size of the ZrO2 micro powder is 0.5-0.1um.
2. The high wear-resistant zirconia ceramic ball according to claim 1, characterized in that: The outermost layer of the surface structure of the high wear-resistant zirconia ceramic ball is sprayed with a plasma sprayed layer, and the plasma sprayed layer is an Al2O3 coating of 50-100 um.
3. The high wear-resistant zirconia ceramic ball according to claim 1, characterized in that: The surface structure thickness is 100-200um, accounting for 10-15% of the total thickness of the high wear-resistant zirconia ceramic ball; the intermediate structure thickness is 300-500um, accounting for 20-30% of the total thickness of the high wear-resistant zirconia ceramic ball; the core structure thickness is 800-1000um, accounting for 55-70% of the total thickness of the high wear-resistant zirconia ceramic ball.
4. The high wear-resistant zirconia ceramic ball according to claim 1, characterized in that: For every 100 parts by mass of the high wear-resistant layer, the mass portion of the self-repairing microcapsule material is 3-5 parts by mass.
5. The highly wear-resistant zirconia ceramic ball according to claim 1, characterized in that: For every 100 parts by mass of the high wear-resistant layer, the mass portion of the self-repairing microcapsule material is 5 parts by mass.
6. The process for preparing a highly wear-resistant zirconia ceramic ball according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: Step 1: Mix the surface structure, the middle structure and the raw materials of each layer in proportion, wherein the purity of ZrO2, Y2O3 and CeO2 is greater than 99%, and then use a ball mill to wet grind for 24 hours, using ethanol as the solvent and ZrO2 balls as the ball milling medium; Step 2: Prepare several different mixture slurries with different composition ratios of zirconium oxide powder for different gradient layers, load the mixture slurry of the core layer into the mold, add the slurry of the middle structure layer layer by layer after preliminary molding, and finally add the slurry of the surface structure layer, perform cold isostatic pressing molding layer by layer, and maintain the pressure at 200-400MPa for 30min; Step 3: pre-sinter the pressed sphere at 600-800°C with a heating rate of 2°C / min and keep warm for 2-4h; Step 4: Use electric field to assist sintering, heating to 1400-1600°C at a rate of 100°C / min, keeping warm for 2-5h, and the electric field strength is 10-20V / cm; Step 5: The surface of the sintered ceramic ball is subjected to high-temperature plasma spraying treatment, and a 50-100um Al2O3 coating is sprayed on the surface of the ceramic ball at a spraying rate of 100mm / min and a spraying temperature of more than 10000℃, and then gradually cooled to room temperature at a rate of 5-10℃ / min; Step 6: Post-process the ceramic ball and polish it with diamond paste for 2 hours.
7. The preparation process of the highly wear-resistant zirconia ceramic ball according to claim 6, characterized in that: In step 4, an electric field is used for auxiliary sintering, heating to 1500° C. at a rate of 100° C. / min, and keeping warm for 3 hours, with an electric field strength of 10-20 V / cm.
8. The process for preparing a highly wear-resistant zirconia ceramic ball according to claim 6, characterized in that: In step five, the surface of the sintered ceramic ball is subjected to high-temperature plasma spraying treatment. A 50-100um Al2O3 coating is sprayed on the surface of the ceramic ball at a spraying rate of 100mm / min and a spraying temperature of more than 10000°C, and then gradually cooled to room temperature at a rate of 7.5°C / min.
Citation Information
Patent Citations
Self-healing epoxy powdery coating containing microcapsule and preparation method thereof
CN105038502A
Self-repairing artificial quartz stone and preparation method thereof
CN110627413A
Wear-resistant zirconium-aluminum composite ceramic ball with gradient structure and preparation method thereof
CN116768607A
Preparation method of double microcapsules for self-repairing freeze-thaw damage of concrete
CN117645430A
Nanocomposite microcapsules for self-healing of composite articles
US20170100902A1
Cited By
Ceramic embolism coating, preparation method thereof, ceramic embolism and application
CN120841987A
High-performance zirconia ceramic particle and preparation method thereof
CN122562504A