Butylbenzene block polymer as well as preparation method and application thereof
By shortening the butadiene block segment and introducing a butadiene and styrene copolymer, the problem of balancing mechanical properties, bending flexibility and transparency of the butadiene block polymer was solved, and high-performance optical materials were realized precursor.
Patent Information
- Application Number
- CN202310362287.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-06
AI Technical Summary
It is difficult to balance the mechanical properties, bending flexibility and transparency of existing butyl-styrene block polymers, especially after high temperature, the strength decreases and the optical loss increases.
By shortening the length of a single butadiene block molecular segment and introducing a certain proportion of butadiene and styrene copolymer into the molecular segment, a butadiene-butadiene block polymer with a specific structure is prepared. The specific steps include multiple polymerizations. React to control the ratio and block distribution of styrene and butadiene.
It has been achieved that while maintaining excellent transparency, the butadiene-styrene block polymer can significantly improve the mechanical properties and bending flexibility, comprehensively improving the performance of the product.
Smart Images

Figure BDA0004166145940000111 
Figure BDA0004166145940000121 
Figure BDA0004166145940000122
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material synthesis and preparation, and in particular to a styrene-butadiene block polymer and a preparation method and application thereof. Background Art
[0002] Plastic optical materials require polymer materials to have excellent transparency and low optical loss, good thermal stability and bending flexibility. Polymethyl methacrylate (PMMA) has excellent optical properties, but PMMA has strong water absorption, and its strength decreases when the temperature is higher than 85°C, and its optical loss also increases significantly.
[0003] Styrene-butadiene-styrene fully (or substantially fully) hydrogenated hard block polymers are widely used in films, profiles, sheets and pultruded products, and are also excellent optical materials. The relative content of butadiene and styrene in the polymer before hydrogenation has a significant impact on product performance. When the butadiene content is low, the polybutadiene block molecular chain segment is short, and the bending flexibility of the end product is poor; when the butadiene content is high, the polybutadiene block molecular chain segment is long, and the overly regular polybutadiene molecular chain segment will cause the hydrogenated product to have a tendency to crystallize, and the optical properties of the end product are poor.
[0004] Therefore, there is an urgent need to develop a butadiene-styrene block copolymer that can be used as a precursor for high-end optical materials while having excellent transparency and significantly improved mechanical strength and bending flexibility. Summary of the invention
[0005] The purpose of the present invention is to overcome the problem that the mechanical properties, bending flexibility and transparency of butadiene block polymers in the prior art cannot be taken into account at the same time, and to provide a butadiene block polymer and a preparation method and application thereof. The butadiene block polymer has a specific structure. Specifically, by shortening the length of a single butadiene block molecular segment and introducing a certain proportion of butadiene and styrene copolymers into the molecular segment, the butadiene block polymer has improved transparency while having significantly improved mechanical properties and bending flexibility.
[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a block butadiene styrene block polymer, characterized in that the polymer has a structure shown as S1-B1-(BS)1-S2-B2-S3;
[0007] Among them, S1, S2, and S3 are polystyrene blocks, B1 and B2 are polybutadiene blocks, and (BS)1 is a butadiene styrene copolymer;
[0008] Based on the total weight of the polymer, the ratio of the total weight of the styrene chain segments to the total weight of the butadiene chain segments is 2.3-9:1.
[0009] A second aspect of the present invention provides a method for preparing a block butadiene styrene block polymer, characterized in that the preparation method comprises the following steps:
[0010] (1) in a solvent, in the presence of an initiator and a regulator, styrene I undergoes a first polymerization reaction to obtain a first polymer solution containing a polystyrene block S1;
[0011] (2) contacting butadiene I and styrene II with the first polymer solution to carry out a second polymerization reaction to obtain a second polymer solution containing S1-B1-(BS)1-S2;
[0012] (3) contacting butadiene II with the second polymer solution to perform a third polymerization reaction to obtain a third polymer solution comprising S1-B1-(BS)1-S2-B2;
[0013] (4) contacting styrene III with the third polymer solution to carry out a fourth polymerization reaction to obtain a fourth polymer solution comprising S1-B1-(BS)1-S2-B2-S3;
[0014] (5) Adding a terminator to the fourth polymer solution to obtain the butadiene-styrene block polymer.
