A trifluoromethyltricarboxylic acid-based MOF material, preparation method and SO2 separation application

By designing the MOF material of trifluoromethyltricarboxylic acid, solubilizing thermal reaction and tetrafluoroboric acid to regulate acidity, a stable porous frame structure is formed, which solves the problems of low separation efficiency and secondary pollution in traditional SO2 capture technology, and achieves the It has efficient and economical SO2 adsorption and separation effects.

CN118772438BActive Publication Date: 2024-11-22DEZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411244191.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Traditional SO2 capture technology uses irreversible acid-base reactions, has low separation efficiency, high regeneration energy consumption, and the production of secondary pollutants. It requires an economical, energy-saving, and reversible adsorption and separation process to capture sulfur dioxide.

Method used

A MOF material based on trifluoromethyl tricarboxylic acid was designed to form a stable porous frame structure through the assembly of new functionalized organic ligands and metal ions. The MOF material was prepared by solvothermal reaction, and combined with tetrafluoroboric acid to regulate acidity. A one-dimensional pore structure with high porosity and stability is formed to improve the adsorption and separation performance of SO2.

Benefits of technology

It realizes efficient and selective adsorption and separation of SO2, improves the chemical stability of MOF and the acid-base resistance environmental ability, ensures efficient performance in humid environments, and significantly improves SO2 separation in SO2/CO2/N2 mixed gases ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772438B_ABST
    Figure CN118772438B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of gas adsorption and separation technology, and particularly relates to a MOF material based on trifluoromethyltricarboxylic acid, a preparation method and SO2 separation application. The chemical formula of the MOF material is [Ni6(OH)6(NTBPC‑3CF3)2(BPY)3] n , and contains abundant trifluoromethyl functional groups, with a three-dimensional skeleton structure. c The MOF material has rhombic channels along the a-axis direction and rectangular channels along the crystallographic a and b-axis directions. The specific surface area is 1656.29 m2 / g, and the pore size distribution is mainly between 4.5 and 11 Å. The MOF material is suitable for the adsorption and separation of sulfur dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gas adsorption and separation, and particularly relates to a MOF material based on trifluoromethyltricarboxylic acid, a preparation method and SO2 separation application. Background Art

[0002] Global development relies heavily on the use of fossil fuels. In addition to carbon dioxide (10-15% concentration) and other gases, fossil fuel exhaust emissions from power plants and the transportation sector also contain sulfur dioxide (SO2) at levels of ~500 ppm. Sulfur dioxide is a primary pollutant that causes many health and environmental problems (such as acid rain) and produces secondary pollutants, so capturing sulfur dioxide in exhaust gases is critical. Traditional SO2 capture technology uses an acid-base reaction between a solid base and SO2, accompanied by a mixture of sulfites and carbonates to produce secondary pollution. The process uses an irreversible acid-base reaction, has low separation efficiency, and consumes a lot of regeneration energy. Therefore, there is an urgent need for an economical, energy-saving, and reversible adsorption separation process to capture sulfur dioxide from carbon dioxide.

[0003] Metal-organic framework (MOF) materials are porous materials assembled by metal ions or clusters and organic ligands through coordination bonds. MOF has the characteristics of diverse composition, customizable structure and high specific surface area. It has received extensive attention in the research and application of adsorption, separation, fluorescence and other fields, and has shown remarkable application prospects in the field of gas adsorption and separation. The rich and diverse structural types of organic ligands and the structural design at the molecular / atomic level are the key links in constructing MOFs with specific functions. Therefore, in the research field of MOF materials, the preparation of new functional MOFs based on the design and synthesis of new ligands is of great research significance and is a research hotspot in the development of new advanced porous materials. The present invention takes the design of new functional organic ligands as the starting point and uses crystal engineering strategies to prepare new porous MOFs for the capture and separation of SO2 gas. Summary of the invention

[0004] The first object of the present invention is to provide a MOF material based on trifluoromethyltricarboxylic acid, wherein the chemical formula of the MOF material is [Ni6(OH)6(NTBPC-3CF3)2(BPY)3] n The first ligand is 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid H3NTBPC-3CF3; the second ligand is 4,4'-bipyridine BPY. In the MOF structure, each Ni 2+ ions and one N atom from the BPY ligand and one from μThe O atom of 3-OH and four O atoms of carboxyl groups from different deprotonated NTBPC-3CF3 ligands are coordinated to form an octahedral configuration.

