Molded MIL-101 (Cr)-SO3Ag-SA material, preparation method and application of molded MIL-101 (Cr)-SO3Ag-SA material
The molded MIL-101(Cr)-SO3Ag-SA material prepared by the hydrothermal synthesis method solves the problem of sulfur dioxide removal problems and low material preparation efficiency in the existing technology, and achieves high-efficiency adsorption desulfurization performance and simplified industrial application.
Patent Information
- Application Number
- CN202410975721.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to effectively remove sulfur dioxide emissions generated when burning coal with the existing technology, and the preparation method of metal organic framework materials has problems with low yield and incomplete crystal structure, which affects its adsorption desulfurization performance.
A preparation method for molding MIL-101(Cr)-SO3Ag-SA material is adopted. MIL-101(Cr)-SO3Ag is synthesized through hydrothermal synthesis. SO3Ag groups are introduced and formed by sodium alginate to form spherical MOFs materials. , improve its adsorption desulfurization performance.
The adsorption desulfurization capacity and yield are improved, the crystal structure of the material is more complete, more active sites are provided, the adsorption effect on sulfur dioxide is enhanced, and the industrial production process is simplified.
Smart Images

Figure CN118772430A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal organic framework materials, and in particular to the preparation and application of a metal organic framework material. Background Art
[0002] Coal is the main energy source in my country, accounting for more than 70% of energy consumption. In the process of high-temperature combustion of coal, in addition to SO2, it not only produces acid rain, but is also one of the factors causing haze. Sulfur dioxide concentration in the atmosphere above 0.5 ppm has potential effects on the human body; at 1-3 ppm, most people begin to feel irritated; at 400-500 ppm, people will develop ulcers and pulmonary edema until suffocation and death. Sulfur dioxide has a synergistic effect with smoke in the atmosphere. When the sulfur dioxide concentration in the atmosphere is 0.21 ppm and the smoke concentration is greater than 0.3 mg / L, the incidence of respiratory diseases can increase and the condition of patients with chronic diseases can deteriorate rapidly.
[0003] Post-combustion flue gas desulfurization is the most studied and fastest-developed technology in SO2 emission reduction technology. It is also the only desulfurization technology currently used on a large scale in commercial applications in the world. According to whether water is added during the desulfurization process and the dry and wet forms of the desulfurization products, it can be divided into three processes: wet, semi-dry and dry. Adsorption desulfurization is a type of dry desulfurization. In addition to reducing solid waste, the adsorbed sulfur oxides can be released during regeneration and recycled as a by-product in the form of dilute sulfuric acid or elemental sulfur.
[0004] Metal organic framework materials are good adsorbents due to their adjustable pore size, large surface area, adjustable functions, etc. They show excellent desulfurization performance in adsorption desulfurization and have great application prospects. They have attracted extensive attention from researchers. The central metal in MOFs plays a key role in regulating the desulfurization performance. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a molded MIL-101(Cr)-SO3Ag-SA material, a preparation method and its application, which has more complete synthesis, high yield and more complete crystal structure, and is conducive to improving the adsorption desulfurization performance.
[0006] The object of the present invention is achieved by: a method for preparing a molded MIL-101(Cr)-SO3Ag-SA material, comprising the following steps: Step 1) The reactants chromium nitrate nonahydrate, monosodium 2-sulfonate terephthalate and terephthalic acid are added to deionized water and hydrofluoric acid and mixed, the mixed solution is ultrasonically stirred until uniformly mixed, and then added to a reactor for mixed reaction, and after cooling, filtered, washed, and dried to obtain MIL-101(Cr)-SO3H; Step 2) dissolve silver nitrate in a mixed solution of acetonitrile and water and stir to dissolve, then add the prepared MIL-101(Cr)-SO3H, stir at room temperature for a set time, filter, and wash with deionized water. Repeat the above steps twice, then wash the sample with deionized water, dry at a set temperature for a set time, and obtain MIL-101(Cr)-SO3Ag powder; Step 3) MIL-101(Cr)-SO3Ag powder, sodium alginate and deionized water are mixed and stirred into a uniform solution, and the uniform solution is added dropwise into a calcium chloride solution. The MOFs powder is formed into a sphere in the solution. The spherical MOFs are soaked in the calcium chloride solution for a set time, filtered, soaked in deionized water, and dried to obtain a molded MOFs material MIL-101(Cr)-SO3Ag-SA.
[0007] Furthermore, in step 1), the molar ratio of the reactants chromium nitrate nonahydrate, monosodium 2-sulfonate terephthalate, and terephthalic acid is 1:0.2~0.4:0.8~0.6.
