Preparation and application of polysaccharide polymer film with high water vapor barrier property

By introducing carboxyl and hydroxyl groups into the polysaccharide polymer film, and using polycarboxylic acid synergistic induced crystallization technology, combined with acid-assisted gelling and cyclic freeze-thaw processes, the problem of insufficient water vapor barrier performance of the degradable polymer-based barrier film was solved. problem, achieving efficient, environmentally friendly water vapor barrier and improved mechanical strength.

CN118772460AInactive Publication Date: 2024-10-15NANJING FORESTRY UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410985789.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing degradable polymer-based barrier films have deficiencies in water vapor barrier properties, the preparation process is complex and costly, and may pose a threat to the environment and human health.

Method used

A method for preparing polysaccharide polymer films with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids is adopted. By coexisting carboxyl and hydroxyl groups on a single polysaccharide polymer and mixing them with polycarboxylic acids, acids are used to assist gelation and circulation. The freeze-thaw process prepares polysaccharide polymer films with high water vapor barrier properties.

Benefits of technology

The water vapor barrier performance and mechanical strength of the polysaccharide polymer film are significantly improved. The preparation process is simple, environmentally friendly, and low cost. The resulting film has good practicality and water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772460A_ABST
    Figure CN118772460A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a polysaccharide polymer film with high water vapor barrier property based on polycarboxylic acid synergistic induced crystallization. The method comprises the following steps: firstly, preparing a polysaccharide polymer-based aqueous solution of a carboxyl and hydroxyl coexistence system; the step comprises two different systems: one system is that hydroxyl and substituted carboxyl exist on a single polysaccharide polymer at the same time, and the other system is a mixed solution of polycarboxylate and polysaccharide polymer. And next, taking the aqueous solution obtained in the first step as a precursor solution, and finally preparing the polysaccharide polymer film with high water vapor barrier property by adopting an acid-assisted gel method and a circulating freeze-thawing method. Based on the theoretical research of correlation between high crystallinity and water vapor permeability, the invention proposes that carboxyl and hydroxyl coexist to synergistically induce hydrogen bond crystallization of polysaccharide molecules by adopting an ion specific effect, acid-assisted gel and a circulating freezing and thawing process, so that the water vapor barrier property and the mechanical strength property of the polysaccharide polymer are remarkably improved. And the preparation method and materials are simple, easy to manufacture and environmentally friendly, and the preparation process is quantitatively designed, regulated and optimized, so that the prepared degradable polymer-based thin film with the high water vapor barrier property has good practicability and has wide application prospects in the field of barrier packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of barrier films, and in particular to a preparation method and application of a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids. Background Art

[0002] Packaging plays a vital role in protecting food, medicine, and electronics from environmental influences and pollution, extending their shelf life, and reducing losses and waste. Packaging materials need to have low water vapor transmission rate (WVTR) and oxygen transmission rate (OTR), as well as excellent water and grease barrier properties. However, polymer-based packaging materials generally have a dense pore structure, so they usually have high grease barrier properties. Therefore, the most important thing for polymer-based packaging materials is to improve their water, water vapor and oxygen barrier properties. At present, petrochemical polymers are widely used in the packaging field due to their advantages such as light weight, easy processing, good mechanical properties and high barrier properties. However, petroleum resources are non-renewable resources, and most petroleum-based polymers are difficult to degrade, easily causing white pollution, leading to serious environmental problems (Kim D, Seo J. Trends in Food Science & Technology, 2018, 76: 15-27.). Therefore, compared with the non-degradability and limited oxygen barrier properties of traditional petroleum-based materials, biomass materials that are green, environmentally friendly, widely available and have good oxygen barrier properties are gradually becoming alternatives to traditional petroleum-based polymers, which is the key to achieving sustainable development.