[0005] Furthermore, from the perspective of skeleton connection construction, the crystal structure of the MOF belongs to the hexagonal system, and the space group is P 63 / mcm , the unit cell parameters are: a = b =25.1031(4) Å, c= 26.4214(9) Å, α = β= 90 o , γ = 120 o .

[0006] Furthermore, in the MOF structure, the six adjacent Ni 2+ The ions are 6 μ 3-OH binds to form a hexanuclear Ni6O6 cluster; the carboxyl groups of the deprotonated NTBPC-3CF3 ligands μ 2- η 1 : η 1 The coordination mode connects Ni 2+ ions; each NTBPC-3CF3 ligand connects to 3 Ni6O6 clusters, and each Ni6O6 cluster connects to 6 NTBPC-3CF3 ligands to form a two-dimensional grid; the two-dimensional grid is supported by BPY ligands to form a three-dimensional framework structure; the three-dimensional framework structure has staggered one-dimensional channels, and trifluoromethyl functional groups are distributed on the pore walls and point to the channels. The porosity of the material is 69.6% calculated by PLATON software based on crystal data.

[0007] The present invention also provides a trifluoromethyl tricarboxylic acid ligand, wherein the trifluoromethyl tricarboxylic acid ligand is 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid H3NTBPC-3CF3, and the structural formula is:

[0008] ;

[0009] The three benzene rings on the outside of the ligand are respectively modified with trifluoromethyl functional groups, and the molecular structure of the ligand is C 3 symmetry, the three benzene rings connected to the central N atom of the ligand have a dihedral angle of 69.99 between each other o The dihedral angle between the two benzene rings of biphenyl is 83.78 o .

[0010] The present invention also provides a method for preparing the trifluoromethyltricarboxylic acid-based MOF material, comprising the following steps:

[0011] Under sealed conditions, organic ligands H3NTBPC-3CF3, BPY and Ni(NO3)2·6H2O were dissolved in a mixed solution of DMA and water, and 52wt% tetrafluoroboric acid aqueous solution was added to adjust the acidity of the solution, and the MOF crystals were obtained through a solvothermal reaction.

[0012] Further, the molar ratio of the H3NTBPC-3CF3 to BPY is 1:(1.5-2), and the molar ratio of the H3NTBPC-3CF3 to Ni(NO3)2·6H2O is 1:(3-4);

[0013] The amount of DMA added is 10 ml of DMA for every 0.1 mmol of H3NTBPC-3CF3;

[0014] The volume ratio of DMA to water in the mixed solution is 1:(0.5-0.75);

[0015] The temperature of the solvent thermal reaction is 100-110°C, and the reaction time is 16-36 hours;

[0016] The amount of tetrafluoroboric acid aqueous solution added was 40-50 μL of 52 wt % tetrafluoroboric acid aqueous solution per 0.01 mmol H3NTBPC-3CF3.

[0017] In the synthesis process of the MOF material, tetrafluoroboric acid is a non-coordinating acid, whose anions are large and spherical, and it is not easy to form coordination bonds with metal centers. In contrast, the anions of other acids may coordinate with metal ions, affecting the crystal structure and formation of MOF. The aqueous solution of tetrafluoroboric acid has strong acidity, but due to its non-coordinating nature, the acidity can be better utilized to regulate the synthesis of MOF without excessively affecting the chemical properties of the ligand or metal. The aqueous solution of tetrafluoroboric acid has good solubility in water and is relatively stable. It can provide a constant acidic environment during the reaction without causing complex side reactions, which helps to better control the growth process of MOF. Since tetrafluoroboric acid does not participate in coordination, it mainly affects the growth of MOF crystals by adjusting the pH value and ionic strength of the solution. This characteristic gives it certain advantages in controlling crystal size, morphology and phase change. Tetrafluoroboric acid is not easy to generate precipitation or other by-products, ensuring the purity of the reaction system, which is crucial for the synthesis of high-quality MOF crystals.