[0015] The third aspect of the present invention provides a butadiene styrene block polymer prepared by the above preparation method.
[0016] A fourth aspect of the present invention provides a use of the above-mentioned butadiene-styrene block polymer in the preparation of an optical material precursor.
[0017] Through the above technical scheme, the styrene-butadiene block polymer provided by the present invention and its preparation method and application obtain the following beneficial effects:
[0018] The butadiene-styrene block polymer provided by the present invention has a specific structure. Specifically, by shortening the length of a single butadiene block molecular segment and introducing a certain proportion of butadiene and styrene copolymers into the molecular segment, the butadiene-styrene block polymer has improved transparency while having excellent mechanical properties and bending flexibility, thereby achieving comprehensive improvement in the mechanical properties, bending flexibility and transparency of the butadiene-styrene block polymer.
[0019] The preparation method of the styrene-butadiene block polymer provided by the invention reduces the feeding process of the multi-block polymer, is simple to operate, and the monomer sequence distribution of the block polymer is controllable. DETAILED DESCRIPTION
[0020] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0021] The first aspect of the present invention provides a butadiene-styrene block polymer, characterized in that the polymer has a structure as shown in S1-B1-(BS)1-S2-B2-S3;
[0022] Among them, S1, S2, and S3 are polystyrene blocks, B1 and B2 are polybutadiene blocks, and (BS)1 is a butadiene-styrene copolymer;
[0023] Based on the total weight of the polymer, the ratio of the total weight of the styrene chain segments to the total weight of the butadiene chain segments is 2.3-9:1.
[0024] In the present invention, the butadiene-styrene block polymer having the above-mentioned specific structure, specifically, introduces a segment structure of butadiene and styrene copolymer into the molecular chain of the polymer, so that the butadiene-styrene block polymer has improved transparency while having excellent mechanical properties and bending flexibility, thereby achieving a comprehensive improvement in the mechanical properties, bending flexibility and transparency of the butadiene-styrene block polymer.
[0025] In the present invention, the butadiene block polymer is a S1-B1-(BS)1-S2-B2-S3 block polymer, wherein S1, S2, and S3 are polystyrene blocks, S1, S2, and S3 are the same or different, B1 and B2 are polybutadiene blocks, B1 and B2 are the same or different, (BS)1 is a butadiene-styrene copolymer, and based on the total weight of the butadiene block polymer, the ratio of the total weight of the styrene segments to the total weight of the butadiene segments is 2.3-9:1.
[0026] In the present invention, by controlling the ratio of the total weight of the styrene segments to the total weight of the butadiene segments to meet the above range, the molecular segment length of the single polybutadiene block (B1 or B2) in the block polymer having the above schematic structure can be shorter, and the total content of the butadiene segments in the polymer is increased, which is beneficial to improving the transparency and bending flexibility of the polymer and its hydrogenated product.
[0027] When the ratio of the total weight of the styrene segments to the total weight of the butadiene segments exceeds 9:1, the flexibility of the polymer and its hydrogenated product will deteriorate; when the ratio of the total weight of the styrene segments to the total weight of the butadiene segments is lower than 2.3, the transparency of the polymer and its hydrogenated product will deteriorate unfavorably due to the excessive length of the molecular chain of the single polybutadiene block (B1 or B2) in the block polymer.
[0028] Furthermore, based on the total weight of the polymer, the ratio of the total weight of the styrene segments to the total weight of the butadiene segments is 3-5.7:1.
[0029] According to the present invention, the number average molecular weight of the styrene-butadiene block polymer is 6×10 4 -12×10 4 .