[0008] Furthermore, the mixing reaction in step 1) is a hydrothermal synthesis reaction carried out in a high-pressure reactor, the reaction temperature is 200-220 °C, and the reaction time is 8-18h.
[0009] Furthermore, in the mixed solution of acetonitrile and water in step 2), the ratio of acetonitrile to water is 1:1.
[0010] Furthermore, in step 2), the mixture is stirred at room temperature for 12 hours.
[0011] Furthermore, the entire process of step 2) is carried out under light-proof conditions.
[0012] A MIL-101(Cr)-SO3Ag-SA material is prepared by adopting the preparation method.
[0013] The invention discloses an application of a MIL-101(Cr)-SO3Ag-SA material for adsorbing and removing sulfur dioxide in flue gas.
[0014] Furthermore, the adsorption desulfurization temperature of the MIL-101(Cr)-SO3Ag-SA material is 80-120°C, and the desulfurization time is 1-6 hours.
[0015] Compared with the prior art, the present invention has the following beneficial effects: (1) The MIL-101(Cr)-SO3Ag-SA in the present invention has adsorption desulfurization ability and a large specific surface area, and the SO3Ag group provides an active site for adsorption desulfurization; at the same time, the preparation method adopts a hydrothermal synthesis method to synthesize MIL-101(Cr)-SO3Ag-SA, which can make the synthesis more complete, the yield is high, and the crystal structure is more complete, which is conducive to improving the adsorption desulfurization performance; (2) The material of the present invention can be synthesized in batches. Compared with other synthesis methods, no adhesive or co-solvent is required during the synthesis of the composite material, the processing time is short, the cost is low, and the operation method is simple and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0017] Figure 1 These are SEM images of MIL-101(Cr) (a) and MIL-101(Cr)-SO3Ag-X (bd) of the present invention.
[0018] Figure 2 FT-IR diagram of MIL-101(Cr) and MIL-101(Cr)-SO3Ag-X of the present invention.
[0019] Figure 3 The XRD diagrams of MIL-101(Cr) and MIL-101(Cr)-SO3Ag-X of the present invention are shown in FIG.
[0020] Figure 4 These are the adsorption breakthrough curves of MIL-101(Cr) and MIL-101(Cr)-SO3Ag-SA-X of the present invention.
[0021] Figure 5 This is a diagram of particles formed by the calcium alginate method in the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1.
[0024] 1. Preparation of metal-organic framework materials.
[0025] The raw materials were weighed according to the following weights: 4 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O) and 1.66 g of terephthalic acid (H2BDC) (the molar ratio of the two was 1:1); the raw materials were placed in a 100 mL polytetrafluoroethylene liner and mixed, 70 mL of deionized water and 0.5 mL of hydrofluoric acid were added, and stirred at room temperature for 6 h. After the solution was evenly mixed, the polytetrafluoroethylene liner was loaded into a high-pressure reactor, and the reaction was carried out at 220 ° C for 8 h to obtain a reaction mother liquor. After cooling to room temperature, it was filtered, washed with ethanol, and vacuum dried to obtain MIL-101 (Cr).
[0026] MIL-101(Cr) powder, sodium alginate and deionized water are mixed and stirred into a uniform solution, and the obtained solution is added dropwise into a calcium chloride solution, and the MOFs powder is formed into a sphere in the solution; the spherical MOFs are soaked in the calcium chloride solution, filtered, soaked in deionized water and then dried to obtain a molded MOFs material MIL-101(Cr)-SA.
[0027] 2. Detection of metal-organic framework materials.
[0028] Attached Figure 1 In (a), it can be seen that MIL-101(Cr) has an octahedral structure and the particle surface is smooth. Figure 2 Figure 3 As shown in the figure, Fourier transform infrared spectroscopy (FT-IR) and X-ray diffraction analysis show that MIL-101(Cr) has sharp peaks, well-developed crystals and high crystallinity. Figure 4 It can be seen that MIL-101 (Cr) has a significant effect in adsorbing SO2.
[0029] 3. Application of MIL-101(Cr)-SA composite materials.
[0030] A standard SO2 gas with a gas content of 2500 mg / Nm³ was selected. 1 g of the adsorbent was weighed and placed in a U-shaped tube, and the U-shaped tube containing 1 g of adsorbent was placed in a 120 ℃ constant temperature oil bath. The SO2 gas with a flow rate of 200 mL / min was used to flow through the adsorbent for the experiment. The dynamic adsorption value of the adsorbent was recorded using a Siemens U23 SO2 analyzer.
[0031] Example 2.
[0032] 1. Preparation of metal-organic framework materials.