[0018] The present invention also provides a method for synthesizing the trifluoromethyltricarboxylic acid ligand, comprising the following steps:

[0019] S1, triphenylamine reacts with bromine to obtain tri-(4-bromophenyl)amine;

[0020] S2, add tris-(4-bromophenyl)amine, potassium carbonate, tetrakistriphenylphosphine palladium, 1,4-dioxane and water obtained in S1 into a reactor, seal, protect with nitrogen, heat to react, remove the solvent after the reaction stops, dissolve the residue in ethyl acetate, wash with ethyl acetate twice in sequence, dry with anhydrous Na2SO4, filter and concentrate; the crude product is purified by column chromatography to obtain 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester;

[0021] S3. Add 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester and 2M NaOH solution to a mixed solvent of tetrahydrofuran and methanol, and heat to reflux for reaction; after the reaction stops, remove the solvent by rotary evaporation; add hydrochloric acid aqueous solution to the remaining solid to acidify to pH = 3 to obtain a yellow precipitate, centrifuge the obtained precipitate, wash with water, and vacuum dry to obtain a yellow solid 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid;

[0022] The reaction equation is:

[0023]

[0024] In step S2, the first function of adding potassium carbonate is to activate boric acid. The base can convert the boric acid group in the aromatic boronic acid into a more active borate form, making it easier to coordinate with the palladium catalyst and then participate in the coupling reaction; the second function is to neutralize the by-products. During the reaction, the bromophenyl compound and the palladium catalyst react to generate palladium bromide and hydrohalic acid. The base can neutralize the generated hydrohalic acid to prevent it from inhibiting the activity of the palladium catalyst, thereby maintaining the efficiency of the catalyst; the third function is to promote reduction elimination. The presence of the base helps the last step of the palladium catalytic cycle, namely, reduction elimination. In this process, the two ligands on the palladium atom combine to form a new carbon-carbon bond, and the palladium is reduced and released into the reaction system to enter the next cycle.

[0025] Further, in step S2, the molar ratio of tri-(4-bromophenyl)amine and 4-methylformate-3-(trifluoromethyl)phenylboronic acid is 1:4.5, the molar ratio of Pd(PPh3)4 and tri-(4-bromophenyl)amine is 1:10, the molar ratio of K2CO3 and tri-(4-bromophenyl)amine is 6:1, the volume ratio of 1,4-dioxane and water is 4:1, and the reaction conditions of the heating reaction are 110°C for 48 hours.

[0026] Further, in step S3, the amount of the mixed solvent added is 120 mL of the mixed solvent per 5 mmol of 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester, the volume ratio of tetrahydrofuran and methanol is 1:1, and the amount of the 2M NaOH solution added is 60 mL of the 2M NaOH solution per 5 mmol of 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester.

[0027] The present invention also provides application of the MOF material in SO2 gas adsorption and separation.

[0028] Beneficial technical effects of the present invention:

[0029] (1) The present invention synthesizes a novel organic molecule 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid (H3NTBPC-3CF3). The H3NTBPC-3CF3 organic molecule has a novel structure and contains abundant trifluoromethyl functional groups. The trifluoromethyl group is a strong electron-attracting group that can stabilize the electronic structure of the ligand, thereby improving the stability of the entire MOF; the trifluoromethyl group has strong hydrophobicity and chemical inertness, which makes the MOF exhibit higher chemical stability in acidic, alkaline and other harsh chemical environments. This stability is very important for practical applications such as gas separation, catalysis and storage, ensuring that the MOF maintains structural integrity under operating conditions. The tricarboxylic acid ligand provides multiple coordination sites and can form a highly cross-linked three-dimensional structure with metal ions. This multi-coordination property makes it possible to precisely control the pore size and shape of the MOF to meet different application requirements. The biphenyl structure in the ligand increases the rigidity and linearity of the molecule, which helps to form a regular and stable pore structure. The rigid structure also prevents the frame from deforming under external pressure, maintaining the integrity of the channel.

[0030] (2) The present invention selects the compound 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid (H3NTBPC-3CF3) as a layered ligand and selects the compound 4,4-bipyridine as a columnar ligand, and constructs a columnar MOF by connecting with a metal cluster [Ni6(μ3-OH)6]. The columnar MOF has a novel structure and a stable framework.

[0031] (3) In the preparation method of the present invention, the above-mentioned columnar structure MOF crystal material is successfully synthesized by precisely controlling the ratio between the two ligands, the amount of solvent used, the reaction temperature, the reaction time and other experimental parameters. It has been verified that the above-mentioned crystal structure cannot be obtained if the above-mentioned reaction conditions are not met.