[0003] Petroleum resources are non-renewable resources, and most petroleum-based polymers are difficult to degrade, which can easily cause white pollution and lead to serious environmental problems. Degradable polymer-based barrier films have the advantages of wide sources, green environmental protection, and good oxygen barrier properties, which make them have a wide range of application scenarios in the field of barrier packaging. Common degradable polymers can be divided into two categories: one is bio-based degradable polymers, such as cellulose and its derivative compounds, chitosan, starch, alginate, etc.; the other is polymers from other sources but degradable, such as polyvinyl alcohol (PVA), etc. For the above-mentioned degradable polymers, due to their inherent hydrophilicity, their water vapor barrier properties are poor, so more research is currently focused on improving the water vapor barrier properties of degradable polymers. For example, Sanos et al. used CNF and CNC to enhance the water vapor barrier properties of CMC, and the WVTR of the composite film was as low as 3.38g / m 2·day (Fernández-Santos J, Valls C, Cusola O, et al. International Journal of Biological Macromolecules, 2022, 211: 218-229.). Tamer et al. used citric acid to cross-link HEC and chitosan (CS), which significantly improved the water vapor barrier properties of the film, with a water vapor permeability coefficient (WVP) as low as 1.24×l0 -11 g·cm / (cm 2 ·s·Pa)( Tamer Y. Polymer-Plastics Technology and Materials, 2023, 62(9): 1138-1156.). Choi et al. used various crosslinking agents (CaCl2), FeCl2, FeCl3 and FeSO4 to develop alginate films based on ionic crosslinking, focusing on cations of different valence states (Ca 2+ , Fe 2+ and Fe 3 + ) and anions (Cl and SO4 2- ) on the water vapor barrier properties of the film. Studies have shown that the WVP of FeSO4 cross-linked film is the lowest (Choi I, Lee Y, Lyu JS, et al. Food Hydrocolloids, 2022, 131: 107785.). Although these methods significantly improve the water resistance of degradable polymer films, there are still problems such as complex preparation process, high cost, environmental hazards and possible harm to the human body. Therefore, it is necessary to find a green and environmentally friendly natural material to improve the water resistance and barrier properties of polysaccharide polymer films through a simple preparation process. Summary of the invention

[0004] The present invention aims at the deficiencies in the prior art and provides a method for preparing a polysaccharide polymer film with high water vapor barrier properties based on polycarboxylic acid synergistic induced crystallization and its application. The method has a simple preparation process, uses environmentally friendly and economical raw materials for preparation, and the prepared polysaccharide polymer film with high water vapor barrier properties has a dense internal structure, high water resistance, and excellent water vapor barrier properties and mechanical properties.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] On the one hand, a method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids is adopted, characterized in that it comprises the following steps:

[0007] Step 1: Prepare a polymer aqueous solution of a carboxyl and hydroxyl coexisting system, including two systems in which hydroxyl and substituted carboxyl groups coexist on a single polysaccharide polymer and a mixed solution of a polycarboxylic acid and a polysaccharide polymer.

[0008] Step 2: Using the aqueous solution obtained in step 1 as a raw material, a polysaccharide polymer film with high water vapor barrier properties is prepared by using an acid-assisted gelation and a freeze-thaw cycle method.

[0009] Furthermore, in step one, the method for preparing a high water vapor barrier polysaccharide polymer film based on the synergistic induced crystallization of polycarboxylic acids is characterized in that, in step one, the single polysaccharide polymer having both carboxyl and hydroxyl groups is one of carboxymethyl cellulose, carboxymethyl starch, carboxymethyl chitosan, alginic acid, hyaluronic acid, etc.; in step one, the mixed solution containing polycarboxylic acids and polysaccharide polymers, the polycarboxylic acid of which is one of citric acid, butane tetraacetic acid, oligomaleic acid, polyacrylic acid, polymethacrylic acid, etc., and the polysaccharide polymer is one of water-soluble cellulose derivatives (such as methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, cyanoethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose), water-soluble chitosan derivatives, water-soluble starch derivatives, etc.

[0010] Furthermore, in step 1, the molecular weight of the polysaccharide is in the range of 50,000 to 1,500,000; the molecular weight of polyacrylic acid and polymethacrylic acid is in the range of 3 to 500,000.

[0011] Furthermore, in step one, the concentration range of the single polysaccharide molecule solution containing both carboxyl and hydroxyl groups is 1 to 5 wt%, and the degree of substitution of carboxyl groups in the polysaccharide molecules is 0.1 to 2.5; the total concentration range of the mixed solution of polycarboxylic acid and polysaccharide polymer is 1 to 5 wt%, and the mass ratio of polycarboxylic acid to polysaccharide molecules is 5:95 to 50:50.