[0030] In the present invention, in order to ensure the processing performance of the styrene-butadiene block polymer, the number average molecular weight of the styrene-butadiene block polymer should not exceed 12×10 4 .
[0031] Furthermore, the number average molecular weight of the styrene-butadiene block polymer is 7×10 4 -11×10 4 , preferably 8×10 4 -10×10 4 .
[0032] In the present invention, in order to obtain a styrene-butadiene block polymer with a uniform polymer block structure, the molecular weight distribution index of the styrene-butadiene block polymer is required to be ≤1.2, for example, 1-1.2. When the molecular weight distribution index of the styrene-butadiene block polymer exceeds 1.2, the molecular weight distribution of the polymer becomes broad, which means that block polymers such as S1-B1, S1-B1-(BS)1, S1-B1-(BS)1-S2, S1-B1-(BS)1-S2-B2 exist simultaneously in the styrene-butadiene block polymer.
[0033] In the present invention, the above-mentioned styrene-butadiene block polymer with narrow molecular weight distribution and its hydrogenation product have excellent mechanical properties.
[0034] Furthermore, the molecular weight distribution index of the styrene-butadiene block polymer is 1.01-1.1.
[0035] According to the present invention, based on the total weight (Bd%) of the butadiene segments in the butadiene-styrene block polymer, the content (Bv%) of 1,2-butadiene structural units is 6-30% by weight.
[0036] In the present invention, when the content of 1,2-butadiene structural units meets the above range based on the total weight of the butadiene segments in the butadiene block polymer, it can not only effectively shorten the molecular segment length in the polybutadiene segment, but also effectively destroy the regularity of the polybutadiene block molecular chain, so that the mechanical properties and bending flexibility of the polymer and its hydrogenated product are significantly improved under the premise of improved transparency. When the content of 1,2-butadiene structural units is too high, the bending flexibility of the butadiene block polymer is reduced.
[0037] In the present invention, the butadiene segment includes a polybutadiene block B1, a polybutadiene block B2 and a butadiene segment in a butadiene-styrene copolymer (BS) 1.
[0038] Furthermore, based on the total weight of the butadiene segments in the butadiene-styrene block polymer, the content of the 1,2-butadiene structural unit is 10-18% by weight.
[0039] According to the present invention, based on the total weight of the styrene-butadiene block polymer, the content of non-block styrene (St-non-block%) is 3-15% by weight.
[0040] In the present invention, non-block styrene refers to a styrene microblock formed by ≤4 styrene monomers in the molecular chain.
[0041] In the present invention, non-block styrene can effectively destroy the regularity of the molecular chain and inhibit the crystallization phenomenon. When the content of non-block styrene meets the above range, it can ensure that the polymer and its hydrogenated product have excellent mechanical properties. When the content of non-block styrene is too high, the high content of non-block styrene will destroy the physical crosslinking points and two-phase separation structure of the styrene-butadiene block polymer, resulting in the unfavorable reduction of the mechanical properties of the polymer and its hydrogenated product.
[0042] Furthermore, based on the total weight of the styrene-butadiene block polymer, the content of non-block styrene is 5-12% by weight.
[0043] In the present invention, in order to ensure the mechanical properties of the butadiene block polymer and its hydrogenated product, the contents of the polystyrene segments S1, S2 and S3 in the butadiene block polymer should not differ too much, and preferably have a symmetrical structure. For example, based on the total weight of the styrene segments in the butadiene block polymer, the content of the polystyrene block S1 is 25-35% by weight, the content of the polystyrene block S2 is 25-35% by weight, and the content of the polystyrene block S3 is 25-35% by weight.
[0044] Furthermore, based on the total weight of the styrene segments in the styrene-butadiene block polymer, the content of the polystyrene block S1 is 27-33% by weight, the content of the polystyrene block S2 is 27-33% by weight, and the content of the polystyrene block S3 is 27-33% by weight.
[0045] In the present invention, in order to ensure the mechanical properties of the block polymer, the number average molecular weight of the styrene blocks (S1 and S3) is generally required to be ≥1.5×10 4 .
