A modified polyester film for composite current collector and preparation method thereof
Through the combination of modified polyester film substrate and hyperbranched polyetherimide epoxy functional coating, the polyester film for composite fluid collection is solved in terms of high temperature resistance, corrosion resistance, flame retardancy and mechanical mechanical properties. The deficiencies have improved the adhesion to the metal layer and are suitable for lithium battery applications.
Patent Information
- Application Number
- CN202411280309.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing polyester films for composite fluid collection have shortcomings in high temperature resistance, corrosion resistance, flame retardancy and mechanical mechanical properties, especially poor adhesion to metals, which affects the energy density and safety of lithium batteries.
Modified polyester film substrate is used, including hydroxy modified PET resin, amino-containing hyperbranched liquid crystal polymer, 3,5-diamino-1,2,4-triazole, 2,2-bis[4- (4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, bis[4-(4-aminophenoxy)phenyl]-1,1,1, 3,3,3-hexafluoropropane, difluoropropane, triethylamine, ferrocene modified graphene fibers, compatibility agents, antioxidants and lubricants, film formation process through twin-screw extrusion and bidirectional stretching Prepare and apply a functional coating of hyperbranched polyetherimide epoxy on the surface.
It significantly improves the high temperature resistance, corrosion resistance, flame retardancy and mechanical properties of the modified polyester film, and at the same time enhances the adhesion to the metal layer, which is suitable for continuous large-scale production and has high promotion and application value.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of current collectors for lithium batteries, and in particular to a modified polyester film for composite current collectors and a preparation method thereof. Background Art
[0002] In recent years, with the new energy vehicles' attention to the safety and mileage of lithium-ion power batteries, the development of power batteries towards high energy density and high safety is an inevitable trend. In order to achieve these performance requirements, composite current collectors for lithium batteries have emerged. As a new type of material, the composite current collector has a multilayer structure, with a polymer film as the substrate in the middle and metal layers on both sides of the substrate. As one of the key components of the composite current collector, the performance of the polymer film directly determines the quality of the composite current collector, which in turn affects the energy density and safety of the lithium battery. It can be seen that it is particularly important to seek polymer films for composite current collectors with excellent comprehensive performance and performance stability.
[0003] Polyester is a general term for polymers obtained by polycondensation of polyols and polyacids, mainly referring to polyethylene terephthalate, which is a type of engineering plastic with excellent performance and wide application. It has good transparency, high gloss, good air tightness and fragrance retention, excellent mechanical properties, excellent heat resistance, cold resistance, chemical resistance and oil resistance. It is widely used in packaging, light industry, photosensitive materials, magnetic recording materials, agriculture and other fields, and in polymer films for composite current collectors. However, its resistivity is high, it is easy to generate static electricity, and its resistance to wet and hot aging, corrosion resistance, flame retardancy, high temperature resistance and adhesion to metal are poor. In order to improve the above properties, the usual practice is to add additives and fillers to ordinary polyester materials. However, due to compatibility issues, these additives and fillers are easy to seep out during the long-term use of the material, affecting the performance stability.
[0004] For example, the Chinese invention patent with the authorization announcement number CN115477833B discloses a modified polyester film, a preparation method, a composite current collector, an electrode sheet and its use. The modified polyester film includes the following raw materials in percentage by weight: 94.0%-99.2% polyester, 0.5%-3.0% bridging agent and 0.3%-3.0% auxiliary agent; the bridging agent includes one or more of diethylene glycol, polyethylene glycol, diglycerol, triglycerol, tetraglycerol, pentaglycerol, hexaglycerol, heptaglycerol, octaglycerol, nonaglycerol and decaglycerol. The modified polyester film provided by the application effectively improves the molecular weight and cross-linking degree of polyester, thereby improving the mechanical properties of the modified polyester film. Applying the modified polyester film to the composite current collector can reduce the defective rate caused by film breakage and improve the mechanical properties of the composite current collector. However, its flame retardancy, corrosion resistance and high temperature resistance still need to be further improved.
[0005] It can be seen that the art still needs a modified polyester film for composite current collector having good high temperature resistance, sufficient corrosion resistance, flame retardancy and mechanical properties, and good adhesion to metal, and a preparation method thereof. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a modified polyester film for a composite current collector having good high temperature resistance, sufficient corrosion resistance, flame retardancy and mechanical properties, and good adhesion to metal, and a preparation method thereof.