[0012] Furthermore, in step 2, the acid is one of sulfuric acid, phosphoric acid, and hydrochloric acid, and the concentration range is 0.5 to 4 mol / L. The actual acid concentration in the polysaccharide molecule solution is controlled to be in the range of 0.035 to 0.14 mol / L by adjusting the addition amount, and stirring is performed for 1 to 2 hours.

[0013] Furthermore, in step 2, the solution casting method used to form the film is uniformly cast at room temperature, and the absolute dry mass per unit area is in the range of 50g / m 2 .

[0014] Furthermore, in step 2, the polymer is induced to crystallize by repeatedly squeezing ice crystals during the freeze-thaw cycle to promote the rearrangement of the polymer molecular chains, the freeze-thaw cycle temperature range is -15 to -30°C, the freezing time is 4 to 16 hours, and the thawing time is 1 to 4 hours at room temperature, which is repeated 2 to 6 times. After the gel is formed, it is washed in pure water for 3 to 5 times, and then dried at 50 to 60°C to form a film.

[0015] Furthermore, the polysaccharide polymer film contains both carboxyl groups and hydroxyl groups, which, combined with the rigid skeleton of the polysaccharide molecules themselves, can improve the mechanical strength and water resistance of the film.

[0016] Furthermore, the water vapor permeability coefficient of the polysaccharide polymer film is in the range of 2.0 to 50.0×10 -11 g m / m 2 ·Pa·s, wet tensile strength ranges from 2 to 15MPa after soaking in water for two months.

[0017] The beneficial effects of the present invention are:

[0018] (1) Based on theoretical research on the correlation between high crystallinity and water vapor permeability, the coexistence of carboxyl and hydroxyl groups synergistically induced hydrogen bond crystallization of polysaccharide molecules by using ion-specific effects, acid-assisted gelation, and cyclic freeze-thaw processes, which significantly improved the water vapor barrier properties and mechanical strength properties of polysaccharide polymers.

[0019] (2) The water vapor barrier and mechanical strength properties of polysaccharide polymer films prepared by acid-assisted gelation and cyclic freeze-thaw method vary with the raw material composition and preparation conditions. The water vapor barrier property of the representative hydroxyethyl cellulose / sodium polyacrylate composite film can be as low as 2.5×10 -11 g m / m 2 ·Pa·s or less (T=37℃ and RH=65%), the maximum dry and wet tensile strengths can reach 45MPa and 14MPa or more respectively.

[0020] (3) The raw materials and preparation method used in the present invention are simple and green and environmentally friendly. The preparation process has been quantitatively designed, regulated and optimized, so that the prepared polysaccharide polymer film with high water vapor barrier performance has good practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the water vapor permeability coefficient test of the film, (a) water vapor permeability coefficient of different samples; (b) water vapor permeability coefficient of different acids; (c) water vapor permeability coefficient prepared under different freezing temperature conditions.

[0022] Figure 2 (a) Dry tensile strength of different samples; (b) Wet tensile strength of different samples;

[0023] Figure 3 SEM images of the surface and cross-section after freeze-thaw treatment without acid addition, freeze-thaw treatment without acid addition, and freeze-thaw treatment with acid addition.

[0024] Figure 4 The water vapor barrier properties of different films: (a) water vapor permeability coefficients of different films in their original state, freeze-thaw without acid addition, and freeze-thaw with acid addition; (b) water vapor permeability coefficients of films with different ratios of hydroxyethyl cellulose (HEC) / sodium polyacrylate (PAANa); (c) and (d) water vapor permeability coefficients of carboxymethyl cellulose (CMC) films with different molecular weights and degrees of substitution before and after acid-assisted gelation / cyclic freeze-thaw.

[0025] Figure 5 are the water contact angles of different samples: (a) untreated sample; (b) sample after acid-assisted gelation and cyclic freeze-thaw treatment.

[0026] Figure 6 (a) Dry tensile strength of different samples; (b) Wet tensile strength of different samples; (c) Appearance and load-bearing capacity of FT-CMC after immersion in water for two months.