[0033] Weigh the following raw materials: 4 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O), 0.57 g of monosodium 2-sulfonatoterephthalate (C8H5NaO7S), and 1.33 g of terephthalic acid (H2BDC) (the molar ratio of the three is 1:0.2:0.8, respectively); place the raw materials in a 100 mL polytetrafluoroethylene liner and mix them, add 70 mL of deionized water and 0.5 mL of hydrofluoric acid, and stir at room temperature for 6 h. After the solution is evenly mixed, put the polytetrafluoroethylene liner into a high-pressure reactor, react at 220 °C for 8 h to obtain a reaction mother liquor, cool it to room temperature, filter it, wash it with ethanol, and vacuum dry it to obtain MIL-101(Cr)-SO3H-0.2; Dissolve 0.8 g of silver nitrate in 20 mL of a mixed solution of acetonitrile and water and stir to dissolve. Then add 3.5 g of the prepared MIL-101(Cr)-SO3H-0.3, stir at 25 °C for 12 hours, filter, and wash with deionized water. Repeat the above steps twice to allow the ion exchange process to proceed fully. Then wash the sample with deionized water and dry it at 120 °C for 24 hours to obtain MIL-101(Cr)-SO3Ag-0.2.
[0034] MIL-101(Cr)-SO3Ag-0.2 powder, sodium alginate and deionized water are mixed and stirred into a uniform solution, and the obtained solution is added dropwise into a calcium chloride solution, and the MOFs powder is formed into a sphere in the solution; the spherical MOFs are soaked in the calcium chloride solution, filtered, soaked in deionized water and then dried to obtain a molded MOFs material MIL-101(Cr)-SO3Ag-SA-0.2.
[0035] 2. Detection of metal-organic framework materials.
[0036] Attached Figure 1 In (b), it can be seen that MIL-101(Cr)-SO3Ag-0.2 has an octahedral structure. Figure 2 As shown in Figure 2, Fourier transform infrared spectroscopy (FT-IR) shows that the introduction of SO3Ag groups did not cause changes in the functional groups and structure of MIL-101(Cr). Figure 3 As shown in the figure, X-ray diffraction analysis confirmed that the crystal structure of MIL-101(Cr)-SO3Ag-0.2 did not change, which was consistent with the pure sample. Figure 4 It can be seen that the adsorption performance of SO2 is further improved after the introduction of silver sulfonate functional groups compared with the pure MIL-101 (Cr) sample.
[0037] 3. Application of MIL-101(Cr)-SO3Ag-SA-0.2 composite material.
[0038] A standard SO2 gas with a gas content of 2500 mg / Nm³ was selected. 1 g of the adsorbent was weighed and placed in a U-shaped tube, and the U-shaped tube containing 1 g of adsorbent was placed in a 120 ℃ constant temperature oil bath. The SO2 gas with a flow rate of 200 mL / min was used to flow through the adsorbent for the experiment. The dynamic adsorption value of the adsorbent was recorded using a Siemens U23 SO2 analyzer.
[0039] Example 3.
[0040] 1. Preparation of metal-organic framework materials.
[0041] Weigh the following raw materials: 4 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O), 0.86 g of monosodium 2-sulfonatoterephthalate (C8H5NaO7S), and 1.16 g of terephthalic acid (H2BDC) (the molar ratio of the three is 1:0.3:0.7, respectively); place the raw materials in a 100 mL polytetrafluoroethylene liner and mix them, add 70 mL of deionized water and 0.5 mL of hydrofluoric acid, and stir at room temperature for 6 h. After the solution is evenly mixed, put the liner into a high-pressure reactor and react at 220 °C for 8 h to obtain a reaction mother liquor. After cooling to room temperature, filter it, wash it with ethanol, and vacuum dry it to obtain MIL-101(Cr)-SO3Ag-0.3; Dissolve 0.8 g of silver nitrate in 20 mL of a mixed solution of acetonitrile and water and stir to dissolve. Then add 3.5 g of the prepared MIL-101(Cr)-SO3H-0.3, stir at 25 °C for 12 hours, filter, and wash with deionized water. Repeat the above steps twice to allow the ion exchange process to proceed fully. Then wash the sample with deionized water and dry it at 120 °C for 24 hours to obtain MIL-101(Cr)-SO3Ag-0.3.
[0042] MIL-101(Cr)-SO3Ag-0.3 powder, sodium alginate and deionized water are mixed and stirred into a uniform solution, and the obtained solution is added dropwise into a calcium chloride solution, and the MOFs powder is formed into a sphere in the solution; the spherical MOFs are soaked in the calcium chloride solution, filtered, soaked in deionized water and then dried to obtain a molded MOFs material MIL-101(Cr)-SO3Ag-SA-0.3.