[0007] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a modified polyester film for a composite current collector, comprising a modified polyester film substrate and a functional coating coated on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 15-25 parts of amino-containing hyperbranched liquid crystal polymer, 3-5 parts of 3,5-diamino-1,2,4-triazole, 3-5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1-2 parts of triethylamine, 10-15 parts of ferrocene-modified graphene fiber, 1-3 parts of a compatibilizer, 0.8-1.2 parts of an antioxidant, and 1-1.5 parts of a lubricant.
[0008] Preferably, the preparation method of the hydroxy-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide, and tris(hydroxymethyl)aminomethanesulfonic acid into a reaction kettle equipped with a reflux device and containing dimethyl sulfoxide, stirring and reacting at 178-185° C. for 5-8 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying in a vacuum drying oven at 95-105° C. to constant weight to obtain a hydroxy-modified PET resin.
[0009] Preferably, the mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid, and dimethyl sulfoxide is 5:0.3:(0.4-0.6):(0.6-1):(15-25).
[0010] Preferably, the PET resin is at least one of China Xiamen Tenglong DSR TL-103 PET resin, Canada AcloCompounders produced PET008L resin, China Hainan Yisheng Petrochemical YS-W01 PET resin.
[0011] Preferably, the amino-containing hyperbranched liquid crystal polymer is prepared according to the method of Example 4 of the Chinese invention patent with authorization publication number CN114437493B.
[0012] Preferably, the preparation method of the ferrocene-modified graphene fiber comprises the following steps: dispersing the graphene fiber in an organic solvent, then adding a silane coupling agent KH560 thereto, stirring at 50-60°C for 3-5h, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 60-80°C for 4-6h, then removing the solvent by rotary evaporation, washing the crude product with ethanol, and finally drying it in a vacuum drying oven at 80-90°C to constant weight to obtain ferrocene-modified graphene fiber.
[0013] Preferably, the mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and 1,1'-diaminoferrocene is (3-5):(15-25):(0.3-0.5):0.3.
[0014] Preferably, the graphene fiber is a single-layer graphene fiber with an average diameter of 3-6 μm and a length of 1-3 mm.
[0015] Preferably, the organic solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone.
[0016] Preferably, the compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.
[0017] Preferably, the antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076.
[0018] Preferably, the lubricant is at least one of ethylene bisstearamide and butyl stearate.
[0019] Preferably, the functional coating is made of a hyperbranched polyetherimide epoxy compound.
[0020] Preferably, there is no special requirement for the source of the hyperbranched polyetherimide epoxy compound. In one embodiment of the present invention, the hyperbranched polyetherimide epoxy compound is prepared according to the method of Example 35 of Chinese invention patent with authorization publication number CN110951076B.
[0021] Preferably, the thickness of the modified polyester film substrate is 2-4 μm; and the thickness of the functional coating is 1 μm.
[0022] Another object of the present invention is to provide a method for preparing the modified polyester film for the composite current collector, comprising the following steps: after uniformly mixing the raw materials of the modified polyester film substrate by weight, adding them into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing the hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating it on the surface of the modified polyester film substrate, and then drying it at 100-110°C to constant weight to obtain a modified polyester film for the composite current collector.
[0023] Preferably, the extrusion temperature of the twin-screw extruder is 235-265°C.
[0024] Preferably, the stretching temperature of the biaxial stretching film-forming machine is 110-120° C., the stretching rate is 120-80 mm / s, the heat setting temperature is 220-240° C., and the stretching ratio is 4:1.
[0025] Preferably, the mass ratio of the hyperbranched polyetherimide epoxy compound to N-methylpyrrolidone is (1-2):1.
[0026] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0027] (1) The method for preparing the modified polyester film for the composite current collector disclosed in the present invention has simple process, convenient operation and control, low dependence on equipment, low energy consumption, high preparation efficiency and finished product qualification rate, is suitable for continuous large-scale production, and has high promotion and application value.