[0027] Figure 7 SEM images of the surface and cross-section of different samples before and after acid-assisted gelation and cyclic freeze-thaw treatment: Surface SEM image of the samples before and after acid-assisted gelation and cyclic freeze-thaw treatment (a) hydroxyethyl cellulose (HEC); (b) sodium polyacrylate (PAANa); (c) HEC / PAANa; (d) carboxymethyl cellulose (CMC); SEM image of the cross-section without treatment (e) HEC; (f) PAANa; (g) HEC / PAANa; (h) CMC; Surface SEM image of the samples after acid-assisted gelation and cyclic freeze-thaw treatment (a′) FT-HEC; (b′) FT-PAANa; (c′) FT-HEC / PAANa; (d′) FT-CMC; SEM image of the cross-section after acid-assisted gelation and cyclic freeze-thaw treatment (e′) FT-HEC; (f) FT-PAANa; (g′) FT-HEC / PAANa; (h′) FT-CMC.

[0028] Figure 8 These are the XRD curves of different samples without treatment and after acid-assisted gelation-cycle freeze-thaw. DETAILED DESCRIPTION

[0029] The present invention will be described in detail below with reference to the accompanying drawings.

[0030] In Example 1, the present invention provides a method for preparing a sodium alginate barrier film with high water vapor barrier performance in which carboxyl groups and hydroxyl groups exist simultaneously on a single polysaccharide polymer, comprising the following steps:

[0031] Preparation of sodium alginate (SA) film: First, prepare a 2wt% SA aqueous solution at 50°C, cool it to room temperature, add 15g of 2wt% SA solution to a 50ml beaker, add 1.15mL of 2.0mol / LH2SO4 to the beaker and stir for 1h, then pour it into a 8.5cm diameter petri dish to make a hydrogel. The hydrogel was subjected to three freeze-thaw cycles (freezing at -20°C for 8h, thawing at room temperature for 3h), washed three times with deionized water, and dried at 55°C for 5h to obtain a flexible and transparent SA film, which was recorded as FT-A-SAm.

[0032] At room temperature, 15 g of SA solution (2.0 wt%) was poured into a plastic petri dish, spread evenly and dried at 55 °C for 5 h to obtain a soluble sodium alginate film without freeze-thaw (FT) treatment or acid addition, which was recorded as SAm, and without acid addition and only FT treatment was recorded as FT-SAm.

[0033] The water vapor permeability coefficient of the above film was measured using a water vapor transmission rate measuring instrument (UAS, MOCON) according to the test standard ASTM-F1249 to evaluate the water vapor barrier performance of the film. Figure 1 As shown in the figure, the water vapor barrier properties of various sodium alginate films were compared and it was found that the water vapor barrier properties of FT-A-SAm film were significantly improved after acid-assisted gelation and cyclic freeze-thaw treatment, and the water vapor permeability coefficient (WVP) could be as low as 4.99×10 -11 g m / m 2 ·Pa·s. The water vapor barrier properties of the films under different acids and temperatures were also studied.

[0034] Wet tensile properties of different films were measured to verify their water resistance, e.g. Figure 2 As shown. The FT-A-SAm film has a wet tensile strength of up to 14.96 MPa, and can still maintain its complete appearance after being immersed in water for two months, and has excellent wet tensile properties.

[0035] Schematic diagram of surface and cross-sectional changes of high water vapor barrier film Figure 3 The surface morphology and cross-sectional morphology of the samples were detected by field emission scanning electron microscopy (FE-SEM, S-4800, Hitachi) and the microscopic morphology of the film was analyzed. It can be observed that the FT-A-SAm film formed a dense surface structure and a lamellar stacking structure appeared in the cross section.

[0036] In another embodiment 2, the present invention provides a method for preparing a hydroxyethyl cellulose (HEC) / sodium polyacrylate (PAANa) composite film with high water vapor barrier performance of a mixed system of polycarboxylic acid and polysaccharide polymers, comprising the following steps:

[0037] Preparation of hydroxyethyl cellulose (HEC) / sodium polyacrylate (PAANa) composite membranes: 15 g of 2.0 wt% HEC / PAANa mixed solution containing different HEC:PAANa ratios was prepared at room temperature and evenly spread on a plastic culture dish, and dried at 55°C for 5 h to obtain HEC / PAANa composite membranes without FT or acid treatment.