[0032] (4) By modifying the layer ligand 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid (H3NTBPC-3CF3) with trifluoromethyl, the adsorption performance of the resulting MOF for SO2 was significantly improved, and its ability to separate SO2 from a mixed gas of SO2 / CO2 / N2 / water vapor was enhanced. Adsorption experiments showed that the trifluoromethyl-modified MOF exhibited excellent SO2 selective adsorption and separation.

[0033] The trifluoromethyl group is a strongly hydrophobic group that can significantly change the chemical properties of the MOF pore surface. Since SO2 is a weakly polar gas, the interface with hydrophilic and non-polar structure helps to enhance the selective adsorption of SO2 by MOF, while repelling water molecules, thereby improving the adsorption performance of MOF in humid environments. The sulfur atoms and oxygen atoms in the SO2 molecule have special electronic properties, and the weak interactions (such as van der Waals forces) formed with the trifluoromethyl group can promote the enrichment of SO2 molecules on the pore surface. This mechanism of action will increase the selectivity of MOF for SO2, thereby improving the gas separation performance.

[0034] In summary, the organic ligand molecule of the present invention has a novel structure and contains abundant trifluoromethyl functional groups. The MOF material prepared based on the ligand molecule has a unique pore structure and a stable framework. c The diamond-shaped channels along the a-axis direction and the rectangular channels along the crystallographic a and b-axis directions. The specific surface area is 1656.29 m2 / g, and the pore size distribution is mainly between 4.5 and 11 Å. This permanent channel and suitable pore size make the metal-organic framework suitable for the adsorption and separation of sulfur dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the H NMR spectrum of 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid ligand.

[0036] Figure 2 This is a crystal photograph of the MOF material prepared in Example 1.

[0037] Figure 3 Coordination environment diagram of Ni metal center in MOF material.

[0038] Figure 4 This is a schematic diagram of the three-dimensional framework construction of MOF materials.

[0039] Figure 5 XRD characterization spectra of MOF materials and after treatment under different conditions.

[0040] Figure 6 The 77 K nitrogen isotherm adsorption-desorption curve and pore size distribution diagram of MOF material.

[0041] Figure 7 This is the isothermal adsorption curve of SO2 and CO2 of MOF material at 15 ℃.

[0042] Figure 8 This is the isothermal adsorption curve of SO2 and CO2 of MOF material at 25 °C.

[0043] Fig. 9 Schematic diagram of the dynamic breakthrough curve of MOF material for SO2 mixed gas at 25 ℃.

[0044] Fig.10 Schematic diagram of the dynamic breakthrough curve of MOF material to SO2 mixed gas at 50% humidity.

[0045] Fig.11 Schematic diagram of the IAST selectivity of MOF materials for SO2 and CO2.

[0046] Fig.12 Schematic diagram of the adsorption heat of SO2 and CO2 on MOF materials.

[0047] Fig.13 A diagram of mixed gas penetration cycle test for MOF materials. DETAILED DESCRIPTION

[0048] The present invention will be further described below in conjunction with examples, but the present invention is not limited to the following examples.

[0049] Example 1 Synthesis of ligand

[0050] First, triphenylamine reacts with halogen Br to obtain tri-(4-bromophenyl)amine; 4.82 g (10 mmol) tri-(4-bromophenyl)amine, 11.16 g (45 mmol) 4-methylformate-3-(trifluoromethyl)phenylboronic acid, 8.29 g (60 mmol) K2CO3, 1.16 g (1 mmol) Pd(PPh3)4, 120 mL 1,4-dioxane and 30 mL deionized water are added to a 500 mL three-necked flask, sealed, nitrogen protected, and reacted at 110 ° C for 48 hours. After the reaction stops, the solvent is removed, and the residue is dissolved in 200 mL ethyl acetate, washed twice with 200 mL water and brine respectively, dried over anhydrous Na2SO4, filtered and concentrated. The crude product was purified by column chromatography (petroleum ether:ethyl acetate) to give methyl 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylate.

[0051] 4.05 g (5 mmol) of methyl 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylate and 60 mL of 2 M NaOH solution were added to a mixed solvent of 60 mL of tetrahydrofuran and 60 mL of methanol and stirred at 75 °C for 24 h. After cooling to room temperature, the organic solvent was removed in vacuo. The remaining solution was acidified to pH = 3 with hydrochloric acid to obtain a yellow precipitate. The obtained precipitate was centrifuged, washed with water, and dried in vacuo at 60 °C to obtain a yellow solid 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid with a yield of 75%.