[0028] (2) The modified polyester film for composite current collector disclosed in the present invention comprises a modified polyester film substrate and a functional coating coated on the surface thereof, wherein the functional coating is made of a hyperbranched polyetherimide epoxy compound; through such a structural design, i.e., providing a functional coating between the current collector substrate and the metal layer, the adhesion performance between the polyester film and the metal layer can be improved; and the epoxy group in the functional coating can react with the hydroxyl group and the amino group in the molecular structure of the modified polyester film substrate to form an interpenetrating network structure, thereby effectively improving the comprehensive performance and performance stability of the prepared modified polyester film, so that it has good high temperature resistance, sufficient corrosion resistance, flame retardancy and mechanical properties.
[0029] (3) The modified polyester film for composite current collector disclosed in the present invention, the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 15-25 parts of amino-containing hyperbranched liquid crystal polymer, 3-5 parts of 3,5-diamino-1,2,4-triazole, 3-5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1-2 parts of triethylamine, 10-15 parts of ferrocene-modified graphene fiber, 1-3 parts of compatibilizer, 0.8-1.2 parts of antioxidant, and 1-1.5 parts of lubricant. Through the mutual cooperation between the raw materials, the product has good high temperature resistance, sufficient corrosion resistance, flame retardancy and mechanical properties, and good adhesion to metal. At the same time, the ester group, hyperbranched liquid crystal polymer, triazole, fluorinated phenyl ether and ferrocene structure introduced, under the multiple effects of electronic effect, steric effect and conjugation effect, make the above-mentioned properties of the manufactured product further improved.
[0030] (4) The modified polyester film for the composite current collector disclosed in the present invention, by modifying the PET resin with hydroxyl groups, can not only provide reaction sites for subsequent cross-linking and curing, but also improve its compatibility with other raw material components; by adding ferrocene-modified graphene fibers, not only the mechanical properties of the film can be improved, but also the conductivity and thermal stability can be improved. DETAILED DESCRIPTION
[0031] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0032] Example 1, a modified polyester film for a composite current collector, comprising a modified polyester film substrate and a functional coating applied on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 15 parts of amino-containing hyperbranched liquid crystal polymer, 3 parts of 3,5-diamino-1,2,4-triazole, 3 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1 part of triethylamine, 10 parts of ferrocene-modified graphene fiber, 1 part of compatibilizer, 0.8 part of antioxidant, and 1 part of lubricant.
[0033] The preparation method of the hydroxyl-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide and tris(hydroxymethyl)aminomethanesulfonic acid) into a reaction kettle with a reflux device and containing dimethyl sulfoxide, stirring and reacting at 178°C for 5 hours, then precipitating in water, washing the precipitated polymer with ethanol for 3 times, and finally drying in a vacuum drying oven at 95°C to constant weight to obtain a hydroxyl-modified PET resin; the mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid and dimethyl sulfoxide is 5:0.3:0.4:0.6:15; the PET resin is DSR TL-103 from Xiamen Tenglong, China PET resin; the amino-containing hyperbranched liquid crystal polymer is prepared according to the method of Example 4 of the Chinese invention patent with authorization announcement number CN114437493B; through elemental analysis and weight change calculation, the grafting rate of tris(hydroxymethyl)aminomethanesulfonic acid is 10wt%, and the grafting rate = (dry weight of hydroxy-modified PET resin - dry weight of PET resin) ÷ dry weight of PET resin × 100%.
[0034] The preparation method of ferrocene-modified graphene fiber comprises the following steps: dispersing graphene fiber in an organic solvent, then adding silane coupling agent KH560 thereto, stirring at 50°C for 3h, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 60°C for 4h, then removing the solvent by back-spin evaporation, washing the crude product with ethanol, and finally drying in a vacuum drying oven at 80°C to constant weight to obtain ferrocene-modified graphene fiber; the mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and the 1,1'-diaminoferrocene is 3:15:0.3:0.3; the graphene fiber is a single-layer graphene fiber with an average diameter of 3μm and a length of 1mm; and the organic solvent is dimethyl sulfoxide.
[0035] The compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1010; and the lubricant is ethylene bisstearamide.
[0036] The functional coating is made of a hyperbranched polyetherimide epoxy compound; the hyperbranched polyetherimide epoxy compound is made according to the method of Example 35 of the Chinese invention patent with authorization announcement number CN110951076B.
[0037] The thickness of the modified polyester film substrate is 4 μm; the thickness of the functional coating is 1 μm.