[0038] FT-HEC / PAANa membrane: Pour the mixed solutions of HEC / PAANa (2.0wt%) in different proportions into a Petri dish. Then pour the mixed PAANa solution into a Petri dish with a diameter of 8cm, cover it with a clean lid, and freeze it in a -17℃ refrigerator for 3h. Then add 1.15mL of H2SO4 (2.0mol / L) to 15mL of deionized water. Pour the sulfuric acid solution evenly on the frozen HEC / PAANa mixed solution. During its melting process, the sulfuric acid solution will evenly penetrate into the HEC / PAANa mixed solution and gradually form a HEC / PAANa hydrogel. Freeze the hydrogel at -20℃ in a refrigerator for 8h, and then thaw it at room temperature for 3h. Repeat the freeze-thaw process three times to obtain a stable HEC / PAANa hydrogel. After that, soak the hydrogel in deionized water for 5min, and repeat three times to remove excess acid. Finally, after the hydrogel was dried in a plastic petri dish in a forced air oven at 55 °C for 5 h, an insoluble and flexible transparent HEC / PAANa film was obtained, which was denoted as FT-HEC / PAANa.

[0039] The water vapor permeability coefficient of the above films was measured to evaluate the water vapor barrier properties of the films. Figure 4 As shown in the figure, the water vapor barrier properties of various films were compared and it was found that when the polymer film contained only hydroxyl groups (HEC), the water vapor barrier properties of the film did not change significantly regardless of whether acid was added and freeze-thaw cycles were performed. When carboxyl-containing polymers (PAANa) were introduced into the film, the water vapor permeability coefficient (WVP) of the film decreased significantly after acid-assisted gelation and freeze-thaw treatment, and the water vapor permeability coefficient (WVP) could be as low as 2.5×10 -11 g m / m 2 ·Pa·s.

[0040] Schematic diagram of water contact angle of different films Figure 5As shown. An optical contact angle tester (T200-Auto3Plus, Biolin, Sweden) was used to measure the water contact angle of the film in the air, and the contact angle data was taken for 300 seconds. The water contact angles of the treated original samples HEC, PAANa, HEC / PAANa, and CMC dropped rapidly within 300 seconds. The water contact angle of HEC is relatively high, but it drops to about 50° after 300 seconds, and it still has high hydrophilicity. However, after acid freeze-thaw treatment, only the films with coexistence of carboxyl and hydroxyl groups (such as HEC / PAANa composite films and CMC films) can still maintain a high water contact angle within 300 seconds.

[0041] Wet tensile properties of different films were measured to verify their water resistance, e.g. Figure 6 As shown. The polycarboxylic acid and polysaccharide polymer mixed system (HEC / PAANa) film has wet tensile strength. Its wet tensile strength can be in the range of 2 to 15MPa, and it can still maintain its complete appearance after being soaked in water for two months, and has excellent load-bearing capacity. A 50μm thick film can withstand a weight of 100g.

[0042] Schematic diagram of surface and cross-sectional changes of high water vapor barrier film Figure 7 The surface morphology and cross-sectional morphology of the samples were detected by field emission scanning electron microscopy (FE-SEM, S-4800, Hitachi) and the microscopic morphology of the film was analyzed. It can be observed that when carboxyl groups and hydroxyl groups coexist, the film forms a dense surface structure and a lamellar stacking structure appears in the cross section.

[0043] XRD analysis of different polymer films showed that Figure 8 From the figure, it can be observed that when the system contains only hydroxyl groups, the crystal structure and crystallinity do not change after acid-assisted gelation and cyclic freeze-thaw. When carboxyl groups are introduced, the main crystal peak of the film shifts and the crystallinity increases.

[0044] Preferably, in Examples 1 and 2, the concentrations of sodium alginate, hydroxyethyl cellulose and sodium polyacrylate may be 1 wt%, 2 wt%, 2.5 wt% or 3 wt%.

[0045] Preferably, in Examples 1 and 2, sulfuric acid can be replaced by hydrochloric acid or phosphoric acid.

[0046] Preferably, in Examples 1 and 2, the concentration of sulfuric acid is 1 mol / L, 1.5 mol / L or 2 mol / L.

[0047] Preferably, in embodiments 1 and 2, the freezing temperature of the freeze-thaw cycle can be -10°C, -20°C, -40°C.

[0048] Preferably, in embodiments 1 and 2, the freezing time of the freeze-thaw cycle is 4 h, 6 h, or 8 h.