[0046] A second aspect of the present invention provides a method for preparing a styrene-butadiene block polymer, characterized in that the preparation method comprises the following steps:
[0047] (1) in a solvent, in the presence of an initiator and a regulator, styrene I undergoes a first polymerization reaction to obtain a first polymer solution containing a polystyrene block S1;
[0048] (2) contacting butadiene I and styrene II with the first polymer solution to carry out a second polymerization reaction to obtain a second polymer solution containing S1-B1-(BS)1-S2;
[0049] (3) contacting butadiene II with the second polymer solution to perform a third polymerization reaction to obtain a third polymer solution comprising S1-B1-(BS)1-S2-B2;
[0050] (4) contacting styrene III with the third polymer solution to carry out a fourth polymerization reaction to obtain a fourth polymer solution comprising S1-B1-(BS)1-S2-B2-S3;
[0051] (5) Adding a terminator to the fourth polymer solution to obtain the butadiene-styrene block polymer.
[0052] In the present invention, the preparation method of the butadiene block polymer has the advantages of fewer steps, simple operation and good parallelism. Compared with the prior art, by introducing the chain segment structure of butadiene and styrene copolymer into the molecular chain of the polymer, the length of the butadiene chain segment in the polymer is effectively reduced, so that the prepared butadiene block polymer has improved transparency while having excellent mechanical properties and bending flexibility, thereby achieving comprehensive improvement of the mechanical properties, bending flexibility and transparency of the butadiene block polymer.
[0053] In the present invention, there is no particular limitation on the type of solvent, and the solvent may be a conventional solvent in the art, such as an organic hydrocarbon solvent.
[0054] In the present invention, the first polymerization reaction, the second polymerization reaction, the third polymerization reaction and the fourth polymerization reaction are each independently anionic solution polymerization reactions.
[0055] In the present invention, styrene I is subjected to homopolymerization reaction under the first polymer reaction conditions to obtain homopolymerized polystyrene block S1. In order to ensure the segment length of the molecular chain of polystyrene block S1, preferably, in step (1), the ratio of the amount of styrene I to the total amount of styrene (styrene I+styrene II+styrene III) is controlled to be 0.25-0.35:1. When the amount of styrene I meets the above range, it can ensure that the number average molecular weight of polystyrene block S1 is 1.5×10 4 -3×10 4 .
[0056] Furthermore, in step (1), the ratio of the amount of styrene I to the total amount of styrene (styrene I+styrene II+styrene III) is 0.3-0.35:1.
[0057] According to the present invention, the conditions of the first polymerization reaction include: the reaction temperature is 50-80°C.
[0058] In the present invention, there is no particular limitation on the time of the first polymerization reaction, as long as the styrene I is completely converted, that is, the conversion rate of styrene I is 100%.
[0059] According to the present invention, the initiator is at least one of methyllithium, ethyllithium, propyllithium, isopropyllithium, n-butyllithium and sec-butyllithium.
[0060] According to the present invention, based on the total amount of the styrene and the butadiene, the amount of the initiator is 0.9-1.6 mmol / 100g.
[0061] According to the present invention, the regulator is at least one of tetrahydrofuran, ditetrahydrofurfuryl propane, ethyl tetrahydrofurfuryl ether and N,N-dimethyltetrahydrofurfuryl amine.
[0062] According to the present invention, the molar ratio of the regulator to the initiator is 0.05-2:1.
[0063] According to the present invention, in step (2), butadiene I, styrene II and the first polymer solution containing polystyrene block S1 are subjected to anionic copolymerization under the second polymerization reaction conditions, wherein, in order to ensure the segment length of the polystyrene block S2 molecular chain, preferably, the ratio of the amount of styrene II to the total amount of styrene (styrene I + styrene II + styrene III) is 0.3-0.5:1.