[0052] The H NMR spectrum of the ligand 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid prepared in Example 1 is as follows: Figure 1 As shown, it is proved that the above ligand was successfully synthesized with high purity.

[0053] Example 2

[0054] The organic ligand H3NTBPC-3CF3 (0.01 mmoL) and BPY (0.015 mmoL) synthesized in Example 1 were ultrasonically dissolved in 1 mL of DMA, and Ni(NO3)3⋅6H2O (0.03 mmoL) was dissolved in 0.5 mL of deionized water. After the two were mixed, 50 microliters of tetrafluoroboric acid aqueous solution (52wt%) were added and sealed in a pressure-resistant glass bottle. After the thermal reaction at 100 °C for 36 hours, the MOF crystal material was activated after the reaction. The obtained crystal photo is shown in the figure. Figure 2 As shown, the obtained crystal is green in color and has a hexagonal prism shape.

[0055] Example 3

[0056] The organic ligand H3NTBPC-3CF3 (0.2 mmol) and BPY (0.4 mmol) synthesized in Example 1 were ultrasonically dissolved in 20 mL of DMA, and Ni(NO3)3⋅6H2O (0.8 mmol) was dissolved in 15 mL of deionized water. After the two were mixed, 800 microliters of tetrafluoroboric acid aqueous solution (52wt%) were added and sealed in a pressure-resistant glass bottle. The MOF crystal material was obtained by thermal reaction at 110°C for 16 hours and activation after the reaction.

[0057] The test results of the product obtained in the above Example 2 are the same, as shown below:

[0058] (1) Crystal structure determination:

[0059] Single crystals of appropriate size were selected under a microscope, and data were collected on a Rigaku Oxford diffractometer. The crystal structure was solved by direct method using the ShelXT-2019 program. The coordinates of all non-hydrogen atoms were first determined using the difference function method and the least squares method, and the positions of hydrogen atoms were obtained using the theoretical hydrogenation method. Then, the crystal structure was refined using ShelXL. See the structure diagram for details. Figure 3 and Figure 4 The crystallographic data are shown in Table 1.

[0060] Table 1 shows the crystallographic data

[0061]

[0062] Figure 3 The structural diagram shows that in the MOF structure, the Ni metal center and atom and a N atom from the BPY ligand and a μ The O atom of 3-OH and four O atoms of carboxyl groups from different NTBPC-3CF3 ligands are coordinated to form an octahedral configuration.

[0063] Figure 4 The MOF structure composition diagram shows that there are 6 metal nodes μ 3-OH binds to six adjacent Ni atoms to form a hexanuclear Ni6O6 cluster. Each NTBPC-3CF3 ligand connects to three Ni6O6 clusters, and each Ni6O6 cluster connects to six NTBPC-3CF3 ligands, forming a two-dimensional grid. The two-dimensional grid is supported by BPY ligands to form a three-dimensional framework structure. The porous framework has staggered one-dimensional channels, and trifluoromethyl functional groups are distributed on the pore walls and point to the channels.

[0064] Figure 5 The X-ray powder diffraction spectrum of the obtained MOF material shows that the prepared MOF crystal material is pure phase, and the crystal skeleton structure of the sample remains unchanged after ethanol activation treatment, gas separation and circulation experiment, indicating that the material has good chemical stability. The trifluoromethyl group is a strong electron-attracting group that can stabilize the electronic structure of the ligand, and the trifluoromethyl group has strong hydrophobicity and chemical inertness, thereby improving the stability of the entire MOF.

[0065] (2) Characterization of gas adsorption and separation performance:

[0066] Figure 6 The MOF material prepared in Example 2 is / Nitrogen adsorption isotherms under P0=1 and 77 K. As can be seen from the figure, the maximum N2 adsorption of the crystalline material is 622.2 cm 3 / g, and the specific surface areas (BET) calculated based on N2 adsorption data are 1656.29 m2 / g, and the pore size distribution is mainly between 0.45 nm and 1.5 nm.