[0049] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids, characterized in that: The steps include: Step 1: prepare a polysaccharide polymer-based aqueous solution in which carboxyl and hydroxyl groups coexist, including two systems in which hydroxyl groups and substituted carboxyl groups coexist on a single polysaccharide polymer and a mixed solution of a polycarboxylate and a polysaccharide polymer. Step 2: Using the aqueous solution system obtained in step 1 as a precursor solution, and utilizing acid-assisted gelation and cyclic freeze-thaw methods to prepare a polysaccharide polymer film with high water vapor barrier properties.

2. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on polycarboxylic acid synergistic induced crystallization according to claim 1, characterized in that: In step one, the single polysaccharide polymer having both carboxyl and hydroxyl groups is one of sodium carboxymethyl cellulose, sodium carboxymethyl starch, sodium carboxymethyl chitosan, sodium alginate, sodium hyaluronate, etc.; in step one, the mixed solution containing polycarboxylic acid and polysaccharide polymer, in which the polycarboxylate is one of sodium citrate, sodium oxalate, sodium succinate, sodium butane tetraacetate, oligomeric sodium maleate, sodium polyacrylate, sodium polymethacrylate, etc., and the polysaccharide polymer is one of water-soluble cellulose derivatives (such as methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, cyanoethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, etc.), water-soluble chitosan derivatives, water-soluble starch derivatives, etc.

3. According to claim 1, it is characterized in that The molecular weight of the polysaccharide is not higher than 90,000 to 1,500,000, and the degree of substitution of the carboxyl group is in the range of 0.1 to 2.5; the molecular weight of polyacrylic acid and polymethacrylic acid is not higher than 5,000,000.

4. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids according to claim 1, characterized in that: In step 1, the concentration range of the single polysaccharide molecule solution containing both carboxyl and hydroxyl groups is 1-5wt%; the total concentration range of the mixed solution of polycarboxylic acid and polysaccharide polymer is 1-5wt%, and the mass ratio of polycarboxylic acid to polysaccharide molecules is 5:95-50:

50.

5. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids according to claim 1, characterized in that: The acid described in step 2 is one of sulfuric acid, phosphoric acid and hydrochloric acid, and the concentration range is 0.5-4 mol / L. The actual acid concentration in the polysaccharide molecule solution is controlled to be 0.035-0.14 mol / L by adjusting the addition amount, and stirring for 1-2 hours.

6. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids according to claim 1, characterized in that: In the step 2, the film is formed by solution casting, and the film is uniformly cast at room temperature, and the absolute dry mass per unit area ranges from 30 to 80 g / m 2 .

7. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on polycarboxylic acid synergistic induced crystallization according to claim 1, characterized in that: In step 2, the polymer is induced to crystallize by repeatedly squeezing ice crystals during the freeze-thaw cycle to promote the rearrangement of the polymer molecular chains, the freeze-thaw cycle temperature range is -15 to -30°C, the freezing time is 4 to 16 hours, and the thawing time is 1 to 4 hours at room temperature, which is repeated 2 to 6 times. After the gel is formed, it is immersed in deionized water for 3 to 5 times and then dried at 40 to 70°C to form a film.

8. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids according to claim 1, characterized in that: The polysaccharide polymer film has strong hydrogen bonds between carboxyl and hydroxyl groups, and forms a dense and evenly distributed lamellar microcrystalline structure through acidification and cyclic freeze-thaw synergistic induction of crystallization, thereby improving the water resistance and mechanical strength of the film.

9. The method for preparing a polysaccharide polymer film with high water vapor barrier properties based on synergistically induced crystallization of polycarboxylic acids according to claim 1, characterized in that: The water vapor permeability coefficient of the polysaccharide polymer film is in the range of 2.0 to 50.0×10 -11 g m / m 2 ·Pa·s, the wet tensile strength ranges from 2 to 15MPa. After soaking in water for two months, the wet tensile strength remains basically stable (the decrease ratio does not exceed 10%).

Citation Information

Patent Citations

  • Method for producing hydrogels

    CN103917092A

  • Transparent gas barrier film materials and production method thereof

    CN104817710A

  • Carboxylated cellulose nanocrystal, intelligent film, preparation method and application

    CN115353568A

  • Method for manufacturing steam barrier film and steam barrier film

    JP2010184984A

  • Method for obtaining biopolymer films

    RU2766223C1