[0064] In the present invention, the reactivity ratio of butadiene is greater than that of styrene. During the copolymerization reaction of styrene II and butadiene I, most of the butadiene I preferentially undergoes a butadiene homopolymerization reaction to generate a polybutadiene block B1. As the reaction proceeds, due to the consumption of butadiene I, the amount of styrene II is much greater than that of butadiene I. Part of butadiene I and styrene II undergo a copolymerization reaction to generate a butadiene-styrene random copolymer (BS) 1. When all butadiene I is consumed, the remaining styrene II undergoes a homopolymerization reaction to generate a polystyrene block S2.
[0065] Furthermore, the ratio of the amount of styrene II to the total amount of styrene (styrene I+styrene II+styrene III) is 0.35-0.45:1.
[0066] According to the present invention, in step (2), the ratio of the amount of butadiene I to the total amount of butadiene (butadiene I + butadiene II) is 0.5-0.7:1, preferably 0.55-0.65:1.
[0067] According to the present invention, the conditions of the second polymerization reaction include: the reaction temperature is 50-80°C.
[0068] In the present invention, when the temperature of the second polymerization reaction satisfies the above range, the ratio of butadiene-styrene copolymer (BS) 1 can be regulated and the polymerization reaction rate can be appropriate.
[0069] In the present invention, the reaction time of the second polymerization reaction is not particularly limited, as long as the complete conversion of styrene II and butadiene I is ensured, that is, the conversion rate of styrene II and butadiene I is 100%.
[0070] According to the present invention, in step (3), butadiene II is contacted with a second polymer solution comprising S1-B1-(BS)1-S2 to carry out anionic copolymerization. In the present invention, in order to ensure that the polybutadiene block B1 and the polybutadiene block B2 have similar molecular chain lengths, thereby improving the comprehensive properties of the block polymer, preferably, the ratio of the amount of butadiene II to the total amount of butadiene is 0.3-0.5:1, preferably 0.35-0.45:1.
[0071] According to the present invention, the conditions of the third polymerization reaction include: the reaction temperature is 50-80°C.
[0072] In the present invention, when the temperature of the third polymerization reaction satisfies the above range, the polymerization reaction can have a suitable reaction rate, and the butadiene block polymer described in the first aspect of the present invention can be finally obtained.
[0073] In the present invention, the reaction time of the third polymerization reaction is not particularly limited, as long as the butadiene II is completely converted, that is, the conversion rate of butadiene II is 100%.
[0074] According to the present invention, in step (4), styrene III is contacted with a third polymer solution comprising S1-B1-(BS)1-S2-B2 to perform an anionic copolymerization reaction, wherein, in order to ensure the segment length of the polystyrene block S3 molecular chain, preferably, the ratio of the amount of styrene III to the total weight of styrene (styrene I+styrene II+styrene III) is 0.25-0.35:1. When the amount of styrene III meets the above range, it can ensure that the number average molecular weight of the polystyrene block S3 is 1.5×10 4 -3×10 4 .
[0075] Furthermore, the ratio of the amount of styrene III to the total weight of styrene (styrene I+styrene II+styrene III) is 0.3-0.35:1.
[0076] According to the present invention, the conditions of the fourth polymerization reaction include: the reaction temperature is 50-80°C.
[0077] In the present invention, the reaction time of the fourth polymerization reaction is not particularly limited, as long as the complete conversion of styrene III is ensured, that is, the conversion rate of styrene III is 100%.
[0078] According to the present invention, the ratio of the total amount of styrene (styrene I+styrene II+styrene III) to the total amount of butadiene (butadiene I+butadiene II) is 2.3-9:1.
[0079] In the present invention, when the ratio of the total amount of styrene to the total amount of butadiene satisfies the above range, it can ensure that the prepared butadiene block polymer has excellent mechanical properties and bending flexibility while having improved transparency, thereby achieving a comprehensive improvement in the mechanical properties, bending flexibility and transparency of the butadiene block polymer.
[0080] Furthermore, the ratio of the total amount of styrene to the total amount of butadiene is 3-5.7:1.