[0043] 2. Detection of metal-organic framework materials.
[0044] Attached Figure 1 In (c), it can be seen that MIL-101(Cr)-SO3Ag-0.3 has an octahedral structure. Figure 2 and Figure 3As shown in the figure, Fourier transform infrared spectroscopy (FT-IR) and X-ray diffraction (XRD) show that the diffraction peak position of MIL-101(Cr)-SO3Ag-0.3 material is basically the same as before, and no new diffraction peak is observed. Only the intensity of the diffraction peak decreases, indicating that the skeleton structure of the crystal remains unchanged and the crystallinity decreases to a certain extent. Figure 4 It can be seen that as the amount of silver sulfonate functional groups introduced increases, the adsorption performance is still higher than that of the pure sample.
[0045] 3. Application of MIL-101(Cr)-SO3Ag-SA-0.3 composite material.
[0046] A standard SO2 gas with a gas content of 2500 mg / Nm³ was selected. 1 g of the adsorbent was weighed and placed in a U-shaped tube, and the U-shaped tube containing 1 g of adsorbent was placed in a 120 ℃ constant temperature oil bath. The SO2 gas with a flow rate of 200 mL / min was used to flow through the adsorbent for the experiment. The dynamic adsorption value of the adsorbent was recorded using a Siemens U23 SO2 analyzer.
[0047] Example 4.
[0048] 1. Preparation of metal-organic framework materials.
[0049] Weigh the following raw materials: 4 g of chromium nitrate nonahydrate (Cr(NO3)3·9H2O), 1.14 g of monosodium 2-sulfonatoterephthalate (C8H5NaO7S), and 0.99 g of terephthalic acid (H2BDC) (the molar ratio of the three is 1:0.4:0.6, respectively); place the reactants in a 100 mL polytetrafluoroethylene liner and mix them, add 70 mL of deionized water and 0.5 mL of hydrofluoric acid, and stir at room temperature for 6 h. After the solution is evenly mixed, put the liner into a high-pressure reactor and react at 220 °C for 8 h to obtain a reaction mother liquor. After cooling to room temperature, filter it, wash it with ethanol, and vacuum dry it to obtain MIL-101(Cr)-SO3Ag-0.4; Dissolve 0.8 g of silver nitrate in 20 mL of a mixed solution of acetonitrile and water and stir to dissolve. Then add 3.5 g of the prepared MIL-101(Cr)-SO3H-0.4, stir at 25 °C for 12 hours, filter, and wash with deionized water. Repeat the above steps twice to allow the ion exchange process to proceed fully. Then wash the sample with deionized water and dry it at 120 °C for 24 hours to obtain MIL-101(Cr)-SO3Ag-0.4.
[0050] MIL-101(Cr)-SO3Ag-0.4 powder, sodium alginate and deionized water are mixed and stirred into a uniform solution, and the obtained solution is added dropwise into a calcium chloride solution, and the MOFs powder is formed into a sphere in the solution; the spherical MOFs are soaked in the calcium chloride solution, filtered, soaked in deionized water and then dried to obtain a molded MOFs material MIL-101(Cr)-SO3Ag-SA-0.4.
[0051] 2. Detection of metal-organic framework materials.
[0052] Attached Figure 1 In (d), MIL-101(Cr)-SO3Ag-0.4 has an octahedral structure. Figure 2 As shown in the figure, Fourier transform infrared spectroscopy (FT-IR) shows that the diffraction peak position of the material is basically the same as before, and no new diffraction peak is observed. Figure 3 As shown, X-ray diffraction analysis showed that the crystal form of MIL-101(Cr)-SO3Ag-0.4 did not change. Figure 4 It can be seen that the adsorption performance gradually improves with the increase of the amount of silver sulfonate functional groups introduced.
[0053] 3. Application of MIL-101(Cr)-SO3Ag-SA-0.4 composite material.
[0054] A standard SO2 gas with a gas content of 2500 mg / Nm³ was selected. 1 g of the adsorbent was weighed and placed in a U-shaped tube, and the U-shaped tube containing 1 g of adsorbent was placed in a 120 ℃ constant temperature oil bath. The SO2 gas with a flow rate of 200 mL / min was used to flow through the adsorbent for the experiment. The dynamic adsorption value of the adsorbent was recorded using a Siemens U23 SO2 analyzer.
[0055] In Examples 1-4, the steps for determining the SO2 content using Siemens U23 SO2 analyzer are as follows: 1. Select SO2 standard gas with a gas content of 2500 mg / Nm³ and heat it to 120 ℃ in a constant temperature oil bath to simulate SO2 in flue gas; 2. SO2 gas flows through the adsorption material and enters the analyzer to record real-time dynamic adsorption data; 3. Through the formula The adsorption amount was calculated as mg SO2 / g.