[0038] A method for preparing a modified polyester film for a composite current collector comprises the following steps: uniformly mixing the raw materials of a modified polyester film substrate in parts by weight, adding the mixture into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing a hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating the mixture on the surface of the modified polyester film substrate, and then drying the mixture at 100°C to a constant weight to obtain a modified polyester film for a composite current collector; the extrusion temperature of the twin-screw extruder is 235°C; the stretching temperature of the biaxial stretching film-forming machine is 110°C, the stretching rate is 120 mm / s, the heat setting temperature is 220°C, and the stretching ratio is 4:1; the mass ratio of the hyperbranched polyetherimide epoxy compound to N-methylpyrrolidone is 1:1.
[0039] Example 2, a modified polyester film for a composite current collector, comprising a modified polyester film substrate and a functional coating applied on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 17 parts of amino-containing hyperbranched liquid crystal polymer, 3.5 parts of 3,5-diamino-1,2,4-triazole, 3.5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1.2 parts of triethylamine, 12 parts of ferrocene-modified graphene fiber, 1.5 parts of a compatibilizer, 0.9 parts of an antioxidant, and 1.1 parts of a lubricant.
[0040] The preparation method of the hydroxyl-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide and tris(hydroxymethyl)aminomethanesulfonic acid) into a reaction kettle with a reflux device and containing dimethyl sulfoxide, stirring and reacting at 180° C. for 6 hours, then precipitating in water, washing the precipitated polymer with ethanol for 4 times, and finally drying in a vacuum drying oven at 97° C. to constant weight to obtain the hydroxyl-modified PET resin; the mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid and dimethyl sulfoxide is 5:0.3:0.45:0.7:17; the PET resin is China Xiamen Tenglong DSR TL-103 PET resin; and the amino-containing hyperbranched liquid crystal polymer is prepared according to the method of Example 4 of the Chinese invention patent with the authorization announcement number CN114437493B.
[0041] The preparation method of ferrocene-modified graphene fiber comprises the following steps: dispersing graphene fiber in an organic solvent, then adding silane coupling agent KH560 thereto, stirring at 52°C for 3.5 hours, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 65°C for 4.5 hours, then removing the solvent by back-spin evaporation, washing the crude product with ethanol, and finally drying in a vacuum drying oven at 83°C to constant weight to obtain ferrocene-modified graphene fiber; the mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and the 1,1'-diaminoferrocene is 3.5:17:0.35:0.3; the graphene fiber is a single-layer graphene fiber with an average diameter of 4μm and a length of 1.5mm; and the organic solvent is N,N-dimethylformamide.
[0042] The compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 168; and the lubricant is butyl stearate.
[0043] The functional coating is made of a hyperbranched polyetherimide epoxy compound; the hyperbranched polyetherimide epoxy compound is made according to the method of Example 35 of the Chinese invention patent with authorization announcement number CN110951076B.
[0044] The thickness of the modified polyester film substrate is 4 μm; the thickness of the functional coating is 1 μm.
[0045] A method for preparing a modified polyester film for a composite current collector comprises the following steps: uniformly mixing the raw materials of a modified polyester film substrate in parts by weight, adding the mixture into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing a hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating the mixture on the surface of the modified polyester film substrate, and then drying the mixture at 103°C to a constant weight to obtain a modified polyester film for a composite current collector; the extrusion temperature of the twin-screw extruder is 245°C; the stretching temperature of the biaxial stretching film-forming machine is 113°C, the stretching rate is 110 mm / s, the heat setting temperature is 225°C, and the stretching ratio is 4:1.
[0046] The mass ratio of the hyperbranched polyetherimide epoxy compound to N-methylpyrrolidone is 1.3:1.
[0047] Example 3, a modified polyester film for a composite current collector, comprising a modified polyester film substrate and a functional coating applied on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 20 parts of amino-containing hyperbranched liquid crystal polymer, 4 parts of 3,5-diamino-1,2,4-triazole, 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1.5 parts of triethylamine, 13 parts of ferrocene-modified graphene fiber, 2 parts of compatibilizer, 1 part of antioxidant, and 1.3 parts of lubricant.