[0081] The third aspect of the present invention provides a butadiene styrene block polymer prepared by the above preparation method.
[0082] A fourth aspect of the present invention provides a use of the above-mentioned butadiene-styrene block polymer in the preparation of an optical material precursor.
[0083] The present invention will be described in detail below through examples.
[0084] The butadiene content (Bd%), 1,2-structural unit content (Bv%), styrene content (St%), block styrene content (St-block%) and non-block styrene content (St-non-block%) of butadiene-styrene block polymers were measured using a Bruker AVANCE400 superconducting nuclear magnetic resonance instrument ( 1 H-NMR) test, 1 The resonance frequency of the H nucleus is 300.13 MHz, the spectrum width is 2747.253 Hz, the pulse width is 5 μs, the data point is 16 K, the sample tube diameter is 5 mm, the solvent is deuterated chloroform CDCl3, the sample concentration is 15% (W / V), the test temperature is room temperature, the number of scans is 16 times, and the chemical shift of tetramethylsilane is calibrated to 0 ppm.
[0085] The molecular weight and molecular weight distribution of the butadiene block polymer were determined using an HLC-8320 gel permeation chromatograph produced by Tosoh Corporation of Japan. The test conditions included: the chromatographic column was TSKgel SuperMultiporeHZ-N, the standard column was TSKgel SuperMultiporeHZ, the solvent was chromatographic grade THF, the calibration standard was polystyrene, the sample mass concentration was 1 mg / mL, the injection volume was 10 μL, the flow rate was 0.35 mL / min, and the test temperature was 40°C.
[0086] The transmittance and haze were tested using a Japanese NDH-1001DP turbidity meter, and the test standard was ASTM D1003-2000.
[0087] The mechanical properties were tested using an INSTRON 5567 electronic tensile testing machine produced by Instron Corporation of the United States.
[0088] The tensile properties are tested according to GB / T 1040.1-2018, and the bending properties are tested according to GB / T 9341-2008.
[0089] The impact strength was tested using a pendulum impact tester Ceast Resil Impactor 6957 produced by CEAST, Italy, in accordance with GB / T 1843-2008.
[0090] Experimental apparatus and process: The experiment was carried out in a 5L polymerization reactor. The solvent, butadiene and styrene monomers were added from the polymerization pipeline, and the initiator, structure regulator and terminator were added from the top of the polymerization reactor using a syringe.
[0091] Cyclohexane was purchased from Sinopharm Reagent Company with a purity of >99.9, and the water content was less than 5ppm after soaking in molecular weight sieve for 15 days;
[0092] Styrene, polymer grade, sourced from Yanshan Petrochemical;
[0093] Butadiene, polymer grade, sourced from Yanshan Petrochemical;
[0094] Butyl lithium (Li) was purchased from J&K Reagent Company, 100 ml, 1.6 mol·L -1 Cyclohexane solution, diluted to 0.4 mol·L -1 Cyclohexane solution;
[0095] Tetrahydrofuran (THF) was purchased from J&K Reagent Company in a 500 g specification, chromatographically pure, and with a relative molecular mass of 72.1 g / mol.
[0096] Example 1
[0097] This example is used to illustrate the styrene-butadiene block polymer and the preparation method thereof of the present invention.
