Method for synchronously improving mechanical and optical characteristics of reactive sintering silicon carbide through laser irradiation

By irradiating the RB-SiC surface with nanosecond laser in a nitrogen environment, micro-nano structures and silicon-based nitrides are formed, which solves the problem of failing to simultaneously improve the surface hardness and reduce the reflectivity of RB-SiC in the existing technology, and achieve Significant improvement in mechanical and optical properties.

CN118771908AActive Publication Date: 2024-10-15JILIN UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410850027.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-15
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing technology fails to achieve both hardness improvement and reflectivity reduction on the surface of reaction-bonded silicon carbide (RB-SiC), which limits its wide application in the optical field.

Method used

Nanosecond lasers with different laser parameters are used to irradiate the RB-SiC surface in a nitrogen environment to form a surface with different micro-nano structures and silicon-based nitrides. By regulating the silicon-based nitride content and micromorphology, the surface hardness is improved. and reduce reflectivity.

Benefits of technology

The surface hardness of RB-SiC can be increased by up to 44.6% and the reflectivity reduced by 95.2%. By changing the laser irradiation parameters to control the silicon-based nitride content and surface morphology, the hardness can be increased and the reflectivity can be reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771908A_ABST
    Figure CN118771908A_ABST
Patent Text Reader

Abstract

The invention relates to a method for synchronously improving mechanical and optical characteristics of reactive sintering silicon carbide through laser irradiation, and belongs to the technical field of ceramic material surface modification. The method comprises the following steps: cleaning, grinding, polishing and drying the surface of RB-SiC; and performing nanosecond laser irradiation on the RB-SiC surface in a nitrogen atmosphere to obtain surfaces with different micro-nano structures and silicon-based nitride contents. By regulating and controlling the content of the silicon-based nitride, the surface hardness of the RB-SiC can be improved, and the maximum amplification can reach 44.6%. In addition, due to the formation of the silicon-based nitride with the high refractive index and the unique micro-nano structure, the reflectivity of the RB-SiC surface is reduced to 1% from 20.8% or above within the wavelength range of 200-2500nm, and is reduced by 95.2% compared with that of the original surface. The method has the advantages of simplicity in operation, high efficiency, low cost and the like. By utilizing the method, the surface hardness of the RB-SiC can be improved and the reflectivity can be reduced at the same time, so that the practical application of the RB-SiC as a surface functional material can be widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for synchronously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation, belonging to the technical field of surface modification of ceramic materials. The present invention can simultaneously improve the surface hardness of RB-SiC and reduce the reflectivity, which is convenient for broadening its practical application as a surface functional material. Background Art

[0002] Reaction-bonded silicon carbide (RB-SiC) is a promising semiconductor material consisting of hard silicon carbide particles and a brittle silicon matrix. It has been widely used in various mechanical devices due to its excellent chemical corrosion resistance, outstanding wear resistance and high stiffness. In addition, RB-SiC also has excellent optoelectronic properties, excellent oxidation resistance and outstanding thermal stability, which make it have potential application prospects in the optical field, such as solar cells and ultraviolet optoelectronic devices. However, the relatively low photoelectric conversion efficiency hinders its widespread application in the optical field. In addition, RB-SiC will inevitably wear and damage during actual use. In order to improve its practical applicability, it is necessary to further improve its surface hardness.