[0048] The preparation method of the hydroxyl-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide and tris(hydroxymethyl)aminomethanesulfonic acid) into a reaction kettle with a reflux device and containing dimethyl sulfoxide, stirring and reacting at 182° C. for 6.5 hours, then precipitating in water, washing the precipitated polymer with ethanol for 4 times, and finally drying in a vacuum drying oven at 100° C. to constant weight to obtain a hydroxyl-modified PET resin; the mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid and dimethyl sulfoxide is 5:0.3:0.5:0.8:20; the PET resin is DSRTL-103 PET resin produced by Xiamen Tenglong of China; and the amino-containing hyperbranched liquid crystal polymer is prepared according to the method of Example 4 of the Chinese invention patent with the authorization announcement number CN114437493B.
[0049] The preparation method of ferrocene-modified graphene fiber comprises the following steps: dispersing graphene fiber in an organic solvent, then adding silane coupling agent KH560 thereto, stirring at 55°C for 4h, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 70°C for 5h, then removing the solvent by back-spin evaporation, washing the crude product with ethanol, and finally drying in a vacuum drying oven at 85°C to constant weight to obtain ferrocene-modified graphene fiber; the mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and the 1,1'-diaminoferrocene is 4:20:0.4:0.3; the graphene fiber is a single-layer graphene fiber with an average diameter of 4.5μm and a length of 2mm; and the organic solvent is N-methylpyrrolidone.
[0050] The compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1076; and the lubricant is ethylene bisstearamide.
[0051] The functional coating is made of a hyperbranched polyetherimide epoxy compound; the hyperbranched polyetherimide epoxy compound is made according to the method of Example 35 of the Chinese invention patent with authorization announcement number CN110951076B.
[0052] The thickness of the modified polyester film substrate is 4 μm; the thickness of the functional coating is 1 μm.
[0053] A method for preparing a modified polyester film for a composite current collector comprises the following steps: uniformly mixing the raw materials of a modified polyester film substrate in parts by weight, adding the mixture into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing a hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating the mixture on the surface of the modified polyester film substrate, and then drying the mixture at 108°C to a constant weight to obtain a modified polyester film for a composite current collector; the extrusion temperature of the twin-screw extruder is 250°C; the stretching temperature of the biaxial stretching film-forming machine is 115°C, the stretching rate is 100 mm / s, the heat setting temperature is 230°C, and the stretching ratio is 4:1.
[0054] The mass ratio of the hyperbranched polyetherimide epoxy compound to N-methylpyrrolidone is 1.5:1.
[0055] Example 4, a modified polyester film for a composite current collector, comprising a modified polyester film substrate and a functional coating applied on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 20 parts of amino-containing hyperbranched liquid crystal polymer, 4 parts of 3,5-diamino-1,2,4-triazole, 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1.5 parts of triethylamine, 13 parts of ferrocene-modified graphene fiber, 2 parts of compatibilizer, 1 part of antioxidant, and 1.3 parts of lubricant.
[0056] The preparation method of the hydroxyl-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide and tris(hydroxymethyl)aminomethanesulfonic acid) into a reaction kettle with a reflux device and containing dimethyl sulfoxide, stirring and reacting at 183° C. for 7.5 hours, then precipitating in water, washing the precipitated polymer with ethanol for 5 times, and finally drying in a vacuum drying oven at 103° C. to constant weight to obtain a hydroxyl-modified PET resin; the mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid and dimethyl sulfoxide is 5:0.3:0.55:0.95:23; the PET resin is DSRTL-103 PET resin produced by Xiamen Tenglong of China; and the amino-containing hyperbranched liquid crystal polymer is prepared according to the method of Example 4 of the Chinese invention patent with the authorization announcement number CN114437493B.
[0057] The preparation method of ferrocene-modified graphene fiber comprises the following steps: dispersing graphene fiber in an organic solvent, then adding silane coupling agent KH560 thereto, stirring at 58°C for 4.5 hours, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 75°C for 5.5 hours, then removing the solvent by back-spin evaporation, washing the crude product with ethanol, and finally drying to constant weight in a vacuum drying oven at 88°C to obtain ferrocene-modified graphene fiber; the mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and the 1,1'-diaminoferrocene is 4.5:23:0.45:0.3; the graphene fiber is a single-layer graphene fiber with an average diameter of 5.5μm and a length of 2.5mm; the organic solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone in a mass ratio of 1:2:3.