[0098] (1) Under nitrogen protection, a solvent (cyclohexane), a structure regulator (tetrahydrofuran), and styrene I (types and amounts are shown in Table 1, and the amounts listed in the table are all measured based on pure compounds) were added to a 5 L reactor, the polymerization temperature was controlled within the range of 50-80° C., a designed amount of n-butyl lithium (amount is shown in Table 1, and the amounts listed in the table are all measured based on pure compounds) was added to the 5 L reactor to prepare polystyrene block S1, and analysis and testing were performed. The results are shown in Table 2;
[0099] (2) After styrene I is completely converted, a designed amount of butadiene I and styrene II (the types and amounts are shown in Table 1, and the amounts listed in the table are all measured based on pure compounds) are added to the reactor to prepare a block polymer S1-B1-(BS)1-S2, and the analysis and testing are performed. The results are shown in Table 2;
[0100] (3) After the butadiene I and styrene II are completely converted, a designed amount of butadiene II (the type and amount are shown in Table 1, and the amounts listed in the table are all measured based on the pure compound) is added to the reactor to prepare a block polymer S1-B1-(BS)1-S2-B2;
[0101] (4) After the butadiene II is completely converted, a designed amount of styrene III (the type and amount are shown in Table 1, and the amounts listed in the table are all measured based on the pure compound) is added to the reactor to prepare a block polymer S1-B1-(BS)1-S2-B2-S3;
[0102] (5) After the complete conversion of styrene III, a designed amount of terminator (isopropanol) was added to the reactor (the type and amount are shown in Table 1, and the amounts listed in the table are all measured based on the pure compound) to obtain S1-B1-(BS)1-S2-B2-S3 butadiene block polymer P1, and a structural analysis test was performed. The results are shown in Table 2; the physical properties of the sample were tested, and the results are shown in Table 3.
[0103] Embodiment 2-8
[0104] This example is used to illustrate the styrene-butadiene block polymer and the preparation method thereof of the present invention.
[0105] The method described in Example 1 is different in that the butadiene block polymers are prepared using the parameters shown in Table 1 to obtain butadiene block polymers P2-P8 respectively, and structural analysis tests are performed. The results are shown in Table 2; the physical properties of the samples are tested, and the results are shown in Table 3.
[0106] Table 1
[0107]
[0108]
[0109] Table 1 (continued)
[0110]
[0111]
[0112] Table 2
[0113]
[0114]
[0115] Note: St% / Bd%, is the ratio of the total weight of styrene segments to the total weight of butadiene segments.
[0116] Table 2 (continued)
[0117]
[0118] Note: St% / Bd%, is the ratio of the total weight of styrene segments to the total weight of butadiene segments.
[0119] Table 3
[0120]
[0121] It can be seen from the results in Table 3 that the butadiene block polymer prepared by the present invention shortens the length of a single butadiene block molecular segment and introduces a certain proportion of butadiene and styrene copolymers into the molecular segment, so that the butadiene block polymer has improved transparency while having excellent mechanical properties and bending flexibility, thereby achieving comprehensive improvement in the mechanical properties, bending flexibility and transparency of the butadiene block polymer.
[0122] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A styrene-butadiene block polymer, characterized in that: The polymer has a structure shown as S1-B1-(BS)1-S2-B2-S3; Among them, S1, S2, and S3 are polystyrene blocks, B1 and B2 are polybutadiene blocks, and (BS)1 is a butadiene-styrene copolymer; Based on the total weight of the polymer, the ratio of the total weight of the styrene chain segments to the total weight of the butadiene chain segments is 2.3-9:
1.
2. The styrene-butadiene block polymer according to claim 1, wherein Based on the total weight of the polymer, the ratio of the total weight of the styrene chain segments to the total weight of the butadiene chain segments is 3-5.7:
1.
3. The styrene-butadiene block polymer according to claim 1 or 2, wherein The number average molecular weight of the styrene-butadiene block polymer is 6×10 4 -12×10 4 , preferably 7×10 4 -11×10 4 , more preferably 8×10 4 -10×10 4 .
4. The styrene-butadiene block polymer according to any one of claims 1 to 3, wherein The molecular weight distribution index of the styrene-butadiene block polymer is 1-1.2, preferably 1.01-1.
1.
5. The styrene-butadiene block polymer according to any one of claims 1 to 4, wherein Based on the total weight of the butadiene segments in the butadiene-styrene block polymer, the content of the 1,2-butadiene structural unit is 6-30% by weight, preferably 10-18% by weight.
6. The styrene-butadiene block polymer according to any one of claims 1 to 5, wherein Based on the total weight of the styrene-butadiene block polymer, the content of non-block styrene is 3-15% by weight, preferably 5-12% by weight.