[0003] Studies have shown that preparing micro-nano structures on the surface of materials can significantly reduce the reflectivity of the material surface, which is beneficial to improving the photoelectric conversion efficiency. For example, in 2013 "Solar Energy Materials And Solar Cells" Volume 108 93-97 (Fabrication of micro-nano surface texture by CsCl lithography with antireflection and photoelectronic properties for solar cells), Liu et al. prepared pyramidal structures and nanocolumn array structures on the silicon surface by combining self-assembly lithography and dry etching, which reduced the reflectivity of the silicon surface from more than 35% to less than 5% in the wavelength range of 400-1000nm, thereby improving its photoelectric conversion efficiency. In addition, laser nitridation has been widely used to improve the hardness of material surfaces. For example, in 2019 "Optics & Laser Technology" Vol. 116, 305-314 (Effect of laser-assisted nitriding with a high-power diode laser on surface hardening of aluminum-containing martensitic steel), Ahjin Sim et al. prepared a plate-like micro-nanostructure mainly composed of aluminum-based nitride (AlN) on the surface of AISIP21 by continuous laser ablation in a nitrogen environment, which increased the surface hardness by about 40%. Therefore, laser irradiation in a nitrogen environment is an effective method to simultaneously improve the surface hardness and construct micro-nanostructures. However, to date, there has been no report on the simultaneous improvement of the surface hardness and reduction of the reflectivity of RB-SiC using this method. Therefore, it is necessary to develop a method for synchronously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for synchronously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation. The method uses nanosecond lasers with different laser parameters to irradiate the surface of RB-SiC to obtain surfaces with different micro-nano structures and silicon-based nitride contents. By regulating the content of silicon-based nitrides, the surface hardness of RB-SiC can be improved, with a maximum increase of 44.6%. In addition, the formation of a large amount of silicon-based nitrides with high refractive index and unique micro-nano structures reduces the reflectivity of the RB-SiC surface from more than 20.8% to 1% in the wavelength range of 200-2500nm, which is a 95.2% reduction compared to the original surface.

[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:

[0006] The method for simultaneously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation specifically comprises the following steps:

[0007] (1) The RB-SiC surface was ultrasonically cleaned for 30 min, and then the cleaned surface was mechanically ground and polished to obtain a mirror surface. Finally, it was wiped with alcohol and left to stand at room temperature for 5 min to obtain a clean and dry RB-SiC surface.

[0008] (2) In a nitrogen environment, the RB-SiC surface was irradiated with nanosecond lasers using different laser parameters to obtain surfaces with different micro-nano structures and different silicon-based nitride contents; the micro-nano structures were recast by the molten material in the molten pool under the combined effects of recoil pressure, plasma effect and Marangoni effect; the formation of the silicon-based nitride can be attributed to the chemical reaction between molten Si or Si vapor and nitrogen; regulating the silicon-based nitride content can increase the surface hardness of RB-SiC, with a maximum increase of 44.6%. In addition, the formation of silicon-based nitrides with high refractive index and unique micro-nano structures reduces the reflectivity of the RB-SiC surface from more than 20.8% to 1% in the wavelength range of 200-2500nm, which is a 95.2% reduction compared to the original surface.

[0009] Furthermore, the surface roughness of the RB-SiC after the mechanical polishing treatment in step (1) is less than 100 nm.

[0010] Furthermore, the laser irradiation parameters described in step (2) include: laser wavelength of 1064nm, frequency of 700kHz, pulse width of 7ns, and laser energy distribution of Gaussian distribution.

[0011] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0012] Nanosecond laser irradiation is performed on the surface of RB-SiC in a nitrogen atmosphere to introduce micro-nano structures and silicon-based nitrides. During the preparation process, the content of silicon-based nitrides and the surface micromorphology can be controlled by changing the laser irradiation parameters, thereby simultaneously achieving an increase in the surface hardness and a decrease in the reflectivity of RB-SiC. The surface hardness of laser-irradiated RB-SiC can be increased by 44.6% compared to the original surface, and its surface reflectivity can be reduced by 95.2% compared to the original surface. In addition, the preparation method of the present invention has the advantages of simple operation, high efficiency, and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The drawings described herein are used to provide further understanding of the present invention and constitute a part of this application. The illustrative examples of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0014] Figure 1 It is a schematic diagram of the nanosecond laser processing system of the present invention.

[0015] Figure 2 The average hardness value and light reflectivity of the surface after nanosecond laser irradiation with a laser power of 7.6 / 14.7 / 22.0 W under a nitrogen atmosphere of the present invention and the original surface.