[0056] Example 5.
[0057] Comparison of adsorption desulfurization performance of different adsorbents Attached Figure 4The adsorption penetration curves of MIL-101(Cr) and MIL-101(Cr)-SO3Ag-SA of the present invention are shown in the figure. From the figure, a comparison table of the adsorption performance of MIL-101(Cr)-SO3Ag-SA-X adsorbents with different synthesis conditions under the SO2 standard gas concentration of 2500 mg / Nm³ can be obtained:
[0058] The material obtained by the present invention has a strong adsorption and removal ability for sulfur dioxide in flue gas because MIL-101(Cr)-SO3Ag-SA contains abundant active sites, which provide adsorption points for combining with sulfur atoms. Although MIL-101(Cr) prepared in the comparative example has a large specific surface area, it lacks active sites and has a weak adsorption effect on sulfur.
[0059] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a molded MIL-101(Cr)-SO3Ag-SA material, characterized in that: The steps include: Step 1) The reactants chromium nitrate nonahydrate, monosodium 2-sulfonate terephthalate and terephthalic acid are added to deionized water and hydrofluoric acid and mixed, the mixed solution is ultrasonically stirred until uniformly mixed, and then added to a reactor for mixed reaction, and after cooling, filtered, washed, and dried to obtain MIL-101(Cr)-SO3H; Step 2) dissolve silver nitrate in a mixed solution of acetonitrile and water and stir to dissolve, then add the prepared MIL-101(Cr)-SO3H, stir at room temperature for a set time, filter, and wash with deionized water. Repeat the above steps twice, then wash the sample with deionized water, dry at a set temperature for a set time, and obtain MIL-101(Cr)-SO3Ag powder; Step 3) MIL-101(Cr)-SO3Ag powder, sodium alginate and deionized water are mixed and stirred into a uniform solution, and the uniform solution is added dropwise into a calcium chloride solution. The MOFs powder is formed into a sphere in the solution. The spherical MOFs are soaked in the calcium chloride solution for a set time, filtered, soaked in deionized water, and dried to obtain a molded MOFs material MIL-101(Cr)-SO3Ag-SA.
2. The method for preparing a molded MIL-101(Cr)-SO3Ag-SA material according to claim 1, characterized in that: In step 1), the molar ratio of the reactants chromium nitrate nonahydrate, monosodium 2-sulfonate terephthalate, and terephthalic acid is 1:0.2-0.4:0.8-0.
6.
3. The method for preparing a MIL-101(Cr)-SO3Ag-SA material according to claim 1 or 2, characterized in that: The mixing reaction in step 1) is a hydrothermal synthesis reaction carried out in a high-pressure reactor, the reaction temperature is 200-220 ° C, and the reaction time is 8-18 h.
4. The method for preparing a MIL-101(Cr)-SO3Ag-SA material according to claim 1 or 2, characterized in that: In the step 2), the mixed solution of acetonitrile and water has a ratio of acetonitrile to water of 1:
1.
5. The method for preparing a MIL-101(Cr)-SO3Ag-SA material according to claim 1 or 2, characterized in that: In the step 2), the mixture is stirred at room temperature for 12 hours.
6. The method for preparing a MIL-101(Cr)-SO3Ag-SA material according to claim 1 or 2, characterized in that: The entire process of step 2) is carried out under light-proof conditions.
7. A MIL-101(Cr)-SO3Ag-SA material, characterized in that: Prepared by the preparation method described in any one of claims 1-5.
8. An application of the MIL-101(Cr)-SO3Ag-SA material as claimed in claim 5, characterized in that: Used to adsorb and remove sulfur dioxide in flue gas.
9. The use of the MIL-101(Cr)-SO3Ag-SA material according to claim 6, characterized in that: The adsorption desulfurization temperature of the MIL-101(Cr)-SO3Ag-SA material is 80-120°C, and the desulfurization time is 1-6 hours.
Citation Information
Patent Citations
Metal organic framework adsorbent as well as preparation method and application thereof
CN104492383A
Preparation and novel application of a type of MIL-101(Cr) adsorbent modified by virtue of post translation
CN105107467A
Sodium alginate-MOF (metal organic framework) composite spherule as well as preparation method and application thereof
CN105498695A
Preparation method of sodium alginate-MOFs composite microsphere for adsorbing heavy metal selenium
CN108339521A
Metal-organic framework material, and molding method and application thereof
CN108940211A