[0067] Figure 7 and 8 is the adsorption isotherm of SO2 and CO2 of MOF materials at 15 ℃ and 25 ℃. It can be seen from the figure that under the conditions of 288 K and 100 kPa, the saturation absorption capacity of MOF materials for CO2 and SO2 is 28.50 cm 3 / g, 285.96 cm 3 / g, and the maximum absorption capacity of CO2 and SO2 at 298 K and 100 kPa is 21.48 cm 3 / g, 295.08 cm 3 / g. This indicates that the material has a higher adsorption performance for SO2 than CO2.

[0068] Fig. 9 The figure is a schematic diagram of the dynamic breakthrough curve of MOF material to SO2 mixed gas at 25 °C. At 298 K and 1 bar, SO2 / CO2 mixed gas (SO2 / CO2 / N2, v:v:v=0.2 / 50 / 49.8, SO2: 2000 ppm) was heated at 100 mL min −1 The flow rate passed through the quartz tube containing 0.4g of the MOF material. From the penetration curve, it can be seen that CO2 first passed through the MOF material, and SO2 gas molecules were detected after a certain interval. The penetration time difference of the mixed gas in the MOF material was 26.5 minutes. Fig.10 The figure is a schematic diagram of the dynamic breakthrough curve of the MOF material for SO2 mixed gas at 50% humidity. It can be seen that even at 50% humidity, the performance of the MOF material in capturing and separating SO2 is not affected, and the penetration time of SO2 increases to 30.5 minutes. The penetration test results show that the MOF material still has the potential for capturing and separating SO2 in actual environments even at higher humidity.

[0069] Fig.11 Schematic diagram of IAST selectivity of MOF materials for SO2 and CO2. Under the conditions of 298 K and 100 kPa, the adsorption selectivity calculated by IAST (ideal adsorption solution theory) is 1.9~11.6. Both the adsorption isotherm and the theoretical selectivity show that in porous MOF materials, ligands containing -CF3 functional groups are conducive to the adsorption of SO2 and the selective adsorption and separation of SO2.

[0070] Fig.12 is the adsorption heat curve of MOF material for sulfur dioxide and carbon dioxide. In the porous coordination polymer crystal material, the Q of SO2 stThe value is 47.8 kJ / mol, which is higher than the corresponding 37.5 kJ / mol of CO2. These calculation results mean that the synthesized MOF material has a stronger affinity for SO2 than CO2.

[0071] Fig.13 The breakthrough curve of MOF material for five consecutive cycles of separation of mixed gas containing SO2. The conditions of each breakthrough experiment were the same. Between each cycle, the sample was regenerated under the conditions of heating at 80 °C with 100 mL min −1 The nitrogen was purged for 2 hours. From the breakthrough curve, it can be seen that there is no significant difference in the effect of the porous coordination polymer crystal material in separating the SO2 / CO2 mixed gas for three consecutive times, indicating that the material has stable cyclic performance.

[0072] In summary, the trifluoromethyl functional group in the ligand plays a multi-faceted positive role in the adsorption and separation of sulfur dioxide gas by MOF. By enhancing the hydrophobicity of MOF, adjusting electronic properties, optimizing pore structure and improving chemical stability, the trifluoromethyl group significantly improves the selective adsorption capacity of MOF for SO2. In addition, the introduction of the trifluoromethyl group helps to reduce the interference of water molecules and ensure high efficiency in practical applications. These advantages make ligands containing trifluoromethyl an ideal choice for the synthesis of efficient SO2 adsorption and separation MOF.

Claims

1. A MOF material based on trifluoromethyltricarboxylic acid, characterized in that: The chemical formula of the MOF material is [Ni6(OH)6(NTBPC-3CF3)2(BPY)3] n The first ligand is 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid H3NTBPC-3CF3; The structural formula is: ; The second ligand is 4,4'-bipyridine BPY; In the MOF structure, each Ni 2+ The ion is coordinated with one N atom from the BPY ligand, one O atom from μ3-OH, and four O atoms from the carboxyl groups of the NTBPC-3CF3 ligands with different deprotonations to form an octahedral configuration; From the perspective of skeleton connection construction, the crystal structure of the MOF material belongs to the hexagonal system, the space group is P63 / mcm, and the unit cell parameters are: a = b = 25.1031(4) Å, c = 26.4214(9) Å, α = β = 90 o , γ = 120 o ; In the MOF structure, the six adjacent Ni 2+ The ions are bound by 6 μ3-OH groups to form a hexanuclear Ni6O6 cluster; the carboxyl groups of the deprotonated NTBPC-3CF3 ligands are bound by μ 2- η 1 :η 1 The coordination mode connects Ni 2+ ions; each NTBPC-3CF3 ligand is connected to 3 Ni6O6 clusters, and each Ni6O6 cluster is connected to 6 NTBPC-3CF3 ligands to form a two-dimensional grid; the two-dimensional grid is supported by BPY ligands to form a three-dimensional framework structure; the three-dimensional framework structure has staggered one-dimensional channels, and trifluoromethyl functional groups are distributed on the pore walls and point to the channels; The three benzene rings on the outside of the 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid ligand are modified with trifluoromethyl functional groups respectively, and the molecular structure of the ligand is C3 symmetric. The three benzene rings connected to the central N atom of the ligand have a dihedral angle of 69.99 between each other. o The dihedral angle between the two benzene rings of biphenyl is 83.78 o .