7. The styrene-butadiene block polymer according to any one of claims 1 to 6, wherein Based on the total weight of the styrene segments in the styrene-butadiene block polymer, the content of the polystyrene block S1 is 25-35% by weight, preferably 27-33% by weight; Preferably, based on the total weight of the styrene segments in the styrene-butadiene block polymer, the content of the polystyrene block S2 is 25-35% by weight, preferably 27-33% by weight; Preferably, based on the total weight of the styrene segments in the styrene-butadiene block polymer, the content of the polystyrene block S3 is 25-35% by weight, preferably 27-33% by weight.
8. A method for preparing a butadiene-styrene block polymer, characterized in that: The preparation method comprises the following steps: (1) in a solvent, in the presence of an initiator and a regulator, styrene I undergoes a first polymerization reaction to obtain a first polymer solution containing a polystyrene block S1; (2) contacting butadiene I and styrene II with the first polymer solution to carry out a second polymerization reaction to obtain a second polymer solution containing S1-B1-(BS)1-S2; (3) contacting butadiene II with the second polymer solution to perform a third polymerization reaction to obtain a third polymer solution comprising S1-B1-(BS)1-S2-B2; (4) contacting styrene III with the third polymer solution to carry out a fourth polymerization reaction to obtain a fourth polymer solution comprising S1-B1-(BS)1-S2-B2-S3; (5) Adding a terminator to the fourth polymer solution to obtain the butadiene-styrene block polymer.
9. The preparation method according to claim 8, wherein: In step (1), the ratio of the amount of styrene I to the total amount of styrene is 0.25-0.35:1; Preferably, the conditions of the first polymerization reaction include: a reaction temperature of 50-80°C; Preferably, the initiator is selected from at least one of methyllithium, ethyllithium, propyllithium, isopropyllithium, n-butyllithium and sec-butyllithium; Preferably, based on the total amount of the styrene and the butadiene, the amount of the initiator is 0.9-1.6 mmol / 100g; Preferably, the regulator is selected from at least one of tetrahydrofuran, ditetrahydrofurfuryl propane, ethyl tetrahydrofurfuryl ether and N,N-dimethyltetrahydrofurfuryl amine; Preferably, the molar ratio of the regulator to the initiator is 0.05-2:
1.
10. The preparation method according to claim 8 or 9, wherein: In step (2), the ratio of the amount of styrene II to the total amount of styrene is 0.3-0.5:1; Preferably, the ratio of the amount of butadiene I to the total amount of butadiene is 0.5-0.7:1; Preferably, the conditions of the second polymerization reaction include: a reaction temperature of 50-80°C.
11. The preparation method according to any one of claims 8 to 10, wherein: In step (3), the ratio of the amount of butadiene II to the total amount of butadiene is 0.3-0.5:1; Preferably, the conditions of the third polymerization reaction include: the reaction temperature is 50-80°C.
12. The preparation method according to any one of claims 8 to 11, wherein: In step (4), the ratio of the amount of styrene III to the total amount of styrene is 0.25-0.35:1; Preferably, the conditions of the fourth polymerization reaction include: the reaction temperature is 50-80°C.
13. The preparation method according to any one of claims 8 to 12, wherein: The ratio of the total amount of styrene to the total amount of butadiene is 2.3-9:
1.
14. A butadiene-styrene block polymer obtained by the preparation method described in any one of claims 8 to 13.
15. Use of the styrene-butadiene block polymer according to any one of claims 1 to 7 and 14 in preparing an optical material precursor.
Citation Information
Patent Citations
Impact-resistant transparent linear asymmetric block copolymer of vinyl aromatic hydrocarbon and conjugated diene and preparation method of block copolymer
CN102108114A
Production of butadiene-styrene block copolymer
CN1123797A
Method for producing transparent block copolymer resin
US4122134A
Transparent block copolymers having two monovinyl-substituted aromatic blocks of different molecular weight
US4939208A