[0058] The compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is a mixture of antioxidant 1010, antioxidant 168, and antioxidant 1076 in a mass ratio of 1:1:3; the lubricant is a mixture of ethylene bisstearamide and butyl stearate in a mass ratio of 3:5.
[0059] The functional coating is made of a hyperbranched polyetherimide epoxy compound; the hyperbranched polyetherimide epoxy compound is made according to the method of Example 35 of the Chinese invention patent with authorization announcement number CN110951076B.
[0060] The thickness of the modified polyester film substrate is 4 μm; the thickness of the functional coating is 1 μm.
[0061] A method for preparing a modified polyester film for a composite current collector comprises the following steps: uniformly mixing the raw materials of a modified polyester film substrate in parts by weight, adding the mixture into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing a hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating the mixture on the surface of the modified polyester film substrate, and then drying the mixture at 108°C to a constant weight to obtain a modified polyester film for a composite current collector; the extrusion temperature of the twin-screw extruder is 260°C; the stretching temperature of the biaxial stretching film-forming machine is 118°C, the stretching rate is 90 mm / s, the heat setting temperature is 235°C, and the stretching ratio is 4:1.
[0062] The mass ratio of the hyperbranched polyetherimide epoxy compound to N-methylpyrrolidone is 1.8:1.
[0063] Example 5, a modified polyester film for a composite current collector, comprising a modified polyester film substrate and a functional coating applied on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 25 parts of amino-containing hyperbranched liquid crystal polymer, 5 parts of 3,5-diamino-1,2,4-triazole, 5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2 parts of triethylamine, 15 parts of ferrocene-modified graphene fiber, 3 parts of compatibilizer, 1.2 parts of antioxidant, and 1.5 parts of lubricant.
[0064] The preparation method of the hydroxyl-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide and tris(hydroxymethyl)aminomethanesulfonic acid into a reaction kettle equipped with dimethyl sulfoxide and a reflux device, stirring and reacting at 185° C. for 8 hours, then precipitating in water, washing the precipitated polymer with ethanol for 6 times, and finally drying in a vacuum drying oven at 105° C. to constant weight to obtain the hydroxyl-modified PET resin.
[0065] The mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid) and dimethyl sulfoxide is 5:0.3:0.6:1:25; the PET resin is Tenglong DSR TL-103 PET resin from Xiamen, China; the amino-containing hyperbranched liquid crystal polymer is prepared according to the method of Example 4 of the Chinese invention patent with authorization announcement number CN114437493B.
[0066] The preparation method of ferrocene-modified graphene fiber comprises the following steps: dispersing graphene fiber in an organic solvent, then adding silane coupling agent KH560 thereto, stirring at 60°C for 5h, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 80°C for 6h, then removing the solvent by back-spin evaporation, washing the crude product with ethanol, and finally drying in a vacuum drying oven at 90°C to constant weight to obtain ferrocene-modified graphene fiber; the mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and the 1,1'-diaminoferrocene is 5:25:0.5:0.3; the graphene fiber is a single-layer graphene fiber with an average diameter of 6μm and a length of 3mm; and the organic solvent is dimethyl sulfoxide.
[0067] The compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1076; and the lubricant is ethylene bisstearamide.
[0068] The functional coating is made of a hyperbranched polyetherimide epoxy compound; the hyperbranched polyetherimide epoxy compound is made according to the method of Example 35 of the Chinese invention patent with authorization announcement number CN110951076B.
[0069] The thickness of the modified polyester film substrate is 4 μm; the thickness of the functional coating is 1 μm.
[0070] A method for preparing a modified polyester film for a composite current collector comprises the following steps: uniformly mixing the raw materials of a modified polyester film substrate in parts by weight, adding the mixture into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing a hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating the mixture on the surface of the modified polyester film substrate, and then drying the mixture at 110°C to a constant weight to obtain a modified polyester film for a composite current collector; the extrusion temperature of the twin-screw extruder is 265°C; the stretching temperature of the biaxial stretching film-forming machine is 120°C, the stretching rate is 80 mm / s, the heat setting temperature is 240°C, and the stretching ratio is 4:1.
[0071] The mass ratio of the hyperbranched polyetherimide epoxy compound to N-methylpyrrolidone is 2:1.
[0072] Comparative Example 1, a modified polyester film for a composite current collector, is substantially the same as Example 1, except that PET resin is used instead of the hydroxy-modified PET resin, and 3,5-diamino-1,2,4-triazole is not added.