2. The MOF material based on trifluoromethyltricarboxylic acid according to claim 1, characterized in that: The synthesis method of the 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid ligand comprises the following steps: S1, triphenylamine reacts with bromine to obtain tri-(4-bromophenyl)amine; S2, add tris-(4-bromophenyl)amine, potassium carbonate, tetrakistriphenylphosphine palladium, 1,4-dioxane and water obtained in S1 into a reactor, seal, protect with nitrogen, heat to react, remove the solvent after the reaction stops, dissolve the residue in ethyl acetate, wash with ethyl acetate twice in sequence, dry with anhydrous Na2SO4, filter and concentrate; the crude product is purified by column chromatography to obtain 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester; S3. Add 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester and 2M NaOH solution to a mixed solvent of tetrahydrofuran and methanol, and heat to reflux for reaction; after the reaction stops, remove the solvent by rotary evaporation; add aqueous hydrochloric acid to the remaining solid to acidify to pH = 3 to obtain a yellow precipitate, centrifuge the obtained precipitate, wash with water, and vacuum dry to obtain a yellow solid 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid.

3. The MOF material based on trifluoromethyltricarboxylic acid according to claim 2, characterized in that: In step S2, the molar ratio of tris-(4-bromophenyl)amine to 4-methylformate-3-(trifluoromethyl)phenylboronic acid is 1:4.5, the molar ratio of tetrakistriphenylphosphine palladium to tris-(4-bromophenyl)amine is 1:10, the molar ratio of potassium carbonate to tris-(4-bromophenyl)amine is 6:1, the volume ratio of 1,4-dioxane to water is 4:1, and the reaction conditions of the heating reaction are 110° C. for 48 hours; In step S3, the amount of the mixed solvent added is 120 mL of the mixed solvent per 5 mmol of 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester, the volume ratio of tetrahydrofuran to methanol is 1:1, and the amount of the 2M NaOH solution added is 60 mL of the 2M NaOH solution per 5 mmol of 4,4'4''-nitrilotris(2-trifluoromethyl-(1,1-biphenyl))-4-carboxylic acid methyl ester.

4. A method for preparing a MOF material based on trifluoromethyltricarboxylic acid as claimed in any one of claims 1 to 3, characterized in that: The steps include: Under sealed conditions, organic ligands H3NTBPC-3CF3, BPY and Ni(NO3)2·6H2O were dissolved in a mixed solution of DMA and water, and 52wt% tetrafluoroboric acid aqueous solution was added to adjust the acidity of the solution, and the MOF crystals were obtained through a solvothermal reaction.

5. The method for preparing a MOF material based on trifluoromethyltricarboxylic acid according to claim 4, characterized in that: The molar ratio of the H3NTBPC-3CF3 to BPY is 1:(1.5-2), and the molar ratio of the H3NTBPC-3CF3 to Ni(NO3)2·6H2O is 1:(3-4); The amount of DMA added was limited to 10 ml of DMA per 0.1 mmol of H3NTBPC-3CF3; The volume ratio of DMA to water in the mixed solution is 1:(0.5-0.75); The temperature of the solvent thermal reaction is 100-110°C, and the reaction time is 16-36 hours; The amount of tetrafluoroboric acid aqueous solution added is limited to 40-50 microliters of 52 wt% tetrafluoroboric acid aqueous solution per 0.01 mmol H3NTBPC-3CF3.

6. Use of the trifluoromethyltricarboxylic acid-based MOF material as claimed in any one of claims 1 to 3 in SO2 gas adsorption and separation.