[0016] Figure 3 The results are Fourier transform infrared spectroscopy (FTIR) test results of the surface after nanosecond laser irradiation with a laser power of 14.7 / 22.0 W and the original surface in a nitrogen atmosphere of the present invention.

[0017] Figure 4 The SEM morphology, three-dimensional morphology and cross-sectional profile curve of the surface after nanosecond laser irradiation with a laser power of 7.6 / 14.7 / 22.0 W in a nitrogen atmosphere of the present invention. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0019] The method of the present invention for synchronously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation specifically comprises the following steps:

[0020] (1) The RB-SiC surface was ultrasonically cleaned for 30 min, and then the cleaned surface was mechanically ground and polished to obtain a mirror surface. Finally, it was wiped with alcohol and left to stand at room temperature for 5 min to obtain a clean and dry RB-SiC surface.

[0021] (2) In a nitrogen environment, the RB-SiC surface was irradiated with nanosecond lasers using different laser parameters to obtain surfaces with different micro-nano structures and different silicon-based nitride contents; the micro-nano structures were recast by the molten material in the molten pool under the combined effects of recoil pressure, plasma effect and Marangoni effect; the formation of the silicon-based nitride can be attributed to the chemical reaction between molten Si or Si vapor and nitrogen; regulating the silicon-based nitride content can increase the surface hardness of RB-SiC, with a maximum increase of 44.6%. In addition, the formation of silicon-based nitrides with high refractive index and unique micro-nano structures reduces the reflectivity of the RB-SiC surface from more than 20.8% to 1% in the wavelength range of 200-2500nm, which is a 95.2% reduction compared to the original surface.

[0022] Furthermore, the surface roughness of the RB-SiC after the mechanical polishing treatment in step (1) is less than 100 nm.

[0023] Furthermore, the laser irradiation parameters described in step (2) include: laser wavelength of 1064nm, frequency of 700kHz, pulse width of 7ns, and laser energy distribution of Gaussian distribution.

[0024] Embodiment 1:

[0025] A RB-SiC sample with a thickness of 1 mm was selected, and its surface was irradiated with nanosecond lasers with different laser parameters. The implementation process and beneficial effects of the present invention are further compared and explained in conjunction with the following examples.

[0026] Figure 2 The results show that the RB-SiC surface was laser irradiated under the conditions of laser scanning speed of 10 mm / s, repetition frequency of 700 kHz, pulse width of 7 ns, and laser power of 7.6 / 14.7 / 22.0 W, and the average hardness value obtained after 10 nanoindentation tests on the laser irradiated surface and the light reflectivity of the above surface in the wavelength range of 200-2500 nm. It can be seen that when the indentation load is 150 mN, as the laser power increases from 7.6 W to 22.0 W, the average hardness value of the laser irradiated surface decreases from 29.90 GPa to 22.26 GPa, but they are all higher than the average hardness value of the original surface (20.11 GPa), with an increase of 10.6-44.6%. This shows that the surface hardness of the RB-SiC surface can be greatly improved by regulating the laser power for laser nitriding. In addition, the original surface reflectivity is above 20.8%. As the laser power gradually increases to 22.0W, the laser irradiated surface reflectivity gradually decreases to about 1%, that is, the laser irradiated surface reflectivity is reduced by 95.2% compared with the original surface. Combining the above results, it can be obtained that laser nitriding can simultaneously improve the surface hardness of RB-SiC and reduce the surface reflectivity of RB-SiC.

[0027] Figure 3 The Fourier transform infrared spectroscopy (FTIR) test results of the surface obtained after laser irradiation of the RB-SiC surface and the original surface under the conditions of laser scanning speed of 10mm / s, repetition frequency of 700kHz, pulse width of 7ns, and laser power of 14.7 / 22.0W are shown. It can be seen that with the increase of laser power, the Si-N intensity detected on the laser irradiated surface increases, indicating that more silicon-based nitrides are introduced into the laser irradiated surface under nitrogen atmosphere. Since the hardness of silicon-based nitrides is higher than that of silicon matrix and its refractive index is higher, this is also the reason for the increase in hardness and decrease in reflectivity of the laser irradiated surface.