[0073] Comparative Example 2, a modified polyester film for a composite current collector, is basically the same as Example 1, except that graphene fibers are used instead of ferrocene-modified graphene fibers, and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane is not added.
[0074] Comparative Example 3, a modified polyester film for a composite current collector, is substantially the same as Example 1, except that p-phenylenediamine is used instead of the amino-containing hyperbranched liquid crystal polymer.
[0075] Comparative Example 4, a modified polyester film for a composite current collector, is substantially the same as Example 1, except that glycidyl ether is used instead of the hyperbranched polyetherimide epoxy compound.
[0076] Comparative Example 5, a modified polyester film for a composite current collector, is substantially the same as Example 1, except that p-phenylenediamine is used instead of 3,5-diamino-1,2,4-triazole.
[0077] Comparative Example 6, a modified polyester film for a composite current collector, is substantially the same as Example 1, except that p-phenylenediamine is used instead of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.
[0078] In order to further illustrate the beneficial technical effects of the modified polyester film for composite current collectors involved in each embodiment of the present invention, relevant performance tests were performed on the modified polyester film for composite current collectors involved in Examples 1-5 and Comparative Examples 1-6; the test method is as follows:
[0079] Tensile properties: Tensile strength and elongation at break were tested according to GB / T 13022-1991.
[0080] (2) High temperature resistance: Refer to ASTM D1204-2008 for heat shrinkage test, the test conditions are 150℃, 30min.
[0081] (3) Electrolyte tolerance: The modified polyester film for the composite current collector prepared in each example was cut into samples of 20 cm × 20 cm in size, and the circumference of the sample was recorded as C1. The samples were then immersed in an electrolyte at 65°C for 48 h. The circumference of the sample after immersion was recorded as C2. The swelling degree SD of the sample was calculated according to the following formula: SD = (C2-C1) / C1 × 100%. The electrolyte was a mixture of ethylene carbonate, diethyl carbonate, and methyl ethyl carbonate in a mass ratio of 1:2:1. The smaller the swelling degree, the better the electrolyte tolerance.
[0082] (4) Adhesion between the film and the metal conductive layer: The base films of each example were placed in a magnetron sputtering chamber, and aluminum metal with a purity of 99.99% was used as the target material and argon gas was used as the gas source. In the magnetron sputtering chamber, a 1200 nm thick aluminum metal layer was plated on both sides of the modified polyester film in the thickness direction of the composite current collector involved in each example to obtain a composite current collector; a layer of Permacel P-94 double-sided tape was adhered to a 1 mm thick aluminum foil, and the composite current collector was adhered on the double-sided tape. A layer of ethylene acrylic acid copolymer film (DuPont Nurcel0903, thickness of 50 μm) was covered on the composite current collector, and then a 1.3×10 5 N / m 2 , hot pressing at 120°C for 10s, cooling to room temperature, and cutting into small strips of 150mm×15mm; finally, the ethylene acrylic acid copolymer film of the small sample strip is fixed on the upper clamp of the tensile machine, and the rest is fixed on the lower clamp. After fixation, the two are peeled off at an angle of 180° and a speed of 100mm / min to test the peeling force, which is the adhesion between the film and the metal conductive layer.
[0083] (5) Flame retardancy: tested in accordance with UL94 standard.
[0084] As can be seen from Table 1, the modified polyester film for the composite current collector involved in each embodiment of the present invention has better mechanical properties, better flame retardancy, high temperature resistance, electrolyte tolerance and adhesion to the metal conductive layer than the comparative example product, and the combined use of hydroxyl-modified PET resin, 3,5-diamino-1,2,4-triazole, ferrocene-modified graphene fiber and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, amino-containing hyperbranched liquid crystal polymer, and hyperbranched polyetherimide epoxy compound is beneficial to improving the above properties.