[0028] Figure 4The SEM morphology, three-dimensional morphology and cross-sectional profile curves of the RB-SiC surface obtained after laser irradiation under the conditions of laser scanning speed of 10 mm / s, repetition frequency of 700 kHz, pulse width of 7 ns and laser power of 7.6 / 14.7 / 22.0 W are shown. It can be seen that laser irradiation in nitrogen atmosphere induces dendritic structure, micro-cone structure and mesh structure on the RB-SiC surface. These micro-nano structures can prevent the incident light beam from overflowing, thereby causing more light beams to dissipate inside the micro-nano structure, which is also an important reason for the decrease in reflectivity of the laser irradiated surface.

[0029] From the example results, it can be seen that based on the method proposed by the present invention for synchronously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation, RB-SiC is irradiated with nanosecond pulse laser in a nitrogen atmosphere, and micro-nano structures and silicon-based nitrides are introduced on the laser irradiated surface, which can simultaneously improve its surface hardness and reduce its reflectivity. This method is suitable for synchronously improving the mechanical and optical properties of RB-SiC samples of different sizes and shapes, thereby enhancing its applicability.

[0030] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, various modifications and changes may be made without departing from the spirit and scope of the present invention. Any modification, equivalent substitution and improvement of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for simultaneously improving the mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation, characterized in that: The method comprises irradiating reactive sintered silicon carbide (RB-SiC) with nanosecond pulse laser in a nitrogen atmosphere, introducing micro-nano structures and silicon-based nitrides, inducing the formation of different types of micro-nano structures and regulating the content of silicon-based nitrides by changing laser irradiation parameters, and further regulating the surface hardness and reflectivity of RB-SiC. The specific steps include: (1) The RB-SiC surface was ultrasonically cleaned for 30 min, and then the cleaned surface was mechanically ground and polished to obtain a mirror surface. Finally, it was wiped with alcohol and left to stand at room temperature for 5 min to obtain a clean and dry RB-SiC surface. (2) In a nitrogen environment, the RB-SiC surface is irradiated with nanosecond laser with different laser parameters to obtain surfaces with different micro-nano structures and different silicon-based nitride contents; the micro-nano structures are recast by the molten material in the molten pool under the combined action of recoil pressure, plasma effect and Marangoni effect; the formation of the silicon-based nitride can be attributed to the chemical reaction between molten Si or Si vapor and nitrogen; the surface hardness of RB-SiC can be improved by regulating the content of silicon-based nitride, with the maximum increase reaching 44.6%; in addition, the formation of silicon-based nitride with high refractive index and unique micro-nano structure reduces the reflectivity of the RB-SiC surface from more than 20.8% to 1% in the wavelength range of 200-2500nm, which is a decrease of 95.2% compared with the original surface.

2. The method of claim 1, wherein: In step 1, the surface roughness of the RB-SiC after the mechanical polishing treatment is less than 100 nm.

3. The method of claim 1 for simultaneously improving mechanical and optical properties of reaction-sintered silicon carbide by laser irradiation, characterized in that: In step 2, the laser irradiation parameters include: laser wavelength is 1064nm, frequency is 700kHz, pulse width is 7ns, and laser energy distribution is Gaussian distribution.

Citation Information

Patent Citations

  • Preparation method for silicon surface anti-reflection nanometer array structure

    CN102351569A

  • Method for preparing reflection increasing film based on laser processing reaction sintering silicon carbide

    CN116143548A

  • Process for surface hardening metallic components e.g. molding tool comprises micro-texturing the components in points or lines in the surface region to be hardened using a laser beam

    DE10059802A1

  • Systems and Methods of Laser Texturing of Material Surfaces and their Applications

    US20100143744A1

  • Laser ablation method for treating a zirconia containing ceramic surface

    US20170137329A1