[0085]
[0086] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A modified polyester film for a composite current collector, characterized in that: The invention comprises a modified polyester film substrate and a functional coating coated on the surface thereof, wherein the modified polyester film substrate is made of the following raw materials in parts by weight: 100 parts of hydroxyl-modified PET resin, 15-25 parts of amino-containing hyperbranched liquid crystal polymer, 3-5 parts of 3,5-diamino-1,2,4-triazole, 3-5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1-2 parts of triethylamine, 10-15 parts of ferrocene-modified graphene fiber, 1-3 parts of compatibilizer, 0.8-1.2 parts of antioxidant and 1-1.5 parts of lubricant; the functional coating is made of hyperbranched liquid crystal polymer. The modified polyester film substrate is made of polyetherimide epoxy compound; the thickness of the modified polyester film substrate is 2-4 μm; the thickness of the functional coating is 1 μm; the preparation method of the ferrocene-modified graphene fiber comprises the following steps: dispersing the graphene fiber in an organic solvent, then adding a silane coupling agent KH560 thereto, stirring at 50-60° C. for 3-5 hours, then adding 1,1'-diaminoferrocene thereto, stirring and reacting at 60-80° C. for 4-6 hours, then removing the solvent by rotary evaporation, washing the crude product with ethanol, and finally drying it in a vacuum drying oven at 80-90° C. to constant weight to obtain the ferrocene-modified graphene fiber.
2. The modified polyester film for composite current collector according to claim 1, characterized in that: The preparation method of the hydroxyl-modified PET resin comprises the following steps: adding PET resin, polyphosphoric acid, phosphorus pentoxide and tris(hydroxymethyl)aminomethanesulfonic acid into a reaction kettle equipped with dimethyl sulfoxide and a reflux device, stirring and reacting at 178-185° C. for 5-8 hours, then precipitating the polymer in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying the polymer in a vacuum drying oven at 95-105° C. to a constant weight to obtain the hydroxyl-modified PET resin.
3. The modified polyester film for composite current collector according to claim 2, characterized in that: The mass ratio of the PET resin, polyphosphoric acid, phosphorus pentoxide, tris(hydroxymethyl)aminomethanesulfonic acid, and dimethyl sulfoxide is 5:0.3:(0.4-0.6):(0.6-1):(15-25).
4. The modified polyester film for composite current collector according to claim 2, characterized in that: The PET resin is at least one of the following: DSR TL-103 PET resin produced by Xiamen Tenglong, China, PET008L resin produced by Aclo Compounders, Canada, and YS-W01 PET resin produced by Hainan Yisheng Petrochemical, China.
5. The modified polyester film for composite current collector according to claim 1, characterized in that: The mass ratio of the graphene fiber, the organic solvent, the silane coupling agent KH560, and 1,1'-diaminoferrocene is (3-5):(15-25):(0.3-0.5):0.3; the graphene fiber is a single-layer graphene fiber with an average diameter of 3-6 μm and a length of 1-3 mm; the organic solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone.
6. The modified polyester film for composite current collector according to claim 1, characterized in that: The compatibilizer is compatibilizer CMG9801; the antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076; and the lubricant is at least one of ethylene bisstearamide and butyl stearate.
7. A method for preparing the modified polyester film for a composite current collector according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: uniformly mixing the raw materials of the modified polyester film substrate according to parts by weight, adding the raw materials into a twin-screw extruder for melt extrusion, and then forming a film of the extruded material through a biaxial stretching film-forming machine to obtain a modified polyester film substrate; then dispersing a hyperbranched polyetherimide epoxy compound in N-methylpyrrolidone, uniformly coating the resultant compound on the surface of the modified polyester film substrate, and then drying the resultant compound at 100-110°C to a constant weight to obtain a modified polyester film for a composite current collector.
8. The method for preparing a modified polyester film for a composite current collector according to claim 7, characterized in that: The extrusion temperature of the twin-screw extruder is 235-265°C; the stretching temperature of the biaxial stretching film-forming machine is 110-120°C, the stretching rate is 120-80 mm / s, the heat setting temperature is 220-240°C, and the stretching ratio is 4:1; the mass ratio of the hyperbranched polyetherimide epoxy compound and N-methylpyrrolidone is (1-2):1.
Citation Information
Patent Citations
A class of hyperbranched polyetherimides and their preparation and application
CN110951076B
A high thermal conductivity elastomer and its preparation method
CN114437493B
Modified polyester film, preparation method, composite current collector, electrode sheet and its application
CN115477833B
A class of hyperbranched polyetherimides, preparation method and applications thereof
CN110951076A
High-thermal-conductivity elastomer and preparation method thereof
CN114437493A